Modified current collector base membrane, preparation method thereof, composite copper current collector and application
By introducing silica aerogel and nano-copper seed chopped fibers into polymer materials, the interlaced crosslinking structure is solved, and the problems of low adhesion, conductivity and mechanical properties of the composite copper current collector are significantly improved Battery energy density.
Patent Information
- Application Number
- CN202411339821.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-24
AI Technical Summary
The existing composite copper current collector based on polymer substrates has problems such as reduced interface adhesion, low conductivity and mechanical properties, and low temperature resistance, which limits its further application in the field of power batteries.
The polymer material is introduced with low density, low thermal conductivity, and high porosity silica aerogels, and the pores are filled with chopped fibers with nano copper seeds attached to the surface to form an interlaced cross-linking structure to improve interface friction It provides nucleation sites for copper layer growth, refining copper grains.
The conductive properties, interface adhesion and mechanical properties of the modified current collector base film are significantly improved, the battery energy density is improved, and the problem of insufficient temperature resistance and mechanical properties of the composite copper current collector is solved.
Smart Images

Figure BDA0005060841290000131
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and in particular relates to a modified current collector base film, a preparation method thereof, a composite copper current collector and applications. Background Art
[0002] With the rapid development of new energy vehicles and energy storage, the demand for lithium-ion power batteries has risen rapidly, which has put forward higher requirements for the performance of current collectors. Therefore, current collectors are developing in the direction of thinner, lighter and safer. As the new current collector material with the most potential for substitution, the composite current collector has subverted the traditional current collector with its "metal-polymer material-metal" sandwich structure, which not only improves its safety performance, but also increases energy density and reduces the cost of raw materials. At present, the mainstream manufacturers' preparation process of composite current collectors is divided into two steps and three steps, both of which are mainly magnetron sputtering and water plating. The specific process is: first, a conductive metal is sputtered on the surface of a polymer substrate with good tensile strength (usually polypropylene (PP), polyethylene terephthalate (PET) or polyimide (PI), etc.) to metalize it, and then the copper ions in the electrolytic cell are reduced and deposited on the surface of the magnetron film through a water electroplating process to thicken the copper layer, so as to obtain a product that meets the process standards.
[0003] Currently, the development of polymer film-based composite copper current collectors is one of the hottest research areas in the power battery industry. However, the polymer-based composite copper current collectors currently produced face unfavorable characteristics such as general tensile strength, poor adhesion and low temperature resistance, and are prone to breakage under physical vapor deposition environments (winding tension, metal ion bombardment, vacuuming, and high temperatures generated during sputtering, etc.), which limits their further application.
[0004] Therefore, it is necessary to develop a new current collector base film to solve the problems of reduced interface adhesion, low conductivity and mechanical properties, and low temperature resistance of composite copper current collectors. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a modified current collector base film, a preparation method thereof, a composite copper current collector and application. The present invention introduces silica aerogel with physical and chemical properties such as low density, low thermal conductivity, high porosity and large specific surface area into a polymer material, and at the same time fills the pores with short-cut fibers with nano-copper seeds attached to the surface for modification. The short-cut fiber material can form interlaced crosslinks in the pores, resulting in a mechanical interlocking effect between the materials, thereby increasing the interface friction and hindering the movement of the interface. At the same time, the nano-copper seeds can serve as active sites to provide nucleation sites for the subsequent copper layer preparation and refine the copper grains, so that the copper layer grows in the (111) direction, so that the modified current collector base film has greatly improved electrical conductivity, interface adhesion, and mechanical properties.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a modified current collector substrate film, which comprises a polymer material and a modified silica aerogel, wherein the modified silica aerogel is a porous structure, and the pores are filled with chopped fibers with nano-copper seeds attached to the surface.
