Lithium-rich manganese-based oxide positive electrode material and preparation method and application thereof

By performing specific doping at lithium sites, transition metal sites and oxygen sites, lithium-rich manganese-based oxide positive electrode materials with pinning effects and other characteristics were prepared, which solved the first time that the Coulombian efficiency and poor circulation performance were low. The problem has achieved improvements in capacity and electrochemical performance.

CN119008927APending Publication Date: 2024-11-22BEIJING CHUANGNENG HUITONG TECH CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411130930.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The first Coulombic acid electrode material has low efficiency, voltage decay, capacity decay and poor rate performance during the cycle, which hinders its commercialization process.

Method used

By performing specific proportions and doping of elements at lithium sites, transition metal sites and oxygen sites, lithium-rich manganese-based oxide positive electrode materials with pinning effects, pillar effects, fast ion conductors and other characteristics are prepared to improve The conductivity and crystal structure stability of the material improve Li+ deintercalation kinetics.

Benefits of technology

It improves the capacity and electrochemical performance of the material, stabilizes the structure, improves the electrochemical performance of lithium-rich materials, and significantly improves the charge and discharge efficiency and cycling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008927A_ABST
    Figure CN119008927A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium-rich manganese-based oxide positive electrode material as well as a preparation method and application thereof. The chemical general formula of the positive electrode material is Li (a-x) A (x) Ni (b) Mn (c) B (y) O (2-z) C (z), wherein A is selected from at least one of Na, K, Mg, Ti and Zn; b is selected from at least one of W, Zr, Al, Mo, La, Y, Nb, Ti, Sc and Ce; c is selected from at least one of B, P, Si, S, Cl, F and N, 1.05 < = a < = 1.23, 0 < b < = 0.48, 0.38 < = c < = 0.95, 0 < x < = 0.05, 0 < y < = 0.2, 0 < z < = 0.05, and a + b + c + y = 2. The lithium-rich manganese-based oxide positive electrode material with the characteristics of pinning effect, pillar effect, fast ion conductor and the like is prepared through multi-site doping, and the electrochemical performance of the lithium-rich material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a lithium-rich manganese-based oxide positive electrode material and a preparation method and application thereof. Background Art

[0002] The over-exploitation and use of non-renewable fossil fuels pose a serious threat to the global ecosystem, and the development of clean and convenient renewable energy has become particularly important. As an effective energy storage device, lithium-ion batteries are widely used in 3C electronic products and rail transportation vehicles. Since they were successfully commercialized by Sony in 1991, they have received continuous attention from the two major fields of science and technology. Since the discharge capacity of commercial graphite negative electrode materials exceeds 350mAh / g, which has far exceeded the market demand, it is particularly important to seek high energy density positive electrode materials.

[0003] Layered lithium-rich manganese-based cathode material xLi 2 MnO 3 (1-x)LiTMO 2 With its advantages of high specific capacity (≈250mAh / g), high operating voltage (≈3.6V), low cost and good thermal stability, it has attracted extensive research and is expected to become the next generation of lithium-ion battery positive electrode materials. However, due to its structural characteristics and the complexity of the charge and discharge mechanism, the low first coulombic efficiency of lithium-rich manganese-based materials, the voltage decay and capacity decay during the cycle, and the poor rate performance have seriously hindered its commercialization process.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a lithium-rich manganese-based oxide positive electrode material and a preparation method and application thereof, so as to improve the above technical problems.

[0006] The present invention is achieved in that:

[0007] In the first aspect, the present invention provides a lithium-rich manganese-based oxide positive electrode material, the chemical formula of which is: Li a- x A x Ni b Mn c B y O 2-z C z; wherein A is a Li site doping element, A is selected from at least one of Na, K, Mg, Ti and Zn; B is a transition metal site doping element, B is selected from at least one of W, Zr, Al, Mo, La, Y, Nb, Ti, Sc and Ce; C is an oxygen site doping element, C is selected from at least one of B, P, Si, S, Cl, F and N, and 1.05≤a≤1.23, 0<b≤0.48, 0.38≤c≤0.95, 0<x≤0.05, 0<y≤0.2, 0<z≤0.05, a+b+c+y=2.

[0008] Optionally, A is selected from any one of Mg, Ti and Zn; B is selected from any one of W, Mo, Nb and Ce; and C is selected from any one of B, P and S.

[0009] Optionally, A is Mg, B is W, and C is P.

[0010] Optionally, 1.12≤a≤1.13, 0.2<b≤0.4, 0.5≤c≤0.65, 0<x≤0.006, 0.001<y≤0.005, 0.001<z≤0.005.

[0011] Optionally, 1.12≤a≤1.13, 0.3<b≤0.35, 0.5≤c≤0.6, 0.003≤x≤0.006, 0.002≤y≤0.004, 0.003≤z≤0.005.

[0012] In a second aspect, the present invention provides a method for preparing the above-mentioned lithium-rich manganese-based oxide positive electrode material, which comprises: obtaining a raw material mixture of a nickel-manganese precursor, a lithium source, a lithium site additive, a transition metal site additive and an oxygen site additive according to the molar ratio of elements in the chemical formula; and sintering the raw material mixture.

[0013] Optionally, the preparation steps of the above-mentioned raw material mixture include: weighing the nickel manganese precursor, lithium source, lithium site additive, transition metal site additive and oxygen site additive according to a lithium molar ratio of Li / TM=1.1~1.6, and adding the doping element at a ratio of 0~5wt% of the precursor mass, and uniformly mixing them in a high-speed mixer.

