Doped and modified multi-shell ternary precursor as well as preparation method and application thereof
By using a multi-shell ternary precursor preparation method in the positive electrode material of lithium-ion batteries, a shell structure with high nickel core and a shell structure that gradually reduces nickel content is solved, and the stability problem of core-shell structure in the electrochemical cycle is solved. It achieves higher electrochemical performance and safety, suitable for large-scale production.
Patent Information
- Application Number
- CN202411126498.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The existing core-shell structure nickel-rich cathode material has problems such as structural collapse, poor thermal stability and unstable electrochemical performance during the electrochemical cycle. The preparation method is complex and the repetition and consistency are not ideal, which limits its use in lithium-ion batteries. Application in.
The preparation method of doping modified multi-shell ternary precursor is adopted. The first stage of co-precipitation of solution A with a high nickel content and the doped metal salt solution to form a high nickel core, and then the solution B with a low nickel content is lower. Multiple co-precipitation is carried out to form a shell layer that gradually reduces the nickel content, forming a multi-shell structure with at least 5 shell layers, solving the problems of cumbersome control of process parameters and unstable electrochemical performance.
It achieves stronger circulation and thermal stability, improves electrochemical performance and safety, is suitable for large-scale production, and promotes the practical application of high-energy nickel-rich layered positive electrodes.
Smart Images

Figure CN119008902A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a doped and modified multi-shell ternary precursor and a preparation method and application thereof. Background Art
[0002] In the past few decades, efforts have been made to develop ideal cathode materials with high capacity, long life, good rate performance and safety to replace the traditional layered LiCoO 2 , has been the main driving force for the development of lithium-ion batteries (LIBs). Relevant researchers have conducted extensive research on three groups of positive electrodes: layered Li[Ni-Co-Mn]O 2 and Li 1+x [Mn-M] 1-x O 2 (M = Ni, Co, Ru, Ti, etc.), spinel LiNi 0.5 Mn 1.5 O 4 Olive-shaped LiMPO 4 (M=Fe and Mn). Among these materials, nickel-rich layered Li[Ni 1-x M x ]O 2 (M=Co, Mn, etc.), i.e. LiNiO 2 -LiMO 2 Solid solutions of Ni-rich Li[Ni] have a specific capacity of more than 200 mAh / g, low cost, and excellent rate capability, and are considered to be a promising class of advanced lithium-ion battery cathodes, especially as a durable power source for electric vehicles (EVs). 1-x M x ]O 2 Electrode, Ni 2+ / 3+ / 4+ The redox couple provides most of the specific capacity. However, it usually exhibits severe structural collapse and poor thermal stability under electrochemical cycling conditions: (1) The highly oxidative Ni 4+ Ions easily react with the electrolyte at the electrode / electrolyte interface, resulting in Ni 2+ dissolution and electrolyte decomposition; (2) the R3m layered phase easily transforms into the Fm3m rock salt phase, Ni 2+ (3a position) easily occupies the adjacent Li + vacancies (3b sites); (3) active oxygen is easily separated from the main structure of the highly charged positive electrode, thus causing safety issues. Therefore, the Ni-rich layered positive electrode exhibits rapid capacity decay during cycling, which is due to the loss of active material mass and Li + This is caused by slow insertion / extraction kinetics and poor safety due to oxygen loss from the host structure.
[0003] In addition, as an energy storage device for electric vehicles, lithium batteries need to improve their practicality by increasing the charging rate to shorten the charging time. Therefore, the development of Ni-rich layered cathodes with good electrochemical performance and safety is urgently needed for their practical application in lithium-ion batteries.
[0004] In order to solve the above shortcomings, relevant researchers proposed a core-shell structured nickel-rich cathode Li[(Ni 0.8 Co 0.1 Mn 0.1 ) 0.8 -(Ni 0.5 Mn 0.5 ) 0.2 ]O 2 , utilizing structurally / thermally stable LiNi 0.5 Mn 0.5 O 2 (NM55) Shell package high capacity nickel-rich LiNi 0.8 Co 0.1 Mn 0.1 O 2 The core-shell structure has two significant roles: (1) the shell can protect the sensitive core from direct penetration into the electrolyte, inhibiting unwanted structural transformations and the loss of nickel-rich active components; (2) the shell has a stable electrode / electrolyte interface and provides available Li + / electron migration path. Due to the protection of the micron-sized shell, the core-shell electrode exhibits stronger cycle / thermal stability compared with other electrodes. For example, CN115924988A discloses a core-shell structure ternary precursor, a preparation method thereof, and a single crystal ternary material. The core-shell structure ternary precursor has an inner core of a loose porous structure with macropores and small pores randomly arranged formed by the interweaving of primary particles, and an outer shell of a serrated structure. In CN114804234A, the ternary precursor material is a spherical particle with a core-shell structure, the core layer material of the ternary precursor material is a nickel-cobalt-manganese ternary precursor, and the shell layer material of the ternary precursor material is a nickel-cobalt-aluminum ternary precursor.