[0008] The present invention introduces silica aerogel with physical and chemical properties such as low density, low thermal conductivity, high porosity and large specific surface area into the polymer material, and at the same time fills the pores of the polymer material with chopped fibers with nano copper seeds attached to the surface for modification. The chopped fiber material can form interlaced crosslinks in the pores, resulting in a mechanical interlocking effect between the materials, thereby increasing the interface friction and hindering the movement of the interface. At the same time, the nano copper seeds can serve as active sites to provide nucleation sites for the subsequent preparation of the copper layer and refine the copper grains, so that the copper layer grows in the (111) direction, so that the modified current collector base film has greatly improved electrical conductivity, interface adhesion, and mechanical properties.
[0009] In summary, the modified current collector base film solves the problems of reduced interface adhesion, low conductivity and mechanical properties, and low temperature resistance of the composite copper current collector. The energy density of the battery prepared based on this is significantly improved.
[0010] It should be noted that the present invention does not limit the specific type of polymer material. For example, it can be any one or a combination of at least two of materials such as polyethylene terephthalate (PET), polypropylene (PP), polyimide (PI), polyamide (PA), polytetrafluoroethylene (PTFE) or polyvinylidene fluoride (PVDF).
[0011] Preferably, the chopped fibers include any one of chopped carbon fibers, chopped glass fibers or chemical staple fibers, or a combination of at least two of them.
[0012] It should be noted that chopped carbon fiber is made by chopping carbon fiber filaments through a fiber cutting machine, and its basic performance mainly depends on the performance of its raw material - carbon fiber filaments. Chopped glass fiber is also called glass fiber chopped strands. Quartz sand is melted at high temperature, and the strands are drawn using a special impregnation (softener), and then chopped online by wet method, or the product glass fiber is chopped. Chemical staple fibers are commonly known as "short fibers" and "short filaments". They are products obtained by cutting chemical fibers into a certain length after they are formed.
[0013] Preferably, the length of the chopped fibers is 100-1000 nm, for example, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm or 1000 nm.
[0014] Preferably, the diameter of the chopped fibers is 10-100 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0015] Preferably, the diameter of the nano copper seed crystal is ≤100 nm, for example, it may be 50 nm, 70 nm or 100 nm.
[0016] In the present invention, nano copper seeds with suitable particle size are beneficial to serve as active sites for subsequent copper plating, providing nucleation points to refine copper grains, thereby improving mechanical properties and electrical conductivity.
[0017] Preferably, based on the total mass of the polymer material and the modified silica aerogel, the mass content of the modified silica aerogel is 0-20%, excluding 0, for example, it can be 2%, 5%, 8%, 11%, 15% or 18%, etc., preferably 5-15%.
[0018] In the present invention, if the mass content of the modified silica aerogel is too large, the tensile strength of the composite material will drop sharply, because the mechanical strength of the modified silica aerogel is lower than that of the polymer material.
[0019] Preferably, the porosity of the modified silica aerogel is 80-99.8%, for example, 80%, 85% or 90%.
[0020] Preferably, the average pore size of the modified silica aerogel is 50-100 nm, for example, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0021] The modified silica aerogel provided by the present invention has a low density (e.g. 0.03 g / cm 3 ), low thermal conductivity, high porosity and high specific surface area, so that the manufactured current collector has a lighter density, which can further improve the battery energy density.
[0022] In a second aspect, the present invention provides a method for preparing the modified current collector base film as described in the first aspect, the preparation method comprising the following steps:
[0023] (1) mixing a polymer material and a silica aerogel, and then sequentially performing melt extrusion, plasticizing and stretching treatment to obtain a semi-treated film;
[0024] (2) coating a chopped fiber solution with nano copper seeds attached to the surface on both sides of the semi-treated film, and rolling it up after drying to obtain the modified current collector base film.
[0025] Preferably, during the melt extrusion process of step (1), the temperature of heating and melting is higher than the melting point of the polymer material. For example, if the polymer material is polypropylene PP, the temperature of heating and melting may be 200°C.
[0026] Preferably, the difference between the heating and melting temperature and the melting point temperature of the polymer material is 15-30°C, for example, it can be 15°C, 20°C, 25°C or 30°C.
[0027] Preferably, during the plasticizing and molding process in step (1), the molding temperature is less than 45°C, for example, it can be 40°C, 35°C, 30°C or 25°C.