[0014] Optionally, the speed of the high-speed mixer is 100-3000 r / min, the material temperature is controlled at 20-150° C., gas is introduced during the mixing process, the gas flow rate is 50-200 L / min, and the gas pressure is 0.2-0.5 MPa.

[0015] Optionally, the particle sizes of the nickel manganese precursor and the lithium source are both 0.5 μm to 20 μm, and the particle sizes of the lithium site additive, the transition metal site additive and the oxygen site additive are all 5 nm to 500 nm.

[0016] Optionally, the nickel-manganese precursor is selected from Ni e Mn f CO 3 and Ni e Mn f (OH) 2 At least one of the following, wherein 0≤e≤0.5, 0.5≤f≤1, and e+f=1.

[0017] Optionally, the lithium source is selected from Li 2 CO 3 、LiOH、LiOH·H 2 O. Li 2 O. Li 2 O 2 , at least one of lithium acetate, lithium oxalate and lithium nitrate.

[0018] Optionally, the lithium site additive is selected from at least one of compounds containing Na, K, Mg, Ti or Zn, preferably at least one of sodium carbonate, sodium bicarbonate, sodium oxalate, sodium acetate, sodium citrate, sodium chloride, sodium nitrate, sodium sulfate, sodium hydroxide, potassium carbonate, potassium bicarbonate, potassium oxalate, potassium acetate, potassium citrate, potassium chloride, potassium nitrate, potassium sulfate, potassium hydroxide, magnesium carbonate, magnesium hydroxide, magnesium oxide, lithium oxalate, magnesium chloride, magnesium sulfate, zinc oxide, zinc hydroxide, zinc carbonate and zinc chloride.

[0019] Optionally, the transition metal site additive is selected from at least one of compounds containing W, Zr, Al, Mo, La, Y, Nb, Ti, Sc or Ce, preferably at least one of tungsten trioxide, ammonium tungstate, niobium pentoxide, niobium acetate, zirconium oxide, zirconium carbonate, zirconium hydroxide, zirconium acetate, zirconium nitrate, zirconium chloride, titanium dioxide, titanium hydroxide, titanium sulfate, aluminum trioxide, aluminum carbonate, aluminum hydroxide, aluminum oxide monohydrate, molybdenum trioxide, lanthanum oxide, yttrium oxide, scandium oxide and cerium oxide.

[0020] Optionally, the oxygen site additive is selected from at least one of compounds containing B, P, Si, S, Cl, F or N, preferably at least one of diammonium phosphate, diammonium hydrogen phosphate, boric acid, ammonium fluoride, ammonium sulfide, molybdenum disulfide, tungsten disulfide, ammonium sulfate, ammonium chloride, silicon dioxide and silica gel.

[0021] Optionally, sintering includes placing the raw material mixture in a crucible and dividing it into a plurality of block regions, and then sintering, and at least one of the following conditions is met:

[0022] (1) The charge is less than or equal to 80% of the total capacity of the crucible;

[0023] (2) Sintering in an air atmosphere with the air flow rate controlled at 10 mL / min to 200 mL / min;

[0024] (3) First raise the temperature to 400°C to 600°C, keep it for 0h to 10h, then raise the temperature to 800°C to 1000°C, preferably 860°C to 900°C, keep it for 5h to 25h, and preferably the heating rate is 0.5°C / min to 10°C / min.

[0025] In a third aspect, the present invention also provides the use of the above-mentioned lithium-rich manganese-based oxide positive electrode material in the preparation of a positive electrode for a lithium-ion battery.

[0026] In a fourth aspect, the present invention further provides a lithium-ion battery, which includes a lithium-ion battery positive electrode prepared by the above application.

[0027] The present invention has the following beneficial effects: by realizing doping of specific proportions and specific elements at different sites, multiple doping elements play a better coordination role, and a lithium-rich manganese-based oxide positive electrode material with pinning effect, pillar effect, fast ion conductor and other characteristics is obtained, the conductivity of the material is improved, the crystal structure is stabilized, the unit cell parameters are increased, and the Li + The insertion and extraction kinetics can improve the material capacity while stabilizing the material structure, thereby improving the electrochemical properties of lithium-rich materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0029] Figure 1 This is a scanning electron microscope image of the lithium-rich manganese-based oxide positive electrode material prepared in Example 1 of the present invention;

[0030] Figure 2 This is a scanning electron microscope image of the additive-free lithium-rich manganese-based positive electrode material prepared in Comparative Example 1 of the present invention;

[0031] Figure 3 The discharge specific capacity cycle curves of the lithium-rich manganese-based oxide positive electrode material prepared in Example 1 of the present invention and the lithium-rich manganese-based positive electrode material prepared in Comparative Example 1 at a rate of 0.5C;

[0032] Figure 4 The first cycle charge and discharge curves of the lithium-rich manganese-based oxide positive electrode material prepared in Example 1 of the present invention and the lithium-rich manganese-based positive electrode material prepared in Comparative Example 1 at a rate of 0.1C. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0034] The following is a detailed description of a lithium-rich manganese-based oxide positive electrode material disclosed in the present invention, as well as a preparation method and application thereof.