[0005] However, after in-depth research on the nickel-rich cathode, it was found that there was a mismatch in the structure, that is, a hole layer of tens of nanometers between the core and the shell. The formed hole layer cuts off the Li + The migration and electron transfer paths limit the electrochemical performance of the core-shell cathode. Related scholars have reported the nickel-rich concentration gradient core-shell material (CG) LiNi 0.64 Co 0.18 Mn 0.18 O 2 , where the core LiNi 0.8 Co 0.1 Mn 0.1O 2 Surrounded by an outer CG layer to address the above-mentioned deficiencies of the core-shell cathode. In recent years, CG nickel-rich layered oxides have been further reported as high-capacity, long-life, and safe advanced lithium-ion battery cathodes. Previous studies have focused on the preparation of core-shell cathode materials using target core-shell precursors. However, the preparation process of the core-shell precursor must be precisely controlled. At the same time, the generated core-shell solution is simultaneously added to a continuous stirred tank reactor (CSTR) to obtain the target core-shell precursor. The complex preparation parameters make the repeatability and consistency of the core-shell precursor unsatisfactory. In fact, the degree of repeatability and consistency is an extremely important factor in the widespread commercialization of positive / negative electrode materials.
[0006] Therefore, there is an urgent need to develop innovative strategies for core-shell cathodes with simple steps and feasibility of large-scale preparation for practical applications, so as to solve the problems of cumbersome process parameter control, unsatisfactory repeatability and consistency, and unstable electrochemical properties such as cycle life and rate characteristics in the existing core-shell material preparation methods. Summary of the invention
[0007] In view of the problems existing in the prior art, the present invention provides a doped and modified multi-shell ternary precursor and a preparation method and application thereof. The preparation method first uses a solution A with a higher nickel content and a doped metal salt solution to carry out a first-stage coprecipitation to form a high-nickel core containing a doping element M, then stops the introduction of the doped metal salt solution, and carries out a second-stage coprecipitation of the solution A with a higher nickel content and a solution B with a lower nickel content to form a shell 1 with a reduced total nickel content and not containing the doping element M, gradually reduces the total volume of the solution A and gradually increases the total volume of the solution B, and repeats the second-stage coprecipitation at least 4 times. The finally obtained doped and modified multi-shell ternary precursor has a high-nickel core containing the doping element M formed inside, contains at least 5 shell layers from the inside to the outside, and the nickel content gradually decreases. The problems of cumbersome process parameter control, unsatisfactory repeatability and consistency, and unstable electrochemical properties such as cycle life and rate characteristics in the existing preparation method can be solved.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] One of the purposes of the present invention is to provide a method for preparing a doped and modified multi-shell ternary precursor, the preparation method comprising the following steps:
[0010] (1) preparing a first nickel-cobalt-manganese ternary solution as solution A, wherein the molar ratio of Ni:Co:Mn in solution A is x 1 :y 1 :z 1 ; Among them, 0.6<x 1 <0.9,0.1<y 1 <0.2, z 1>0,x 1 +y 1 +z 1 =1;
[0011] Prepare a second nickel-cobalt-manganese ternary solution as solution B, wherein the molar ratio of Ni:Co:Mn in solution B is x 2 :y 2 :z 2 ; Among them, 0.2<x 2 <0.4,0.2<y 2 <0.4, z 2 >0,x 2 +y 2 +z 2 =1;
[0012] preparing a doping metal salt solution containing a doping element M, wherein the doping element M comprises at least one of aluminum, titanium, niobium, zirconium, tungsten, vanadium, strontium, gallium, cerium, yttrium or lanthanum;
[0013] (2) Injecting the solution A, the doped metal salt solution, the complexing agent solution and the precipitant solution into the reaction base solution in parallel to perform the first stage of co-precipitation to achieve the first target particle size D50 1 Afterwards, a core is formed;
[0014] (3) stopping the introduction of the doped metal salt solution, and injecting the solution A, the solution B, the complexing agent solution and the precipitant solution in parallel to perform the second stage of co-precipitation to form a shell layer 1;
[0015] (4) Repeat step (3) at least 4 times, each time the total volume of the second-stage co-precipitation solution A gradually decreases, and each time the total volume of the second-stage co-precipitation solution B gradually increases, stop the reaction, and obtain a doped and modified multi-shell ternary precursor through solid-liquid separation.
[0016] The preparation method of the present invention first uses a solution A with a higher nickel content and a doped metal salt solution to perform a first-stage coprecipitation to form a high-nickel core containing a doping element M, then stops introducing the doped metal salt solution, and performs a second-stage coprecipitation on the solution A with a higher nickel content and a solution B with a lower nickel content to form a shell layer 1 with a reduced total nickel content and not containing the doping element M, then gradually reduces the total volume of the solution A and gradually increases the total volume of the solution B, and repeats the second-stage coprecipitation at least 4 times, and finally obtains a doped-modified multi-shell ternary precursor, wherein a high-nickel core containing the doping element M is formed inside, contains at least 5 shell layers from the inside to the outside, and the nickel content gradually decreases, which can solve the problems of cumbersome process parameter control, unsatisfactory repeatability and consistency, and unstable electrochemical properties such as cycle life and rate characteristics in the existing core-shell material preparation method.