[0028] Preferably, the stretching treatment in step (1) includes longitudinal stretching and transverse stretching.
[0029] Preferably, the stretching ratio of the longitudinal stretching in step (1) is (3.2-6.1):1, for example, it can be 3.2:1, 4:1, 5:1 or 6:1, etc., the stretching temperature of the longitudinal stretching is 50-180°C, for example, it can be 50°C, 80°C, 100°C, 150°C or 180°C, etc., the stretching ratio of the transverse stretching is (3.4-5.5):1, for example, it can be 3.5:1, 4:1, 4.5:1 or 5:1, etc., and the stretching temperature of the transverse stretching is 50-180°C, for example, it can be 50°C, 80°C, 100°C, 150°C or 180°C, etc.
[0030] Preferably, the coating method in step (2) includes spraying, preferably ultrasonic spraying.
[0031] Preferably, the concentration of the chopped fiber solution with nano copper seeds attached to the surface in step (2) is 0-0.15 g / L, excluding 0, for example, it can be 0.02 g / L, 0.05 g / L, 0.08 g / L, 0.1 g / L, 0.12 g / L or 0.15 g / L, preferably 0.05-0.1 g / L. It should be noted that the concentration refers to the ratio of the mass of the chopped fiber with nano copper seeds attached to the surface to the total volume of the solution.
[0032] In the present invention, if the concentration of the chopped fiber solution with nano copper seeds attached to the surface is too high, it will lead to uneven distribution, pore blockage, and difficulty in forming cross-links, so that the improvement of mechanical properties is not obvious.
[0033] Preferably, the step of preparing the chopped fiber solution with nano copper seeds attached to the surface in step (2) comprises:
[0034] The copper source, chopped fibers, a complexing buffer, a dispersant, a reducing agent and a non-organic solvent are mixed to obtain the chopped fiber solution with nano copper crystal seeds attached to the surface.
[0035] It should be noted that the copper source provides copper atoms for the generation of copper seeds, the complexing buffer has the dual effects of complexing and buffering, the dispersant is to prevent the agglomeration of copper ions, and the reducing agent is to convert copper ions into copper atoms.
[0036] Preferably, the copper source comprises a tetrachlorocupric acid solution. For example, 1 g of tetrachlorocupric acid is dissolved in 50 mL of water to obtain a 0.02 g / mL tetrachlorocupric acid solution.
[0037] Preferably, the complexing buffer comprises a trisodium citrate solution. Exemplarily, the concentration of the trisodium citrate solution may be, for example, 0.04 mol / L.
[0038] Preferably, the dispersant comprises a polyvinyl pyrrolidone solution. Exemplarily, the concentration of the polyvinyl pyrrolidone solution may be, for example, 5 mol / L.
[0039] Preferably, the reducing agent comprises a sodium borohydride solution. Exemplarily, the concentration of the sodium borohydride solution may be, for example, 0.1 mol / L.
[0040] Preferably, the ratio of the copper source, chopped fibers, complexing buffer, dispersant and reducing agent is (0.5-1) mL: 1 g: (0.8-1.2) mL: (3-5) mL: (0.9-1.1) mL. The selection range of the copper source "(0.5-1) mL" can be, for example, 0.5 mL, 0.6 mL, 0.7 mL, 0.8 mL, 0.9 mL or 1 mL, the selection range of the complexing buffer "(0.8-1.2) mL" can be, for example, 0.8 mL, 0.9 mL, 1 mL, 1.1 mL or 1.2 mL, the selection range of the dispersant "(3-5) mL" can be, for example, 3 mL, 3.5 mL, 4 mL, 4.5 mL or 5 mL, the selection range of the reducing agent "(0.9-1.1) mL" can be, for example, 0.9 mL, 1 mL or 1.1 mL, and is preferably 0.7 mL: 1 g: 1 mL: 4 mL: 1 mL.
[0041] Preferably, the non-organic solvent comprises water.