[0035] Some embodiments of the present invention provide a lithium-rich manganese-based oxide positive electrode material, the general chemical formula of which is: Li a-x A x Ni b Mn c B y O 2-z C z ; wherein A is a Li site doping element, A is selected from at least one of Na, K, Mg, Ti and Zn; B is a transition metal site doping element, B is selected from at least one of W, Zr, Al, Mo, La, Y, Nb, Ti, Sc and Ce; C is an oxygen site doping element, C is selected from at least one of B, P, Si, S, Cl, F and N, and 1.05≤a≤1.23, 0<b≤0.48, 0.38≤c≤0.95, 0<x≤0.05, 0<y≤0.2, 0<z≤0.05, a+b+c+y=2.

[0036] Based on the existing modification methods, the inventors creatively proposed to achieve the doping of specific proportions and specific elements at different sites, realize the coordination of multiple doping elements, and obtain lithium-rich manganese-based oxide positive electrode materials with pinning effect, pillar effect, fast ion conductor and other characteristics, improve the conductivity of the material, stabilize the crystal structure, increase the unit cell parameters, and improve the Li + The insertion and extraction kinetics can improve the material capacity while stabilizing the material structure, thereby improving the electrochemical properties of lithium-rich materials.

[0037] For reference, A is selected from any one of Mg, Ti and Zn. B is selected from any one of W, Mo, Nb and Ce. C is selected from any one of B, P and S. For example, Nb 2 O 5 As Nb 5+ The additive can form Nb-O bonds to passivate the material surface. 5+ Doping increases the energy barrier for transition metal migration and inhibits the material phase transition caused by transition metal migration.

[0038] Furthermore, the inventors have found through extensive research and practice that different doping elements and corresponding combinations of different doping elements also show unexpected electrochemical performance improvement effects to a certain extent. Therefore, in some preferred embodiments, A is Mg, B is W, and C is P. This combination of elements shows better electrochemical material performance, which may be due to the fact that phosphorus will be converted into Li during the sintering process. 3 PO 4 phase, with extremely high Li + Conductivity, which can enhance the Li + The diffusion rate is increased, thus achieving the effect of rapid ion transmission. 3 As W 6+ The doping of W element is beneficial to improve the electronic conductivity of the material. 6+ A larger radius can partially replace the position of the transition metal, increase the interlayer spacing, increase the difficulty of nickel migrating to the lithium layer, and ensure that the detached lithium can return to its original position.

[0039] Furthermore, the ratio of various elements also has a certain degree of influence on the performance of the positive electrode material. Therefore, as a reference, in some embodiments, 1.12≤a≤1.13, 0.2<b≤0.4, 0.5≤c≤0.65, 0<x≤0.006, 0.001<y≤0.005, 0.001<z≤0.005.

[0040] For example, 1.12≤a≤1.13, 0.3<b≤0.35, 0.5≤c≤0.6, 0.003≤x≤0.006, 0.002≤y≤0.004, 0.003≤z≤0.005.

[0041] Furthermore, some embodiments of the present invention also provide a method for preparing the above-mentioned lithium-rich manganese-based oxide positive electrode material, which includes: obtaining a raw material mixture of a nickel-manganese precursor, a lithium source, a lithium site additive, a transition metal site additive and an oxygen site additive according to the molar ratio of elements in the chemical formula; and sintering the raw material mixture.

[0042] The preparation method has low raw material cost, very simple process operation, and high matching degree with the current production line, which is suitable for industrial production. The electrochemical performance of the modified lithium-rich manganese-based oxide positive electrode material is significantly improved. The modification method has both ionic and electronic conductivity modification characteristics, improves material conductivity, stabilizes crystal structure, increases unit cell parameters, and improves Li + The electrochemical performance of the material can be improved.

[0043] For reference, some embodiments provide a method for preparing a lithium-rich manganese-based oxide positive electrode material, which specifically includes the following steps:

[0044] S1. Mix the raw materials.

[0045] Specifically, the nickel-manganese precursor, the lithium source, the lithium site additive, the transition metal site additive and the oxygen site additive are weighed according to the molar ratio of the elements in the chemical formula, and then mixed by a high-speed mixer.

[0046] In some embodiments, the nickel manganese precursor, lithium source, lithium site additive, transition metal site additive and oxygen site additive are weighed according to a lithium molar ratio of Li / TM=1.1-1.6 and an element addition ratio of 0-5wt% of the precursor mass.

[0047] In order to ensure that the raw materials are fully mixed and have better sintering performance in the subsequent sintering process, in some embodiments, the particle size of the nickel manganese precursor and the lithium source is selected to be 0.5μm~20μm, and the particle size of the lithium site additive, transition metal site additive and oxygen site additive is selected to be 5nm~500nm.

[0048] For reference, nickel-manganese precursors include but are not limited to Ni e Mn f CO 3 and Ni e Mn f (OH) 2 At least one of the two, that is, it can be any one of the two, or a mixture of the two, and the mixing ratio is not limited, wherein 0≤e≤0.5, 0.5≤f≤1, e+f=1.

[0049] For reference, lithium sources include but are not limited to Li 2 CO 3 、LiOH、LiOH·H 2 O. Li 2 O. Li 2 O 2 , lithium acetate, lithium oxalate and lithium nitrate, that is, any one of the above substances can be selected, or a combination of two or more of them can be selected.