[0017] It should be noted that in the preparation method described in the present invention, element M is only doped in the first stage of co-precipitation to ensure that the inside of the core is loose and porous, which can alleviate stress concentration in subsequent electrochemical tests; moreover, in at least 5 times of the second stage of co-precipitation, the added volume ratio of solution A and solution B decreases gradually, so that the nickel content of at least 5 shell layers from the inside to the outside gradually decreases.
[0018] It should be noted that in the preparation method of the present invention, the second stage co-precipitation is repeated at least 4 times, that is, the second stage co-precipitation is carried out at least 5 times, and at least 5 shell layers will be formed on the outside of the core. This is because the shell layer is to achieve a more uniform transition from the components of the core to the components of the outer shell. The more shell layers there are, the smaller the content gradient between the shell layers, the smoother the transition, and the more conducive to subsequent electrochemical performance.
[0019] It should be noted that in the preparation method of the present invention, after the core preparation is completed, the introduction of the doping metal salt solution is stopped, the pH and ammonia concentration in the reaction system are stably controlled, the remaining solution A is divided into five parts, recorded as A1, A2, A3, A4, and A5, and the solution B is also divided into five parts, recorded as B1, B2, B3, B4, and B5, and the complexing agent solution, the precipitant solution, the solution A1, and the solution B1 are successively introduced into the reactor to form a shell layer 1, and the complexing agent solution, the precipitant solution, the solution A2, and the solution B2 are continuously introduced into the reactor to form a shell layer 2, and the complexing agent solution, the precipitant solution, the solution A3 are continuously introduced into the reactor to form a shell layer 2. and solution B3 to form shell 3, and continue to introduce complexing agent solution, precipitant solution, solution A4 and solution B4 into the reactor to form shell 4, and continue to introduce complexing agent solution, precipitant solution, solution A5 and solution B5 into the reactor to form shell 5, and finally form a doped and modified multi-shell ternary precursor, and the volumes of solution A1, solution A2, solution A3, solution A4 and solution A5 show a gradually decreasing trend, that is, V(A1)>V(A2)>V(A3)>V(A4)>V(A5), and the volumes of solution B1, solution B2, solution B3, solution B4 and solution B5 show a gradually increasing trend, that is, V(B1) <V(B2)<V(B3)<V(B4)<V(B5)。
[0020] The preparation method of the present invention prepares a core-shell with a certain concentration gradient. The shell can protect the sensitive core from directly penetrating into the electrolyte, inhibiting unnecessary structural transformation and loss of nickel-rich active components; at the same time, the shell has a stable electrode / electrolyte interface and provides available Li during the redox process. + / electron migration path; compared with the traditional technology of preparing core-shell positive electrodes from core-shell precursors, the preparation method of the present invention is more suitable for large-scale production, which will promote the practical application of high-energy nickel-rich layered positive electrodes.
[0021] It should be noted that a doped metal salt solution containing a doping element M is prepared, and the doping element M includes at least one of aluminum (Al), titanium (Ti), niobium (Nb), zirconium (Zr), tungsten (W), vanadium (V), strontium (Sr), gallium (Ga), cerium (Ce), yttrium (Y) or lanthanum (La), and the doping element M is preferably strontium (Sr); the preparation method of the present invention is modified by the doping element M, especially by doping Sr, which can be uniformly doped within a certain range, and the interlayer spacing of metal ions can be further expanded, so that the distance of lithium ion transmission is shortened, the rate performance and cycle performance of the material are improved, and at the same time, the crystal structure is stabilized, and the safety during the electrochemical reaction is improved.
[0022] It should be noted that the soluble nickel salt in the solution A and the solution B in step (1) includes at least one of nickel sulfate, nickel nitrate, nickel acetate or nickel chloride, preferably nickel chloride; the soluble cobalt salt in the solution A and the solution B in step (1) includes at least one of cobalt sulfate, cobalt nitrate, cobalt acetate or cobalt chloride, preferably cobalt chloride; the soluble manganese salt in the solution A and the solution B in step (1) includes at least one of manganese sulfate, manganese nitrate, manganese acetate or manganese chloride, preferably manganese chloride; that is, solution A is preferably a mixed solution of nickel chloride, cobalt chloride and manganese chloride with a total concentration of nickel, cobalt and manganese elements of 20-120 g / L, and solution B is preferably a mixed solution of nickel chloride, cobalt chloride and manganese chloride with a total concentration of nickel, cobalt and manganese elements of 20-120 g / L.
[0023] As a preferred technical solution of the present invention, in step (1), the total concentration of ternary ions in solution A and solution B is the same, both of which are 20-120 g / L, for example, 20 g / L, 40 g / L, 60 g / L, 80 g / L, 100 g / L or 120 g / L, etc.