[0042] Preferably, the preparation method comprises the following steps:
[0043] (1) A polymer material and a silica aerogel are mixed, and then added to a twin-screw extruder for heating and melting treatment, and then the obtained melt is extruded through a die under pressure, and then the extrudate is cast onto a casting roll, and is cooled by the casting roll and cooling water to form a casting, and the cooling temperature is less than 45° C. to obtain a formed casting, and then the formed casting is stretched in a longitudinal and transverse direction step by step, and the longitudinal stretching parameters include: a stretching ratio of (3.2-6.1):1, and a stretching temperature of 50-180° C.; the transverse stretching parameters include: a stretching ratio of (3.4-5.5):1, and a stretching temperature of 50-180° C.; after the stretching is completed, a semi-treated film is obtained;
[0044] The heating and melting temperature is higher than the melting point of the polymer material, and the difference is 15-30°C;
[0045] (2) ultrasonically spraying a chopped fiber solution with nano-copper seeds attached to the surface onto both sides of the semi-treated film, and then drying it with a main roller at a surface temperature of 30-50° C. and rolling it up to obtain the modified current collector base film;
[0046] The concentration of the chopped fiber solution with nano-copper seeds attached to the surface is 0-0.15 g / L and is not 0. The preparation steps include: adding a copper source into water, then adding a complexing buffer and a dispersant, then adding chopped fibers and stirring for 1 hour, and then adding a reducing agent to obtain the chopped fiber solution with nano-copper seeds attached to the surface; the ratio of the copper source, chopped fibers, complexing buffer, dispersant and reducing agent is (0.5-1) mL: 1 g: (0.8-1.2) mL: (3-5) mL: (0.9-1.1) mL.
[0047] In a third aspect, the present invention provides a composite copper current collector, comprising a back conductive copper layer, a modified current collector base film as described in the first aspect, and a front conductive copper layer stacked in layers.
[0048] In the present invention, the back conductive copper layer and the front conductive copper layer are respectively located on both sides of the modified current collector base film, serving as current-carrying layers in subsequent battery production, and the surface carries the negative electrode material.
[0049] It should be noted that the present invention does not limit the preparation method of the copper layer. For example, it may be an electron beam evaporation coating process or a magnetron sputtering plus water electroplating coating process.
[0050] Preferably, the material of the back conductive copper layer and the front conductive copper layer independently includes copper metal or copper alloy.
[0051] Preferably, the thickness of the back conductive copper layer and the front conductive copper layer is independently 500-2500 nm, for example, 100 nm, 500 nm, 1000 nm, 1500 nm, 2000 nm or 2500 nm, etc., preferably 900-1200 nm.
[0052] In the present invention, in order to take into account both the conductivity of the current collector and the improvement of the battery energy density, the thickness is preferably between 900 nm and 1200 nm.
[0053] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the negative electrode plate of the lithium-ion battery comprises the composite copper current collector as described in the third aspect, or comprises a composite copper current collector made based on the modified current collector base film described in the first aspect.
[0054] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0055] Compared with the prior art, the present invention has the following beneficial effects:
[0056] The present invention introduces silica aerogel with physical and chemical properties such as low density, low thermal conductivity, high porosity and large specific surface area into the polymer material, and at the same time fills the pores with short-cut fibers with nano copper seeds attached to the surface for modification. The short-cut fiber material can form interlaced crosslinks in the pores, resulting in a mechanical interlocking effect between the materials, thereby increasing the interface friction and hindering the movement of the interface. At the same time, the nano copper seeds can be used as active sites to provide nucleation sites for the subsequent copper layer preparation and refine the copper grains, so that the copper layer grows in the (111) direction, so that the modified current collector base film has greatly improved electrical conductivity, interface adhesion, and mechanical properties. In summary, the modified current collector base film solves the problems of reduced interface adhesion, low electrical conductivity and mechanical properties, and low temperature resistance of the composite copper current collector, and the energy density of the battery prepared based on this is significantly improved. DETAILED DESCRIPTION
[0057] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0058] Example 1
[0059] This embodiment provides a modified current collector base film, comprising a polymer material and a modified silica aerogel, wherein the modified silica aerogel is a porous structure, and the pores are filled with chopped fibers with nano-copper crystal seeds attached to the surface;
[0060] The polymer material is polyethylene terephthalate, the length of the chopped fibers is 500 nm, the diameter is 40 nm, the chopped fibers are chopped carbon fibers, and the diameter of the nano-copper seed is 50 nm;
[0061] Based on the total mass of the polymer material and the modified silica aerogel, the mass content of the polymer material is 85%, and the mass content of the modified silica aerogel is 15%;
[0062] The porosity of the modified silica aerogel is 85%, and the average pore size of the modified silica aerogel is 100 nm.