[0050] For reference, the lithium site additive includes but is not limited to at least one of compounds containing Na, K, Mg, Ti or Zn, preferably at least one of sodium carbonate, sodium bicarbonate, sodium oxalate, sodium acetate, sodium citrate, sodium chloride, sodium nitrate, sodium sulfate, sodium hydroxide, potassium carbonate, potassium bicarbonate, potassium oxalate, potassium acetate, potassium citrate, potassium chloride, potassium nitrate, potassium sulfate, potassium hydroxide, magnesium carbonate, magnesium hydroxide, magnesium oxide, lithium oxalate, magnesium chloride, magnesium sulfate, zinc oxide, zinc hydroxide, zinc carbonate and zinc chloride, that is, any one of the above substances can be selected, or a combination of two or more of them can be selected.

[0051] For reference, the transition metal site additives include but are not limited to at least one of compounds containing W, Zr, Al, Mo, La, Y, Nb, Ti, Sc or Ce, preferably at least one of tungsten trioxide, ammonium tungstate, niobium pentoxide, niobium acetate, zirconium oxide, zirconium carbonate, zirconium hydroxide, zirconium acetate, zirconium nitrate, zirconium chloride, titanium dioxide, titanium hydroxide, titanium sulfate, aluminum trioxide, aluminum carbonate, aluminum hydroxide, aluminum oxide monohydrate, molybdenum trioxide, lanthanum oxide, yttrium oxide, scandium oxide and cerium oxide. Any one of the above substances can be selected, or a combination of two or more of them can be selected.

[0052] For reference, the oxygen site additive includes but is not limited to at least one of compounds containing B, P, Si, S, Cl, F or N, preferably at least one of diammonium phosphate, diammonium hydrogen phosphate, boric acid, ammonium fluoride, ammonium sulfide, molybdenum disulfide, tungsten disulfide, ammonium sulfate, ammonium chloride, silicon dioxide and silica gel, that is, any one of the above substances can be selected, or a combination of two or more of them can be selected.

[0053] In some embodiments, in order to make the various raw materials fully mixed, the speed of the high-speed mixer is 100 to 3000 r / min, for example, 100 r / min, 200 r / min, 300 r / min, 500 r / min, 800 r / min, 1000 r / min, 1300 r / min, 1500 r / min, 1800 r / min, 2000 r / min, 2500 r / min or 3000 r / min, and the material temperature is controlled at 20 to 150 ° C, for example, 20 ° C, 30 ° C, 40 ° C, 50 ° C, 60 ° C, 70 ° C , 80℃, 90℃, 100℃, 110℃, 120℃, 130℃, 140℃ or 150℃, etc., gas is introduced into the mixing process, the gas flow rate is 50-200L / min, such as 50L / min, 60L / min, 70L / min, 80L / min, 90L / min, 100L / min, 120L / min, 140L / min, 160L / min, 180L / min or 200L / min, etc., and the gas pressure is 0.2-0.5MPa, such as 0.2MPa, 0.3MPa, 0.4MPa or 0.5MPa, etc. It should be noted that the gas introduced can be an inert gas or air. Generally speaking, air is better and has a lower cost. By passing a certain pressure of gas through the high-speed mixer, turbulence and agitation can be generated, which promotes full contact and uniform distribution between different materials and improves the efficiency and quality of mixing. At the same time, a certain air pressure can exert a certain pressure on the materials, making the materials more closely combined, which is beneficial to the subsequent sintering effect.

[0054] In some embodiments, sintering includes placing the raw material mixture in a crucible and dividing it into a plurality of square regions, and then sintering, and at least one of the following conditions is met:

[0055] (1) The charge is less than or equal to 80% of the total capacity of the crucible;

[0056] (2) Sintering in an air atmosphere with an air flow rate controlled between 10 mL / min and 200 mL / min, for example, 10 mL / min, 20 mL / min, 30 mL / min, 40 mL / min, 50 mL / min, 60 mL / min, 70 mL / min, 80 mL / min, 90 mL / min, 100 mL / min, 110 mL / min, 120 mL / min, 130 mL / min, 140 mL / min, 150 mL / min, 160 mL / min, 170 mL / min, 180 mL / min, 190 mL / min or 200 mL / min, or between any two of the above values.

[0057] (3) first heating to 400°C to 600°C, keeping the temperature for 0h to 10h, then heating to 800°C to 1000°C, for example, 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C, 950°C, 960°C, 970°C, 980°C, 990°C or 1000°C, or between any two temperatures above, preferably 860°C to 900°C, and keeping the temperature for 5h to 25h, for example, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h The temperature may be varied from 0.1 to 10 ℃ / min, for example, 0.5 ℃ / min, 1 ℃ / min, 1.5 ℃ / min, 2 ℃ / min, 2.5 ℃ / min, 3 ℃ / min, 3.5 ℃ / min, 4 ℃ / min, 4.5 ℃ / min, 5 ℃ / min, 5.5 ℃ / min, 6 ℃ / min, 6.5 ℃ / min, 7 ℃ / min, 7.5 ℃ / min, 8 ℃ / min, 8.5 ℃ / min, 9 ℃ / min, 9.5 ℃ / min or 10 ℃ / min, or a rate between any two of the above temperature rise rates.

[0058] Some embodiments of the present invention also provide the use of the above-mentioned lithium-rich manganese-based oxide positive electrode material in the preparation of lithium-ion battery positive electrodes. Generally speaking, the battery positive electrode raw materials also include adhesives and conductive agents.

[0059] Some embodiments of the present invention further provide a lithium-ion battery, which includes a lithium-ion battery positive electrode prepared by the above application. Generally speaking, the lithium-ion battery also includes a negative electrode and a separator.