[0024] It should be noted that the preparation method of the present invention preferably has the same total concentration of ternary ions in solution A and solution B in order to achieve a more uniform composition gradient change in the shell layer. If the total concentration of ternary ions in solution A and solution B is different or even too different, the uniformly transitioned shell layer content will change abnormally, thereby affecting the final main content.
[0025] Preferably, in step (1), the doping element M in the doping metal salt solution is strontium.
[0026] Preferably, the strontium source in the doped metal salt solution includes at least one of strontium nitrate, strontium chloride, strontium acetate or strontium sulfate.
[0027] Preferably, in step (1), the doping metal salt solution has a doping element M metal salt content of 10-50 g / L, such as 10 g / L, 20 g / L, 30 g / L, 40 g / L or 50 g / L.
[0028] As a preferred technical solution of the present invention, in step (2), the doping amount of the doping element M is controlled to be 0.05-5% of the total molar amount of nickel, cobalt and manganese, for example, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc.
[0029] It should be noted that the doping amount of the doping element M described in the present invention is 0.05-5% of the total molar amount of nickel, cobalt and manganese ternary, which refers to the target doping amount formulated in the design stage before the preparation method starts, that is, the doping element M is compared to the total molar amount of nickel, cobalt and manganese in the doped and modified multi-shell ternary precursor obtained by the entire preparation method.
[0030] Preferably, the reaction base liquid in step (2) is prepared from pure water, a precipitant and a complexing agent.
[0031] Preferably, the temperature of the reaction base solution in step (2) is 50-70°C, for example, 50°C, 55°C, 60°C, 65°C or 70°C.
[0032] Preferably, the pH value of the reaction base solution in step (2) is 11-13, such as 11, 11.5, 12, 12 or 13.
[0033] Preferably, the complexing agent concentration of the reaction base solution in step (2) is 4-10 g / L, for example 4 g / L, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L or 10 g / L, etc. When the complexing agent solution is ammonia water, the complexing agent concentration of the reaction base solution is the ammonia concentration.
[0034] Preferably, before the parallel injection in step (2), N 2 Stir and control N 2 The entry rate is 0.2-2m 3 / h, for example 0.2m 3 / h、0.5m 3 / h、0.8m 3 / h、1m 3 / h、1.3m 3 / h、1.5m 3 / h、1.7m 3 / h or 2m 3 / h, etc.
[0035] It should be noted that the pH value of the first stage co-precipitation is controlled at 10.0-10.5, the ammonia concentration is controlled at 3-5 g / L, and the pH value of the second stage co-precipitation is controlled at 10.5-11.2, the ammonia concentration is controlled at 6-8 g / L.
[0036] As a preferred technical solution of the present invention, in step (2), the flow rate of solution A is 2-4 L / h, for example, 2 L / h, 2.5 L / h, 3 L / h, 3.5 L / h or 4 L / h, the flow rate of the doped metal salt solution is 200-600 mL / h, for example, 200 mL / h, 300 mL / h, 400 mL / h, 500 mL / h or 600 mL / h, the flow rate of the complexing agent solution is 400-600 mL / h, for example, 400 mL / h, 450 mL / h, 500 mL / h, 550 mL / h or 600 mL / h, and the flow rate of the precipitant solution is 1-1.4 L / h, for example, 1 L / h, 1.1 L / h, 1.2 L / h, 1.3 L / h or 1.4 L / h, etc.
[0037] As a preferred technical solution of the present invention, in step (2), the first target particle size D50 1 It is 3-4μm, for example, 3μm, 3.1μm, 3.3μm, 3.5μm, 3.7μm, 3.8μm or 4μm, etc.
[0038] As a preferred technical solution of the present invention, in step (3), the flow rate of the complexing agent solution is 600-800mL / h, for example, 600mL / h, 650mL / h, 700mL / h, 750mL / h or 800mL / h, and the flow rate of the precipitant solution is 1.5-2.0L / h, for example, 1.5L / h, 1.6L / h, 1.7L / h, 1.8L / h, 1.9L / h or 2.0L / h, etc.
[0039] It should be noted that in the second stage co-precipitation corresponding to step (3) and the subsequently repeated step (4), the flow rate of solution A is 0.1-5 L / h, and the flow rate of solution B is 0.1-5 L / h, and the feed size corresponding to each second stage co-precipitation depends on the prepared volume to ensure that solution A and solution B complete the feeding of their respective corresponding volumes within the same time.
[0040] It should be noted that the flow rates of the complexing agent solution and the precipitant solution in the second stage co-precipitation corresponding to step (3) and step (4) are increased, and the flow rate of the ternary solution of solution A and solution B is also increased, which can accelerate the growth rate and make the morphology of the ternary precursor more loose.
[0041] As a preferred technical solution of the present invention, in step (4), the solid-liquid separation includes aging, washing, drying and post-treatment performed in sequence.
[0042] Preferably, the washing comprises at least three washings with hot water.
[0043] Preferably, the drying temperature is 100-150°C, such as 100°C, 110°C, 120°C, 130°C, 140°C or 150°C.