[0063] This embodiment also provides a method for preparing the modified current collector base film, comprising the following steps:
[0064] (1) Polyethylene terephthalate and silica aerogel are mixed, and then added to a twin-screw extruder, heated and melted at 280° C., and then the obtained melt is extruded through a die under pressure, and then the extrudate is cast onto a casting roll, and is cooled by the casting roll and cooling water to form a casting, and the cooling temperature is 25° C. to obtain a formed casting, and then the formed casting is stretched step by step in the longitudinal and transverse directions, and the longitudinal stretching parameters include: a stretching ratio of 4.4:1 and a stretching temperature of 175° C.; the transverse stretching parameters include: a stretching ratio of 4:1 and a stretching temperature of 165° C.; after the stretching is completed, a semi-treated film is obtained;
[0065] (2) After the semi-treated film is heat treated at 160° C., it is sent to a cooling system to cool to room temperature 25° C., and then the cooled semi-treated film is sprayed by an ultrasonic spraying system, and a chopped carbon fiber solution with nano-copper crystals attached to the surface with a concentration of 0.05 g / L is selected as the spraying liquid, the spray volume is 0.01 mL / min, and the belt speed is 4 m / min. After the spraying is completed, it is dried by a main roller with a surface temperature of 40° C., and then it is wound into a winding system through a traction system to obtain a modified current collector base film;
[0066] The preparation steps of the chopped fiber solution with nano copper seeds attached to the surface include: adding a tetrachlorocupric acid solution with a concentration of 0.02 g / mL into water and stirring, then adding a trisodium citrate solution with a concentration of 0.04 mol / L and a polyvinyl pyrrolidone solution with a concentration of 5 mol / L, then adding 1 g of chopped carbon fiber and stirring for 1 hour, and then adding a sodium borohydride solution with a concentration of 0.1 mol / L, and observing that copper seeds are precipitated and attached to the surface of the chopped carbon fiber. After continuous stirring for 1 hour, a chopped carbon fiber solution with nano copper seeds attached to the surface is obtained; wherein the ratio of the tetrachlorocupric acid solution, the chopped carbon fiber, the trisodium citrate solution, the polyvinyl pyrrolidone solution and the sodium borohydride solution is 0.7 mL:1 g:1 mL:4 mL:1 mL.
[0067] This embodiment also provides a composite copper current collector, which includes a back conductive copper layer, the modified current collector base film as described above, and a front conductive copper layer stacked in layers;
[0068] The back conductive copper layer and the front conductive copper layer are both made of copper metal, and both have a thickness of 1000 nm.
[0069] This embodiment also provides a method for preparing the composite copper current collector, the specific steps of which include:
[0070] In a magnetron sputtering system, a 1000 nm thick conductive copper layer was sputtered on both sides of the modified current collector substrate. The back vacuum was 3×10 -3 Pa, the sputtering gas flow is 100 sccm, and the sputtering pressure is 2×10 -1 Pa, the sputtering power is 15kW, and the main roller cooling temperature is -15°C; then the semi-finished product is placed in a chemical copper plating solution with a pH of 12, electroplated at 30°C, and the belt speed is 3m / min to obtain a composite copper current collector.
[0071] Example 2
[0072] The difference between this embodiment and embodiment 1 is that, based on the total mass of the polymer material and the modified silica aerogel, the mass content of the polymer material is 98%, and the mass content of the modified silica aerogel is 2%.
[0073] The rest of the preparation methods and parameters were the same as those in Example 1.