[0060] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0061] Example 1

[0062] This embodiment provides a method for preparing a lithium-rich manganese-based oxide positive electrode material, which comprises the following steps:

[0063] According to the lithium molar ratio of Li / TM=1.3, weigh the precursor Ni 0.35 Mn 0.65 (OH) 2 and lithium carbonate, and then weigh elemental additives such as magnesium oxide, tungsten oxide, and ammonium dihydrogen phosphate, so that Mg, W, and P account for 0.1wt%, 0.5wt%, and 0.1wt% of the precursor, respectively. The particle sizes of the precursor and lithium carbonate are both 0.5-20μm, and the particle sizes of the elemental additives are both 5-500nm.

[0064] Pour the above materials into a high-speed mixer for mixing, first perform preliminary mixing at a speed of 500r / min, then perform further mixing at a speed of 1000r / min, and finally perform uniform mixing at 2000r / min, the gas (air) flow rate is 100L / min, the air pressure is 0.3MPa, turn on the water cooling to control the temperature of the mixture at 35-40°C, after sufficient mixing, pour the raw material mixture into a corundum crucible, the mixture is roughly 1 / 3 of the total capacity of the crucible, and the mixture is divided into multiple small square areas. Put the loaded crucible into a muffle furnace, set the air flow rate to 80mL / min, first heat up to 500 at 2℃ / min and keep warm for 5h, then heat up to 880℃ at 5℃ / min and keep warm for 12h.

[0065] After natural cooling, the lithium-rich manganese-based oxide positive electrode material Li was sieved using a 400-mesh sieve. 1.127 Mg 0.003 Ni 0.304 Mn 0.564 W 0.002 O 1.997 P 0.003 .

[0066] Example 2

[0067] This embodiment provides a method for preparing a lithium-rich manganese-based oxide positive electrode material. The only difference between this embodiment and embodiment 1 is that the element additives added are zinc oxide, niobium pentoxide, and boric acid, so that Zn, Nb, and B account for 0.1wt%, 0.5wt%, and 0.05wt% of the precursor, respectively. Finally, a lithium-rich manganese-based oxide positive electrode material Li 1.127 Zn 0.001 Ni 0.304 Mn 0.564 Nb 0.004 O 1.996 B 0.004 .

[0068] Example 3

[0069] This embodiment provides a method for preparing a lithium-rich manganese-based oxide positive electrode material. The only difference between this embodiment and embodiment 1 is that the element additives added are titanium dioxide, molybdenum trioxide, and molybdenum disulfide, so that Ti, Mo, and S account for 0.1wt%, 0.5wt%, and 0.1wt% of the precursor, respectively. Finally, a lithium-rich manganese-based oxide positive electrode material Li 1.127 Ti 0.002 Ni 0.303 Mn 0.564 Mo 0.004 O 1.998 S 0.002 .

[0070] Example 4

[0071] This embodiment provides a method for preparing a lithium-rich manganese-based oxide positive electrode material. The only difference between this embodiment and embodiment 1 is that the element additives added are magnesium oxide, cerium oxide, and ammonium dihydrogen phosphate, so that Mg, Ce, and P account for 0.1wt%, 0.5wt%, and 0.1wt% of the precursor, respectively. Finally, a lithium-rich manganese-based oxide positive electrode material Li 1.127 Mg 0.003 Ni 0.303 Mn 0.564 Ce 0.003 O 1.997 P 0.003 .

[0072] Example 5

[0073] This embodiment provides a method for preparing a lithium-rich manganese-based oxide positive electrode material. The only difference between this embodiment and embodiment 1 is that the element additives added are zinc oxide, zirconium oxide, and boric acid, so that Zn, Zr, and B account for 0.1wt%, 0.5wt%, and 0.05wt% of the precursor, respectively. Finally, a lithium-rich manganese-based oxide positive electrode material Li 1.127 Zn 0.001 Ni 0.304 Mn 0.564 Zr 0.004 O 1.996 B 0.004 .

[0074] Example 6

[0075] This embodiment provides a method for preparing a lithium-rich manganese-based oxide positive electrode material. The only difference between this embodiment and embodiment 1 is that the element additives added are magnesium oxide, tungsten trioxide, and ammonium dihydrogen phosphate, so that Mg, W, and P account for 0.1wt%, 0.8wt%, and 0.1wt% of the precursor, respectively. Finally, a lithium-rich manganese-based oxide positive electrode material Li 1.127 Mg 0.003 Ni 0.303 Mn 0.563 W 0.003 O 1.997 P 0.003 .

[0076] Example 7

[0077] This embodiment provides a method for preparing a lithium-rich manganese-based oxide positive electrode material. The only difference between this embodiment and embodiment 1 is that the element additives added are magnesium oxide, tungsten trioxide, and ammonium dihydrogen phosphate, so that Mg, W, and P account for 0.2wt%, 0.5wt%, and 0.1wt% of the precursor, respectively. Finally, a lithium-rich manganese-based oxide positive electrode material Li 1.126 Mg0.006 Ni 0.303 Mn 0.563 W 0.002 O 1.997 P 0.003 .