[0044] Preferably, the complexing agent solution in step (2) and step (3) is aqueous ammonia.
[0045] Preferably, the precipitant solution in step (2) and step (3) is a sodium hydroxide solution.
[0046] The second object of the present invention is to provide a doped and modified multi-shell ternary precursor, which is prepared by the preparation method described in the first object, and has the general formula of Ni a Co b Mn c Sr d (OH) 2 ; Among them, 0.6<a<0.9, 0<b<0.2, 0<c<0.2, 0<d<0.1, a+b+c+d=1.
[0047] The third object of the present invention is to provide an application of a doped and modified multi-shell ternary precursor, wherein the doped and modified multi-shell ternary precursor is uniformly mixed with a lithium source and sintered at a high temperature to obtain a lithium positive electrode material;
[0048] Wherein, the doped and modified multi-shell ternary precursor is prepared by the preparation method described in the first purpose, or the doped and modified multi-shell ternary precursor is the doped and modified multi-shell ternary precursor described in the second purpose.
[0049] As a preferred technical solution of the present invention, the molar ratio of the total molar amount of nickel, cobalt and manganese in the doped modified multi-shell ternary precursor to the molar amount of lithium element in the lithium source is 1:(1-1.1), for example, 1:1, 1:1.01, 1:1.03, 1:1.05, 1:1.07, 1:1.08 or 1:1.1, etc.
[0050] Preferably, the high temperature sintering includes a first sintering stage and a second sintering stage.
[0051] Preferably, the target temperature of the first sintering stage is 400-700°C, for example 400°C, 450°C, 500°C, 550°C, 600°C, 650°C or 700°C, etc., the holding time is 3-6h, for example 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h, etc., and the heating rate is 2-6°C / min, for example 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min or 6°C / min, etc.
[0052] Preferably, the target temperature of the second sintering stage is 700-1000°C, for example 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, the holding time is 10-20h, for example 10h, 11h, 13h, 15h, 17h, 19h or 20h, and the heating rate is 2-6°C / min, for example 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min or 6°C / min, etc.
[0053] Compared with the prior art solutions, the present invention has at least the following beneficial effects:
[0054] (1) The preparation method of the present invention first uses a solution A with a high nickel content and a doped metal salt solution to perform a first-stage coprecipitation to form a high-nickel core containing a doping element M, then stops the introduction of the doped metal salt solution, and performs a second-stage coprecipitation on the solution A with a high nickel content and a solution B with a low nickel content to form a shell layer 1 with a reduced total nickel content and not containing the doping element M, then gradually reduces the total volume of solution A and gradually increases the total volume of solution B, and repeats the second-stage coprecipitation at least 4 times, and finally obtains a doped-modified multi-shell ternary precursor, wherein a high-nickel core containing a doping element M is formed inside, and contains at least 5 shell layers from the inside to the outside, and the nickel content gradually decreases. This can solve the problems of cumbersome process parameter control, unsatisfactory repeatability and consistency, and unstable electrochemical properties such as cycle life and rate characteristics in the existing core-shell material preparation method;
[0055] (2) The preparation method of the present invention prepares a core-shell with a certain concentration gradient. The shell can protect the sensitive core from directly penetrating into the electrolyte, inhibiting unnecessary structural transformation and loss of nickel-rich active components; at the same time, the shell has a stable electrode / electrolyte interface and provides available Li during the redox process. + / electron migration path; compared with the traditional technology of preparing core-shell positive electrodes from core-shell precursors, the preparation method of the present invention is more suitable for large-scale production, which will promote the practical application of high-energy nickel-rich layered positive electrodes. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 is a SEM image of the doped and modified multi-shell ternary precursor obtained in this example;
[0057] Figure 2 is a cross-sectional SEM image of the doped and modified multi-shell ternary precursor obtained in this example. DETAILED DESCRIPTION
[0058] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0059] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0060] Example 1
[0061] This embodiment provides a method for preparing a doped and modified multi-shell ternary precursor, the preparation method comprising the following steps:
[0062] A first nickel-cobalt-manganese ternary solution is prepared as solution A, wherein the molar ratio of Ni:Co:Mn in the solution A is 0.9:0.05:0.05, the soluble salts of nickel, cobalt and manganese are all chlorides, and the total concentration of ternary ions in the solution A is 50 g / L;
[0063] A second nickel-cobalt-manganese ternary solution is prepared as solution B, wherein the molar ratio of Ni:Co:Mn in solution B is 0.4:0.3:0.3, the soluble salts of nickel, cobalt and manganese are all chlorides, and the total concentration of ternary ions in solution B is 50 g / L;