[0074] Example 3
[0075] The difference between this embodiment and embodiment 1 is that, based on the total mass of the polymer material and the modified silica aerogel, the mass content of the polymer material is 95%, and the mass content of the modified silica aerogel is 5%.
[0076] The rest of the preparation methods and parameters were the same as those in Example 1.
[0077] Example 4
[0078] The difference between this embodiment and embodiment 1 is that, based on the total mass of the polymer material and the modified silica aerogel, the mass content of the polymer material is 92%, and the mass content of the modified silica aerogel is 8%.
[0079] The rest of the preparation methods and parameters were the same as those in Example 1.
[0080] Example 5
[0081] The difference between this embodiment and embodiment 1 is that, based on the total mass of the polymer material and the modified silica aerogel, the mass content of the polymer material is 89%, and the mass content of the modified silica aerogel is 11%.
[0082] The rest of the preparation methods and parameters were the same as those in Example 1.
[0083] Example 6
[0084] The difference between this embodiment and embodiment 1 is that, based on the total mass of the polymer material and the modified silica aerogel, the mass content of the polymer material is 82%, and the mass content of the modified silica aerogel is 18%.
[0085] The rest of the preparation methods and parameters were the same as those in Example 1.
[0086] Example 7
[0087] The difference between this embodiment and embodiment 1 is that, based on the total mass of the polymer material and the modified silica aerogel, the mass content of the polymer material is 80%, and the mass content of the modified silica aerogel is 20%.
[0088] The rest of the preparation methods and parameters were the same as those in Example 1.
[0089] Example 8
[0090] The difference between this embodiment and embodiment 1 is that the concentration of the chopped carbon fiber solution with nano copper seeds attached to the surface is 0.1 g / L.
[0091] The rest of the preparation methods and parameters were the same as those in Example 1.
[0092] Example 9
[0093] The difference between this embodiment and embodiment 1 is that the concentration of the chopped carbon fiber solution with nano copper seeds attached to the surface is 0.15 g / L.
[0094] The rest of the preparation methods and parameters were the same as those in Example 1.
[0095] Example 10
[0096] The difference between this embodiment and embodiment 1 is that, based on the total mass of the polymer material and the modified silica aerogel, the mass content of the polymer material is 70%, and the mass content of the modified silica aerogel is 30%.
[0097] The rest of the preparation methods and parameters were the same as those in Example 1.
[0098] Embodiment 11
[0099] The difference between this embodiment and embodiment 1 is that the concentration of the chopped carbon fiber solution with nano copper seeds attached to the surface is 0.2 g / L.
[0100] The rest of the preparation methods and parameters were the same as those in Example 1.
[0101] Comparative Example 1
[0102] The difference between this comparative example and Example 1 is that the spraying treatment of the chopped carbon fiber solution with nano copper seeds attached to the surface in step (2) is not performed, that is, the pores of the silica aerogel are not filled with chopped fibers with nano copper seeds attached to the surface.
[0103] The rest of the preparation methods and parameters were the same as those in Example 1.
[0104] Comparative Example 2
[0105] The difference between this comparative example and Example 1 is that in the method for preparing the chopped carbon fiber solution with nano-copper seeds attached to the surface in step (2), no tetrachlorocupric acid is added, that is, nano-copper seeds are not attached to the surface of the chopped fibers.
[0106] The rest of the preparation methods and parameters were the same as those in Example 1.
[0107] Performance Testing
[0108] The modified current collector base film and the composite copper current collector provided in the above embodiments and comparative examples were tested for tensile strength respectively, and the test standard was referred to the national standard GB / T 1040.3-2006; the square resistance of the composite copper current collector was measured using a four-probe tester, and attention was paid to flattening the current collector during the test; the bonding strength of the composite copper current collector was tested with reference to the "Composite Current Collector Bonding Strength Test Method" of the China Automobile Association; and the flame retardancy of the composite copper current collector was tested according to the UL94 standard.
[0109] The above test results are shown in Table 1.