[0078] Example 8

[0079] This embodiment provides a method for preparing a lithium-rich manganese-based oxide positive electrode material. The only difference between this embodiment and embodiment 1 is that the element additives added are magnesium oxide, tungsten trioxide, and ammonium dihydrogen phosphate, so that Mg, W, and P account for 0.1wt%, 0.5wt%, and 0.2wt% of the precursor, respectively. Finally, a lithium-rich manganese-based oxide positive electrode material Li 1.127 Mg 0.003 Ni 0.304 Mn 0.564 W 0.002 O 1.995 P 0.005 .

[0080] Example 9

[0081] This embodiment provides a method for preparing a lithium-rich manganese-based oxide positive electrode material. The only difference between this embodiment and embodiment 1 is that the sintering temperature in the second stage is 860°C, and the other conditions and parameters are exactly the same as those in embodiment 1. Finally, a lithium-rich manganese-based oxide positive electrode material Li 1.127 Mg 0.003 Ni 0.304 Mn 0.564 W 0.002 O 1.997 P 0.003 .

[0082] Example 10

[0083] This embodiment provides a method for preparing a lithium-rich manganese-based oxide positive electrode material. The only difference between this embodiment and embodiment 1 is that the sintering temperature in the second stage is 900°C, and the other conditions and parameters are exactly the same as those in embodiment 1. Finally, a lithium-rich manganese-based oxide positive electrode material Li 1.127 Mg 0.003 Ni 0.304 Mn 0.564 W 0.002 O 1.997 P 0.003 .

[0084] Embodiment 11

[0085] The difference between this embodiment and embodiment 1 is that the precursor Ni is weighed according to the lithium molar ratio of Li / TM=1.4. 0.35 Mn 0.65 (OH) 2The other conditions are exactly the same as those in Example 1 to obtain a lithium-rich manganese-based oxide positive electrode material Li 1.214 Mg 0.003 Ni 0.304 Mn 0.564 W 0.002 O 1.997 P 0.003 .

[0086] Example 12

[0087] The difference between this embodiment and embodiment 1 is that the precursor is Ni 0.37 Mn 0.63 (OH) 2 , other conditions and parameters are exactly the same as those in Example 1, and finally a lithium-rich manganese-based oxide positive electrode material Li 1.127 Mg 0.003 Ni 0.321 Mn 0.546 W 0.00 2 O 1.997 P 0.003 .

[0088] Comparative Example 1

[0089] The only difference between this comparative example and Example 1 is that no element additive is added, and other conditions and parameters are exactly the same as those in Example 1 to obtain a lithium-rich manganese-based oxide positive electrode material Li 1.130 Ni 0.304 Mn 0.565 O 2 .

[0090] Comparative Example 2

[0091] The difference between this comparative example and Example 1 is that the element additive is only tungsten oxide, so that W accounts for 0.5wt% of the precursor, and the other conditions and parameters are exactly the same as those in Example 1 to obtain a lithium-rich manganese-based oxide positive electrode material Li 1.129 Ni 0.304 Mn 0.565 W 0.002 O 2 .

[0092] Comparative Example 3

[0093] The only difference between this comparative example and Example 1 is that the element additive is only niobium pentoxide, so that Nb accounts for 0.5wt% of the precursor. The other conditions and parameters are exactly the same as those in Example 1. 1.128 Ni 0.304 Mn 0.564 Nb 0.004 O 2 .

[0094] Comparative Example 4

[0095] The only difference between this comparative example and Example 1 is that the element additive is only magnesium oxide, so that Mg accounts for 0.1wt% of the precursor. The other conditions and parameters are exactly the same as those in Example 1 to obtain a lithium-rich manganese-based oxide positive electrode material Li 1.129 Mg 0.003 Ni 0.304 Mn 0.564 O 2 .

[0096] Comparative Example 5

[0097] The difference between this comparative example and Example 1 is that the element additive is only zinc oxide, so that Zn accounts for 0.1wt% of the precursor, and the other conditions and parameters are exactly the same as those in Example 1 to obtain a lithium-rich manganese-based oxide positive electrode material Li 1.130 Zn 0.001 Ni 0.304 Mn 0.565 O 2 .

[0098] Comparative Example 6

[0099] The difference between this comparative example and Example 1 is that the element additive is only ammonium dihydrogen phosphate, so that P accounts for 0.1wt% of the precursor. The other conditions and parameters are exactly the same as those in Example 1 to obtain a lithium-rich manganese-based oxide positive electrode material Li 1.130 Ni 0.304 Mn 0.565 O 1.997 P 0.003 .

[0100] Comparative Example 7

[0101] The only difference between this comparative example and Example 1 is that the element additive is only boric acid, so that B accounts for 0.05wt% of the precursor. The other conditions and parameters are exactly the same as those in Example 1 to obtain a lithium-rich manganese-based oxide positive electrode material Li 1.130 Ni 0.304 Mn 0.565 O 1.996 B 0.004 .

[0102] Comparative Example 8

[0103] The only difference between this comparative example and Example 1 is that element additives magnesium oxide and ammonium dihydrogen phosphate are added so that Mg and P account for 0.1wt% and 0.1wt% of the precursor respectively. Other conditions and parameters are exactly the same as those in Example 1. The lithium-rich manganese-based material Li modified by two site elements is obtained. 1.129 Mg 0.003 Ni0.304 Mn 0.564 O 1.997 P 0.003 .