[0064] Prepare a sodium hydroxide solution with a mass concentration of 30% as a precipitant solution;
[0065] Prepare 12% ammonia water as a complexing agent solution;
[0066] A strontium chloride solution with a concentration of 25 g / L is prepared as a doping metal salt solution, and the doping element M is strontium;
[0067] Among them, solution A is prepared in total of 100L, and solution B is prepared in total of 20L; 80L of solution A is taken for the first stage of coprecipitation, and the remaining solution A is divided into five parts, denoted as A1, A2, A3, A4, and A5, and their volumes are V(A1)=7L, V(A2)=6L, V(A3)=4L, V(A4)=2L, and V(A5)=1L respectively; solution B is divided into five parts, denoted as B1, B2, B3, B4, and B5, and their volumes are V(B1)=1L, V(B2)=2L, V(B3)=4L, V(B4)=6L, and V(B5)=7L respectively;
[0068] Add 250L of pure water and a certain amount of NaOH solution and ammonia water into a 500L reactor to prepare the reaction base solution, and 3 / h rate of nitrogen gas into the reaction bottom liquid, stirring at a speed of 150r / min to make it evenly mixed, then heating to 50°C, controlling the pH value to 11.5, the ammonia concentration to 4g / L, and the total alkalinity to 20g / L;
[0069] The reaction temperature is controlled at 50-70°C, the stirring speed is 200-400r / min, the pH is 10-11.5, the ammonia concentration is 3-8g / L, the flow rates of the complexing agent solution, the precipitant solution, solution A and / or solution B, and the doped metal salt solution are stabilized, and the coprecipitation reaction of the following stages is carried out:
[0070] a. Control the pH value to 10.0-10.5, the ammonia concentration to 4g / L, and simultaneously introduce the complexing agent solution, the precipitant solution, the solution A and the doped metal salt solution into the reactor, control the flow rate of the complexing agent solution to 500ml / h, the flow rate of the precipitant solution to 1.2L / h, the flow rate of solution A to 3L / h, the flow rate of the strontium source to 400ml / h, so that the molar percentage of strontium solution added is 0.5%, and the internal nucleation is completed and grows to 3.5μm to form a stable core, and the first stage of the reaction is completed;
[0071] b. Stop the introduction of the doped metal salt solution, stabilize the pH and ammonia in the reaction system, control the pH value to 10.5-11.2, and the ammonia concentration to 7g / L, and successively introduce the complexing agent solution, the precipitant solution, the solution A1, and the solution B1 into the reactor to form shell 1, continue to introduce the complexing agent solution, the precipitant solution, the solution A2, and the solution B2 into the reactor to form shell 2, continue to introduce the complexing agent solution, the precipitant solution, the solution A3, and the solution B3 into the reactor to form shell 3, and continue to introduce the complexing agent solution, the precipitant solution, the solution A4, and the solution B5 into the reactor to form shell 4. Solution A4 and solution B4 form shell 4, and the complexing agent solution, precipitant solution, solution A5 and solution B5 are continuously introduced into the reactor to form shell 5; in the second stage of the reaction, the flow rate of the complexing agent solution is controlled to be 700 ml / L, the flow rate of the precipitant solution is 1.8 L / h, the flow rates of solutions A1, A2, A3, A4 and A5 are 3.5 L / h, 3 L / h, 2 L / h, 1 L / h and 0.5 L / h respectively, and the flow rates of solutions B1, B2, B3, B4 and B5 are 0.5 L / h, 1 L / h, 2 L / h, 3 L / h and 3.5 L / h respectively;
[0072] The obtained qualified slurry is washed and dried, wherein the washing is performed five times with hot water, and the drying is performed at a relatively low temperature of 90° C., thereby finally forming a doped and modified multi-shell ternary precursor.
[0073] Figure 1 The SEM image of the doped and modified multi-shell ternary precursor obtained in this embodiment is shown, and it can be seen that the primary particles present a flake-like morphology; Figure 2 The cross-sectional SEM image of the doped and modified multi-shell ternary precursor obtained in this embodiment is shown. It can be seen that the core is relatively loosely stacked, while the shell is relatively dense. The gradient distribution of the core-shell morphology is beneficial to improving the tap density of the material while taking into account the electrochemical cycle performance and capacity of the material.
[0074] Example 2
[0075] This embodiment provides a method for preparing a doped and modified multi-shell ternary precursor. Compared with Embodiment 1, the only difference is that the molar percentage of the added strontium solution is controlled to be 0.05%.
[0076] Example 3
[0077] This embodiment provides a method for preparing a doped and modified multi-shell ternary precursor. Compared with Embodiment 1, the only difference is that the molar percentage of the added strontium solution is controlled to be 0.1%.
[0078] Example 4
[0079] This embodiment provides a method for preparing a doped and modified multi-shell ternary precursor. Compared with Embodiment 1, the only difference is that the molar percentage of the added strontium solution is controlled to be 1%.
[0080] Example 5
[0081] This embodiment provides a method for preparing a doped and modified multi-shell ternary precursor. Compared with Embodiment 1, the only difference is that the molar percentage of the added strontium solution is controlled to be 5%.