[0110] Table 1
[0111]
[0112] analyze:
[0113] From the above results, it can be seen that the present invention introduces silica aerogel into the polymer material, and at the same time fills the pores of the silica aerogel with short-cut fibers attached with nano-copper seeds on the surface for modification, thereby preparing a modified current collector base film with better mechanical properties. Moreover, the introduction of short-cut fibers with copper seeds provides nucleation points for the growth of copper grains, refines the copper grains, and is conducive to the growth of copper grains along a specific crystal direction, which not only improves the bonding effect between the conductive copper layer and the modified current collector base film, but also greatly improves the conductivity and tensile strength of the current collector. In addition, since the modified silica aerogel has good thermal conductivity, the subsequent current collector has better heat resistance, which provides a direction for subsequent process optimization and changes, and accelerates the effective application of composite copper current collectors.
[0114] It can be seen from Examples 1 and 2-7 that the introduction of modified silica aerogel enhances the tensile strength of the base film, which is due to the different interfaces of different materials and the increase in friction during stretching. However, with the substantial addition of modified silica aerogel, the tensile strength of the current collector decreases rapidly, but the heat resistance changes rapidly.
[0115] It can be seen from Examples 1 and 10 that when the amount of modified silica aerogel added is too large, the tensile strength of the base film decreases rapidly. This is because the mechanical properties of the modified silica aerogel are relatively low, and when the content is too high, agglomeration occurs, causing defects, resulting in the above results.
[0116] It can be seen from Example 1, Example 8-9 and Example 11 that the appropriate concentration of the chopped carbon fiber solution with nano copper seeds attached to the surface can effectively increase the interface friction, improve the tensile strength of the base film, and improve the bonding strength between the base film and the conductive copper layer. However, if the concentration of the chopped carbon fiber solution with nano copper seeds attached to the surface is too high, it will lead to uneven distribution, pore blockage, and difficulty in forming cross-links, so that the improvement of mechanical properties is not obvious.
[0117] It can be seen from Example 1 and Comparative Example 1 that if the pores of the silica aerogel are not filled with chopped fibers with nano-copper seeds attached to the surface, the tensile strength of the modified base film is not significantly improved, and the mechanical properties, bonding force and conductive properties of the prepared current collector do not change significantly.
[0118] It can be seen from Example 1 and Comparative Example 2 that if the nano-copper seeds are not attached to the surface of the chopped fibers, the bonding force and conductivity between the conductive copper layer and the base film in the manufactured current collector cannot be improved.
[0119] The applicant declares that the present invention illustrates the technical solution of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A modified current collector base film, characterized in that: The modified current collector base film comprises a polymer material and a modified silica aerogel. The modified silica aerogel is a porous structure, and the pores are filled with short-cut fibers with nano copper crystal seeds attached to the surface.
2. The modified current collector base film according to claim 1, characterized in that: The chopped fibers include any one of chopped carbon fibers, chopped glass fibers or chemical short fibers, or a combination of at least two thereof; Preferably, the length of the chopped fibers is 100-1000 nm; Preferably, the diameter of the chopped fibers is 10-100 nm; Preferably, the diameter of the nano copper seed is ≤100 nm.
3. The modified current collector base film according to claim 1, characterized in that: Based on the total mass of the polymer material and the modified silica aerogel, the mass content of the modified silica aerogel is 0-20%, excluding 0, and preferably 5-15%.
4. The modified current collector base film according to claim 1, characterized in that: The porosity of the modified silica aerogel is 80-99.8%; Preferably, the average pore size of the modified silica aerogel is 50-100 nm.
5. A method for preparing a modified current collector base film according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) mixing a polymer material and a silica aerogel, and then sequentially performing melt extrusion, plasticizing and stretching treatment to obtain a semi-treated film; (2) coating a chopped fiber solution with nano copper seeds attached to the surface on both sides of the semi-treated film, and rolling it up after drying to obtain the modified current collector base film.
