Comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material as well as preparation method and application thereof
Through the comb crosslinking network polymer-based polymetal oxygen cluster composite proton exchange membrane material, proton exchange in hydrogen fuel cells is solved by using the combination of polyethylene glycol diamine, polyglycidyl methacrylate and polymetal oxygen cluster. The membrane has high humidity requirements and complex manufacturing process, which achieves efficient water-free proton conduction and simplified processes, and improves the mechanical properties and electrical conductivity of the material.
Patent Information
- Application Number
- CN202410988406.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-22
AI Technical Summary
The proton exchange membranes in existing hydrogen fuel cells have high humidity requirements, and the perfluorosulfonic acid membranes lack sufficient performance under anhydrous conditions, and the manufacturing process is complex and contaminated, making it difficult to achieve cost-effective proton conduction.
Using a comb-shaped crosslinking network polymer-based polymetal oxygen cluster composite proton exchange membrane material, a high-efficiency proton conduction channel is formed through the combination of polyethylene glycol diamine, polyglycidyl methacrylate and polymetal oxygen cluster, and through The solvent blending method is simply prepared to form a proton exchange membrane under anhydrous conditions.
It realizes efficient proton conduction under water conditions, simplifies the manufacturing process, reduces pollution, improves the mechanical strength and water-annual proton conductivity of the material, and solves the problem of insufficient performance of the existing membrane under low humidity conditions.
Smart Images

Figure CN119008997A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of proton exchange membrane materials for hydrogen fuel cells, and in particular relates to a comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material and a preparation method and application thereof. Background Art
[0002] Fuel cells (FCs), especially hydrogen fuel cells, have gained increasing attention worldwide, from government energy and climate agencies, sustainable energy institutes to the automotive industry, due to their expected high energy density, zero emissions, and widespread and sustainable supply of hydrogen fuel. Among them, proton exchange membranes (PEMs), as the core components of FCs, must act as proton conductors, electrical insulators, mechanical barriers, and gas barriers, placing high demands on the synergistic effects of multiple functions. Currently, the state-of-the-art Nafion perfluorosulfonic acid (PFSA) polymers used in fuel cells have high proton conductivity and good stability, which are attributed to the water permeation channels formed by its grafted sulfonic acid groups and perfluorinated chemical structure, respectively. However, in order to make the membrane have well-phase-separated proton-conducting water channels, complex and expensive processing is required to weaken the physical and chemical interactions of PFSA chains. Moreover, since perfluorosulfonic acid-based proton exchange membranes are rich in fluorine, the process of fluorinating polymers will cause environmental pollution. In addition, since its proton conduction process is highly dependent on water channels, its conductivity level has very high requirements on humidity, which hinders its anhydrous proton conduction.
[0003] Therefore, it is of great significance to develop a proton exchange membrane with high cost performance, simple manufacturing process and the ability to conduct protons under anhydrous conditions. Summary of the invention
[0004] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a comb-like cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material.
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned comb-like cross-linked network polymer-based polymetallic oxygen cluster composite proton exchange membrane material.
[0006] Another object of the present invention is to provide an application of the above-mentioned comb-like cross-linked network polymer-based polymetallic oxygen cluster composite proton exchange membrane material.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A comb-shaped cross-linked network polymer-based polyoxometallic cluster composite proton exchange membrane material is mainly prepared from polyethylene glycol diamine, polyglycidyl methacrylate and molecular clusters; the molecular cluster is a polyoxometallic cluster, specifically one of Keggin-type polyoxometallic clusters, Dawson-type polyoxometallic clusters or Anderson-type polyoxometallic clusters.
[0009] Preferably, the number average molecular weight of the polyethylene glycol diamine is 1,000 to 10,000.
[0010] More preferably, the number average molecular weight of the polyethylene glycol diamine is 2000.
[0011] Preferably, the number average molecular weight of the polyglycidyl methacrylate is 2000-20000.
[0012] More preferably, the number average molecular weight of the polyglycidyl methacrylate is 5,000.