[0082] Comparative Example 1
[0083] This comparative example provides a method for preparing a doped and modified multi-shell ternary precursor. Compared with Example 1, the only difference is that:
[0084] A total of 100 L of solution A and 20 L of solution B were prepared; 80 L of solution A was used for the first stage of coprecipitation, and the remaining solution A was divided into five parts, denoted as A1, A2, A3, A4, and A5, with volumes of V(A1) = 1 L, V(A2) = 2 L, V(A3) = 4 L, V(A4) = 6 L, and V(A5) = 7 L, respectively; solution B was divided into five parts, denoted as B1, B2, B3, B4, and B5, with volumes of V(B1) = 7 L, V(B2) = 6 L, V(B3) = 4 L, V(B4) = 2 L, and V(B5) = 1 L, respectively;
[0085] Correspondingly, the flow rates of solutions A1, A2, A3, A4, and A5 are 0.5 L / h, 1 L / h, 2 L / h, 3 L / h, and 3.5 L / h, respectively, and the flow rates of solutions B1, B2, B3, B4, and B5 are 3.5 L / h, 3 L / h, 2 L / h, 1 L / h, and 0.5 L / h, respectively.
[0086] Comparative Example 2
[0087] This comparative example provides a method for preparing a doped and modified multi-shell ternary precursor. Compared with Example 1, the only difference is that after the preparation of solution A and solution B is completed, the liquid separation process is no longer performed, that is, in the first stage coprecipitation, solution A is fully fed into the reaction, and in the second stage coprecipitation, solution B is fully fed into the reaction.
[0088] Comparative Example 3
[0089] This comparative example provides a method for preparing a doped and modified multi-shell ternary precursor. Compared with Example 1, the only difference is that there is no liquid separation process of solutions A1-A5 and a liquid separation process of solution B, that is, the reaction is stopped after the first stage reaction is completed, and the second stage of the reaction is not carried out, and the core is finally obtained.
[0090] Comparative Example 4
[0091] This comparative example provides a method for preparing a doped and modified multi-shell ternary precursor. Compared with Example 1, the only difference is that the introduction of the doping metal salt solution is omitted in the first stage of coprecipitation, that is, no doping is performed.
[0092] The precursor hydroxides prepared in the above embodiments and comparative examples are batch mixed with lithium hydroxide in a high-speed mixer, and the molar ratio of the total molar amount of nickel, cobalt and manganese in the precursor to the molar amount of lithium element in the lithium source is controlled to be 1:1.05. The obtained mixture is sintered in a box furnace. The target temperature of the first sintering stage is 450°C, the holding time is 5h, and the heating rate is 3°C / min. The target temperature of the second sintering stage is 850°C, the holding time is 20h, and the heating rate is 3°C / min. After the sintered materials are cooled, they are crushed and sieved to obtain lithium positive electrode materials; the respectively obtained lithium positive electrode materials are used as positive electrode active materials, and are mixed with conductive carbon and PVDF in a ratio of 94:3:3, and then the mixture is dispersed in methyl pyrrolidone (NMP) as a solvent to obtain a positive electrode slurry, which is evenly coated on an aluminum foil. After coating, the current collector is punched to obtain a coin-shaped electrode, and the positive electrode sheet is obtained after vacuum drying at 120°C overnight. Metal lithium is selected for the negative electrode, 1M LiPF6 is dissolved in EC and DMC solvents (volume ratio 3:7) as the electrolyte. The positive electrode, negative electrode and separator are wound to prepare the battery cell, which is then packaged, injected, formed and divided into volumes to assemble into a lithium-ion battery.
[0093] The prepared lithium-ion battery was subjected to electrochemical performance testing. At 0.1C, the + ) to measure the initial discharge capacity and initial efficiency, and the discharge capacity at the 100th time to obtain the capacity retention rate after 100 cycles. The test results are shown in Table 1.
[0094] Table 1
[0095] project First discharge capacity (mAh / g) First coulombic efficiency (%) Capacity retention rate (%) Example 1 215.5 93.8 89.2 Example 2 201.3 90.3 87.9 Example 3 210.7 91.7 88.5 Example 4 209.8 92.9 88.7 Example 5 198.6 89.4 87.1 Comparative Example 1 189.2 85.6 80.9 Comparative Example 2 195.8 88.3 85.2 Comparative Example 3 187.4 84.5 80.1 Comparative Example 4 194.9 87.8 84.4
[0096] Referring to Table 1, we can see that:
[0097] (1) The first discharge capacity, first coulombic efficiency and capacity retention rate of Example 1 are relatively high, which are 215.5 mAh / g, 93.8% and 89.2% respectively;
[0098] (2) Examples 1, 3, and 4 all achieved relatively good capacity and cycle performance, indicating that doping with strontium solution in the molar ratio range of 0.1-1% can further expand the interlayer spacing of metal ions, shorten the distance of lithium ion transmission, improve the rate performance and cycle performance of the material, and stabilize the crystal structure, thereby improving the safety during the electrochemical reaction process;
[0099] (3) By comparing Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3, it can be seen that the metal ions have a moderate concentration gradient diffusion between the core-shell and shell / shell, and the side reaction of the formed multi-shell positive electrode is reduced. + Dynamics enhancement.