6. The preparation method according to claim 5, characterized in that: During the melt extrusion process of step (1), the heating and melting temperature is higher than the melting point of the polymer material; Preferably, the difference between the heating and melting temperature and the melting point temperature of the polymer material is 15-30°C; Preferably, the stretching treatment in step (1) includes longitudinal stretching and transverse stretching; Preferably, the stretching ratio of the longitudinal stretching in step (1) is (3.2-6.1):1, the stretching temperature of the longitudinal stretching is 50-180°C, the stretching ratio of the transverse stretching is (3.4-5.5):1, and the stretching temperature of the transverse stretching is 50-180°C; Preferably, the coating method in step (2) includes spraying.
7. The preparation method according to claim 5 or 6, characterized in that: The concentration of the chopped fiber solution with nano copper seeds attached to the surface in step (2) is 0-0.15 g / L, and is not 0; Preferably, the steps of preparing the chopped fiber solution with nano copper seeds attached to the surface in step (2) include: Mixing a copper source, chopped fibers, a complexing buffer, a dispersant, a reducing agent, and a non-organic solvent to obtain a chopped fiber solution having nano-copper crystal seeds attached to the surface; Preferably, the copper source comprises a tetrachlorocupric acid solution; Preferably, the complexing buffer comprises trisodium citrate solution; Preferably, the dispersant comprises a polyvinyl pyrrolidone solution; Preferably, the reducing agent comprises sodium borohydride solution; Preferably, the ratio of the copper source, chopped fibers, complexing buffer, dispersant and reducing agent is (0.5-1) mL: 1 g: (0.8-1.2) mL: (3-5) mL: (0.9-1.1) mL; Preferably, the non-organic solvent comprises water.
8. The preparation method according to any one of claims 5 to 7, characterized in that: The preparation method comprises the following steps: (1) A polymer material and a silica aerogel are mixed, and then added to a twin-screw extruder for heating and melting treatment, and then the obtained melt is extruded through a die under pressure, and then the extrudate is cast onto a casting roll, and is cooled by the casting roll and cooling water to form a casting, and the cooling temperature is less than 45° C. to obtain a formed casting, and then the formed casting is stretched in a longitudinal and transverse direction step by step, and the longitudinal stretching parameters include: a stretching ratio of (3.2-6.1):1, and a stretching temperature of 50-180° C.; the transverse stretching parameters include: a stretching ratio of (3.4-5.5):1, and a stretching temperature of 50-180° C.; after the stretching is completed, a semi-treated film is obtained; The heating and melting temperature is higher than the melting point of the polymer material, and the difference is 15-30°C; (2) ultrasonically spraying a chopped fiber solution with nano-copper seeds attached to the surface onto both sides of the semi-treated film, and then drying it with a main roller at a surface temperature of 30-50° C. and then rolling it up to obtain the modified current collector base film; The concentration of the chopped fiber solution with nano-copper seeds attached to the surface is 0-0.15 g / L and is not 0. The preparation steps include: adding a copper source into water, then adding a complexing buffer and a dispersant, then adding chopped fibers and stirring for 1 hour, and then adding a reducing agent to obtain the chopped fiber solution with nano-copper seeds attached to the surface; the ratio of the copper source, chopped fibers, complexing buffer, dispersant and reducing agent is (0.5-1) mL: 1 g: (0.8-1.2) mL: (3-5) mL: (0.9-1.1) mL.
9. A composite copper current collector, characterized in that: The composite copper current collector comprises a back conductive copper layer, a modified current collector base film according to any one of claims 1 to 4, and a front conductive copper layer which are stacked.
10. A lithium ion battery, characterized in that: The negative electrode plate of the lithium-ion battery includes the composite copper current collector as claimed in claim 9, or includes a composite copper current collector made from the modified current collector base film according to any one of claims 1 to 4.
Citation Information
Patent Citations
Preparation method, product and application of aerogel composite material
CN113548817A
Composite membrane and preparation method thereof, secondary battery, battery module, battery pack and electric device
CN115819932A
Composite current collector for lithium ion battery and preparation method of composite current collector
CN116632252A
Composite current collector heat-resistant base film and preparation method thereof
CN118027559A
Composite current collector based on polyarylene sulfide resin, lithium ion battery and preparation method
CN118380588A