[0013] Preferably, the molecular cluster is a Keggin-type polymetallic oxygen cluster, and its molecular formula is Y n [XM 12 O 40 ] n- ·mH2O, X = P, Si, Co or Al; M = W, Mo or Nb; n = 3, 4 or 6; where X represents the central atom, M represents the coordinated polyatoms, Y is called the counter ion, Y = H, Li, Na or K; n is the number of charges carried by the polyanions, and m is the number of crystal waters.
[0014] Further preferably, the Keggin type polyoxometallic cluster has a molecular formula of Y n [XM 12 O 40 ] n- mH2O, wherein X is a P or Si atom, M is a W or Mo atom, n=3 or 4, and Y is a H or Na atom.
[0015] More preferably, the Keggin-type polyoxometallic cluster has a molecular formula of Y n [XM 12 O 40 ] n- mH2O, wherein X is a P atom, M is a W atom, n=3, and Y is a H atom.
[0016] Preferably, the mass ratio of the polyethylene glycol diamine, polyglycidyl methacrylate and polyoxometalate is (1-8): (0.2-4): (2-15).
[0017] More preferably, the mass ratio of the polyethylene glycol diamine, polyglycidyl methacrylate, and polyoxymetallic clusters is (1.5-6): (0.5-3): (3-13).
[0018] More preferably, the mass ratio of the polyethylene glycol diamine, polyglycidyl methacrylate, and polyoxometalate is (2-5):(0.8-1.5):(5-11).
[0019] The preparation method of the comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material comprises the following steps:
[0020] Polyethylene glycol diamine and poly(glycidyl methacrylate) are stirred evenly in a solvent to make them fully cross-linked, and then polyoxometalates are added and stirred evenly to obtain a composite solution; the composite solution is dried to form a film to obtain a composite proton exchange membrane, that is, the comb-like cross-linked network polymer-based polyoxometalates composite proton exchange membrane material.
[0021] Preferably, the mass fraction of the polyoxometallic clusters in the composite solution is 40-70%.
[0022] Preferably, the solvent includes at least one of furan solvents, alcohol solvents, dimethyl sulfoxide and dimethylacetamide.
[0023] Further preferably, the solvent includes at least one of tetrahydrofuran, ethanol, methanol, dimethyl sulfoxide and dimethylacetamide.
[0024] Preferably, after adding the polyoxometalate, the mixture is stirred uniformly at 40°C to 100°C to obtain a complex solution; further preferably, after adding the polyoxometalate, the mixture is stirred uniformly at 60°C to 100°C to obtain a complex solution.
[0025] Preferably, the film forming process refers to film forming on a substrate; further preferably, the film forming process refers to film forming on a polytetrafluoroethylene-based substrate.
[0026] The membrane forming process is to cast the mixed composite solution on a clean and flat polytetrafluoroethylene mold, dry it at 80-100° C. for 24-40 hours, and obtain a composite proton exchange membrane.
[0027] The comb-like cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material is used in hydrogen and oxygen fuel cells.
[0028] Principle of the present invention:
[0029] The comb-like cross-linked network polymer-based polyoxometalate composite proton exchange membrane material of the present invention introduces a macromolecular cross-linking agent poly(glycidyl methacrylate) (PGMA) by adding polyoxometalate into the comb-like cross-linked network structure, and the epoxy side groups on the side chains and the polyethylene glycol (PEG-BA) with amino groups form a series of comb chain cross-linking agent networks. A series of proton exchange membranes with different cross-linking ratios are obtained by changing the molar ratio of polyethylene glycol diamine to poly(glycidyl methacrylate). Due to the abundant hydrogen bonds and electrostatic interactions between polyethylene glycol and polyoxometalate, an efficient proton transfer channel is provided. Proton conduction under anhydrous conditions is effectively achieved, and excellent mechanical properties are given to the material system.