[0100] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0101] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0102] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0103] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a doped and modified multi-shell ternary precursor, It is characterized in that The preparation method comprises the following steps: (1) preparing a first nickel-cobalt-manganese ternary solution as solution A, wherein the molar ratio of Ni:Co:Mn in solution A is x 1 :y 1 :z 1 ; Among them, 0.6<x 1 <0.9,0.1<y 1 <0.2, z 1 >0,x 1 +y 1 +z 1 =1; Prepare a second nickel-cobalt-manganese ternary solution as solution B, wherein the molar ratio of Ni:Co:Mn in solution B is x 2 :y 2 :z 2 ; Among them, 0.2<x 2 <0.4,0.2<y 2 <0.4, z 2 >0,x 2 +y 2 +z 2 =1; preparing a doping metal salt solution containing a doping element M, wherein the doping element M comprises at least one of aluminum, titanium, niobium, zirconium, tungsten, vanadium, strontium, gallium, cerium, yttrium or lanthanum; (2) Injecting the solution A, the doped metal salt solution, the complexing agent solution and the precipitant solution into the reaction base solution in parallel to perform the first stage of co-precipitation to achieve the first target particle size D50 1 Afterwards, a core is formed; (3) stopping the introduction of the doped metal salt solution, and injecting the solution A, the solution B, the complexing agent solution and the precipitant solution in parallel to perform the second stage of co-precipitation to form a shell layer 1; (4) Repeat step (3) at least 4 times, each time the total volume of the second-stage co-precipitation solution A gradually decreases, and each time the total volume of the second-stage co-precipitation solution B gradually increases, stop the reaction, and obtain a doped and modified multi-shell ternary precursor through solid-liquid separation.
2. The preparation method according to claim 1, It is characterized in that In step (1), the total concentration of ternary ions in solution A and solution B is the same, both of which are 20-120 g / L; Preferably, in step (1), the doping element M in the doping metal salt solution is strontium; Preferably, the strontium source in the doped metal salt solution includes at least one of strontium nitrate, strontium chloride, strontium acetate or strontium sulfate; Preferably, in step (1), the doping metal salt solution has a doping element M metal salt content of 10-50 g / L.
3. The preparation method according to claim 1 or 2, It is characterized in that In step (2), the doping amount of the doping element M is controlled to be 0.05-5% of the total molar amount of nickel, cobalt and manganese; Preferably, the reaction base liquid in step (2) is prepared from pure water, a precipitant and a complexing agent; Preferably, the temperature of the reaction base solution in step (2) is 50-70°C; Preferably, the pH value of the reaction base solution in step (2) is 11-13; Preferably, the concentration of the complexing agent in the reaction base solution in step (2) is 4-10 g / L; Preferably, before the parallel injection in step (2), N 2 and stir to control N 2 The entry rate is 0.2-2m 3 / h.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that In step (2), the flow rate of solution A is 2-4 L / h, the flow rate of the doped metal salt solution is 200-600 mL / h, the flow rate of the complexing agent solution is 400-600 mL / h, and the flow rate of the precipitant solution is 1-1.4 L / h.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that Step (2) The first target particle size D50 1 3-4μm.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that In step (3), the flow rate of the complexing agent solution is 600-800 mL / h, and the flow rate of the precipitant solution is 1.5-2.0 L / h.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that In step (4), the solid-liquid separation includes aging, washing, drying and post-treatment performed in sequence; Preferably, the washing comprises at least three washings with hot water; Preferably, the drying temperature is 100-150°C.
8. A doped and modified multi-shell ternary precursor, It is characterized in that It is prepared by the preparation method according to any one of claims 1 to 7, and the general formula is Ni a Co b Mn c Sr d (OH) 2 ; Among them, 0.6<a<0.9, 0<b<0.2, 0<c<0.2, 0<d<0.1, a+b+c+d=1.
9. Application of a doped and modified multi-shell ternary precursor, It is characterized in that The doped and modified multi-shell ternary precursor is uniformly mixed with a lithium source, and sintered at a high temperature to obtain a lithium positive electrode material; Wherein, the doped and modified multi-shell ternary precursor is prepared by the preparation method according to any one of claims 1 to 7, or the doped and modified multi-shell ternary precursor is the doped and modified multi-shell ternary precursor according to claim 8.
10. The use according to claim 9, It is characterized in that The molar ratio of the total molar amount of nickel, cobalt and manganese in the doped and modified multi-shell ternary precursor to the molar amount of lithium in the lithium source is 1:(1-1.1); Preferably, the high temperature sintering includes a first sintering stage and a second sintering stage; Preferably, the target temperature of the first sintering stage is 400-700°C, the holding time is 3-6h, and the heating rate is 2-6°C / min; Preferably, the target temperature of the second sintering stage is 700-1000° C., the holding time is 10-20 h, and the heating rate is 2-6° C. / min.
Citation Information
Cited By
Modified lithium-rich positive electrode material as well as preparation method and application thereof