[0104] The electrochemical performance of the positive electrode materials prepared in the above examples and comparative examples was evaluated, and the specific evaluation method is as follows:

[0105] The positive electrode materials of each embodiment and comparative example are weighed with conductive carbon black and polyvinylidene fluoride adhesive in a mass ratio of 90:5:5 and mixed to form a uniform slurry. The slurry is evenly scraped on the carbon-coated aluminum foil and transferred to a vacuum oven at 100°C. After being completely dried, the aluminum foil is cut into positive electrode sheets for standby use. The metal lithium sheet is used as the negative electrode, the double-sided ceramic coating film (12μm dry base film + 2μm double-sided ceramic layer) is used as the diaphragm, and the electrolyte is the lithium-ion battery high-voltage electrolyte produced by Zhangjiagang Guotai Huarong Chemical New Materials Co., Ltd., which is assembled into a CR2032 button battery in a glove box protected by an argon atmosphere.

[0106] The electrical performance test conditions are: charge and discharge voltage range 2.8V ~ 4.55V, test temperature 25℃. First, activate once at a rate of 0.1C in the voltage range of 2.8 ~ 4.55V, then test the activated button cell at 0.33C and 0.5C rates in the same voltage range, and perform a cycle test at 0.5C rate.

[0107] The test results are shown in Table 1 and Table 2.

[0108] Table 1

[0109]

[0110]

[0111] Table 2

[0112]

[0113] As can be seen from Table 1, from Examples 1-12 and Comparative Example 1, the charge and discharge efficiency of the lithium-rich manganese-based positive electrode material prepared by the modification method of the present invention is improved compared with the unmodified positive electrode material, and the discharge capacity at each rate is also improved by more than 10 mAh / g.

[0114] As can be seen from Table 2, from Examples 1 to 12, the discharge capacity of the battery made of the lithium-rich manganese-based positive electrode material prepared by the modification method of the present invention can reach more than 199 mAh / g at a rate of 0.5C in the voltage range of 2.8 to 4.55 V, and the capacity has no attenuation for 50 weeks and the retention rate is more than 100%, and the capacity retention rate for 100 weeks is more than 98%. The multi-dimensional synergistically modified lithium-rich manganese-based positive electrode materials in Examples 1 to 11 have a significant improvement in cycle performance compared to the single-element modified lithium-rich manganese-based positive electrode materials of Comparative Examples 2-7.

[0115] Further comparison of the data in Example 1 and Examples 6-8 shows that the doping of tungsten in the multi-dimensional synergistically modified lithium-rich manganese-based positive electrode material has a significant improvement in the charge and discharge capacity, even in the case of only adding tungsten in Comparative Example 2, there is a high discharge capacity of 227.51 mAh / g at 0.1C. And increasing the content of tungsten and phosphorus on the basis of Example 1 can further improve the charge and discharge capacity performance of the material. In addition, it can be obtained from Examples 1 and 9-10 that the optimal sintering temperature for obtaining a lithium-rich manganese-based positive electrode material is 880°C. Comparison of the results of Example 1 and Example 11 shows that increasing the amount of lithium during mixing will reduce the charge and discharge capacity of the prepared positive electrode material, and the capacity cycle retention rate is improved due to the lithium supplementation effect. Comparison of Example 1 and Example 12 shows that the charge and discharge capacity of the prepared positive electrode material can be improved by selecting a precursor with a higher nickel content.

[0116] The comparison between Example 1 and Comparative Example 8 further confirms that tungsten doping has a significant effect on improving the charge and discharge capacity.

[0117] The positive electrode materials obtained in Example 1 and the comparative example were respectively observed by scanning electron microscope for microscopic morphology, and the results are as follows: Figure 1 and Figure 2 The discharge capacity cycle curves of the positive electrode materials obtained in Example 1 and the comparative example at a rate of 0.5C obtained by the above performance test are shown in FIG. Figure 3 As shown, the first cycle charge and discharge curve at 0.1C rate is as follows Figure 4 As shown. Figure 1-Figure 4 It can also be obtained that after modification by doping with multiple elements, the morphology of the lithium-rich manganese-based positive electrode material has been optimized, and its first charge performance and cycle performance have been significantly improved.

[0118] In summary, the embodiments of the present invention prepare a lithium-rich manganese-based oxide positive electrode material having properties such as pinning effect, pillar effect, and fast ion conductor through multi-site doping of lithium sites, transition metal sites, and oxygen sites. This method has a simple doping process and can stabilize the structure of the material while increasing the material capacity, thereby improving the electrochemical properties of the lithium-rich material.

[0119] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A lithium-rich manganese-based oxide positive electrode material, characterized in that: Its general chemical formula is: Li a-x A x Ni b Mr c B y O 2-z C z ; Wherein A is a Li site doping element, A is selected from at least one of Na, K, Mg, Ti and Zn; B is a transition metal site doping element, B is selected from at least one of W, Zr, Al, Mo, La, Y, Nb, Ti, Sc and Ce; C is an oxygen site doping element, C is selected from at least one of B, P, Si, S, Cl, F and N, and 1.05≤a≤1.23, 0<b≤0.48, 0.38≤c≤0.95, 0<x≤0.05, 0<y≤0.2, 0<z≤0.05, a+b+c+y=2.

2. The lithium-rich manganese-based oxide positive electrode material according to claim 1, characterized in that: A is selected from any one of Mg, Ti and Zn; B is selected from any one of W, Mo, Nb and Ce; C is selected from any one of B, P and S; Preferably, A is Mg, B is W, and C is P.

3. The lithium-rich manganese-based oxide positive electrode material according to claim 1 or 2, characterized in that: 1.12≤a≤1.13, 0.2<b≤0.4, 0.5≤c≤0.65, 0<x≤0.006, 0.001<y≤0.005, 0.001<z≤0.005; Preferably, 1.12≤a≤1.13, 0.3<b≤0.35, 0.5≤c≤0.6, 0.003≤x≤0.006, 0.002≤y≤0.004, and 0.003≤z≤0.

005.

4. A method for preparing a lithium-rich manganese-based oxide positive electrode material according to any one of claims 1 to 3, characterized in that: It includes: According to the molar ratio of the elements in the chemical formula, a raw material mixture of a nickel-manganese precursor, a lithium source, a lithium site additive, a transition metal site additive, and an oxygen site additive is obtained; The raw material mixture is sintered.

5. The method for preparing a lithium-rich manganese-based oxide positive electrode material according to claim 4, characterized in that: The steps of preparing the raw material mixture include: weighing a nickel-manganese precursor, a lithium source, a lithium site additive, a transition metal site additive and an oxygen site additive and uniformly mixing them in a high-speed mixer according to a lithium molar ratio of Li / TM=1.1-1.6 and a doping element addition ratio of 0-5wt% of the precursor mass; Preferably, the rotation speed of the high-speed mixer is 100-3000 r / min, the material temperature is controlled at 20-150° C., gas is introduced during the mixing process, the gas flow rate is 50-200 L / min, and the gas pressure is 0.2-0.5 MPa.

6. The method for preparing a lithium-rich manganese-based oxide positive electrode material according to claim 4, characterized in that: The particle sizes of the nickel-manganese precursor and the lithium source are both 0.5 μm to 20 μm, and the particle sizes of the lithium site additive, the transition metal site additive and the oxygen site additive are all 5 nm to 500 nm.

7. The method for preparing a lithium-rich manganese-based oxide positive electrode material according to claim 4, characterized in that: The nickel-manganese precursor is selected from Ni e Mn f CO3 and Ni e Mn f At least one of (OH)2, wherein 0≤e≤0.5, 0.5≤f≤1, e+f=1; and / or, the lithium source is selected from at least one of Li2CO3, LiOH, LiOH·H2O, Li2O, Li2O2, lithium acetate, lithium oxalate and lithium nitrate; and / or, the lithium site additive is selected from at least one of compounds containing Na, K, Mg, Ti or Zn, preferably at least one of sodium carbonate, sodium bicarbonate, sodium oxalate, sodium acetate, sodium citrate, sodium chloride, sodium nitrate, sodium sulfate, sodium hydroxide, potassium carbonate, potassium bicarbonate, potassium oxalate, potassium acetate, potassium citrate, potassium chloride, potassium nitrate, potassium sulfate, potassium hydroxide, magnesium carbonate, magnesium hydroxide, magnesium oxide, lithium oxalate, magnesium chloride, magnesium sulfate, zinc oxide, zinc hydroxide, zinc carbonate and zinc chloride; and / or, the transition metal site additive is selected from at least one of compounds containing W, Zr, Al, Mo, La, Y, Nb, Ti, Sc or Ce, preferably at least one of tungsten trioxide, ammonium tungstate, niobium pentoxide, niobium acetate, zirconium oxide, zirconium carbonate, zirconium hydroxide, zirconium acetate, zirconium nitrate, zirconium chloride, titanium dioxide, titanium hydroxide, titanium sulfate, aluminum trioxide, aluminum carbonate, aluminum hydroxide, aluminum oxide monohydrate, molybdenum trioxide, lanthanum oxide, yttrium oxide, scandium oxide and cerium oxide; And / or, the oxygen site additive is selected from at least one of compounds containing B, P, Si, S, Cl, F or N, preferably at least one of diammonium phosphate, diammonium hydrogen phosphate, boric acid, ammonium fluoride, ammonium sulfide, molybdenum disulfide, tungsten disulfide, ammonium sulfate, ammonium chloride, silicon dioxide and silicic acid gel.

8. The method for preparing a lithium-rich manganese-based oxide positive electrode material according to any one of claims 4 to 7, characterized in that: The sintering process includes placing the raw material mixture in a crucible and dividing it into a plurality of square regions, and then sintering the raw material mixture, and at least one of the following conditions is met: (1) The charge is less than or equal to 80% of the total capacity of the crucible; (2) Sintering in an air atmosphere with the air flow rate controlled at 10 mL / min to 200 mL / min; (3) First raise the temperature to 400°C to 600°C, keep it for 0h to 10h, then raise the temperature to 800°C to 1000°C, preferably 860°C to 900°C, keep it for 5h to 25h, and preferably the heating rate is 0.5°C / min to 10°C / min.

9. Use of the lithium-rich manganese-based oxide positive electrode material according to any one of claims 1 to 3 in preparing a positive electrode for a lithium-ion battery.

10. A lithium ion battery, characterized in that: It includes a lithium-ion battery positive electrode prepared by the application as claimed in claim 9.

Citation Information

Cited By

  • Molybdenum disulfide and lithium lanthanum niobium oxygen co-coated lithium-rich manganese-based positive electrode material and preparation method thereof

    CN120072912A

  • A lithium-rich manganese-based cathode material co-coated with molybdenum disulfide and lithium lanthanum niobium oxide and its preparation method

    CN120072912B

  • Lithium ion secondary battery, positive electrode active material, preparation method and electric equipment

    CN121215860A