[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0031] 1. The most advanced Nafion perfluorosulfonic acid (PFSA) polymer has very high requirements for humidity, and since the perfluorosulfonic acid type proton exchange membrane is rich in fluorine, the process of fluorination of polymers will pollute the environment. The preparation method of the comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane described in the present invention is simple, and its raw materials are all commercial industrial products with low cost. At the same time, a solvent blending method is adopted, and the raw materials are uniformly mixed in a solvent and then cast into a film and dried to obtain the product. The production process is simple and there is no serious pollution. It effectively overcomes the problem of insufficient performance of the perfluorosulfonic acid type proton exchange membrane under low humidity conditions, and effectively realizes anhydrous proton conduction.
[0032] 2. The comb-like cross-linked network polymer-based polyoxometallic cluster composite proton exchange membrane material of the present invention is based on the covalent cross-linking interaction between polymer macromolecular chains, and polyoxometallic clusters are doped as proton sources and cross-linking agents to simultaneously improve the mechanical strength of the composite material system and give the material better anhydrous proton conductivity. At the same time, the mass fraction of polyoxometallic clusters and the cross-linking ratio of the network can be controlled to regulate the mechanical properties and conductivity of the composite proton exchange membrane material, providing a feasible method for producing proton exchange membrane materials. The comb-like cross-linked network polymer-based polyoxometallic cluster composite proton exchange membrane material of the present invention has strong mechanical strength and high anhydrous proton conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a process flow chart of the comb-like cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material of the present invention.
[0034] Figure 2 This is an optical image of the composite proton exchange membrane material obtained in Example 2.
[0035] Figure 3It is the infrared absorption spectra of Example 1, Comparative Example 1 and poly(glycidyl methacrylate).
[0036] Figure 4 It is a small angle X-ray scattering test curve graph of Example 1, Comparative Example 1, poly(glycidyl methacrylate), phosphotungstic acid and polyethylene glycol diamine.
[0037] Figure 5 It is the tensile curve diagram of the composite film material prepared in Comparative Examples 1 to 3.
[0038] Figure 6 This is a tensile curve diagram of the composite proton exchange membrane material prepared in Examples 1 to 3.
[0039] Figure 7 The temperature dependence curve of the conductivity of the composite proton exchange membrane materials prepared in Examples 1 to 3 and Comparative Example 4 is shown. DETAILED DESCRIPTION
[0040] The specific implementation of the present invention is further described below in conjunction with examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. If the manufacturer of the reagents or instruments used is not indicated, they are deemed to be conventional products that can be purchased commercially.
[0041] Figure 1 This is a process flow chart of the comb-like cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material of the present invention.
[0042] The number average molecular weight of polyethylene glycol diamine used in the embodiment is 2000, the number average molecular weight of poly(glycidyl methacrylate) is 5000, and the polyoxometalate is Keggin type phosphotungstic acid (H3PW 12 O 40 ·mH2O), and the organic solvent used was dimethyl sulfoxide (DMSO).
[0043] Example 1
[0044] 0.348g of polyethylene glycol diamine particles and 0.0744g of poly(glycidyl methacrylate) powder were added to 5mL of dimethyl sulfoxide organic solvent, stirred at 50°C for 48 hours to fully crosslink to obtain a white transparent liquid, 0.812g of white crystalline particles of phosphotungstic acid were added to the white transparent liquid, and continued to stir at 60°C for 24 hours to obtain a uniform yellow transparent liquid. The obtained yellow transparent liquid was poured into a clean and flat polytetrafluoroethylene substrate, heated at 90°C on a heating table for 24 hours, and then placed in a vacuum oven at 90°C for vacuum drying for 24 hours to obtain a yellow transparent comb-like cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material.
[0045] Example 2
[0046] 0.348g of polyethylene glycol diamine particles and 0.0992g of poly(glycidyl methacrylate) powder were added to 5mL of dimethyl sulfoxide organic solvent, stirred at 50°C for 48 hours to fully crosslink to obtain a white transparent liquid, 0.812g of white crystalline particles of phosphotungstic acid were added to the white transparent liquid, and continued to stir at 60°C for 24 hours to obtain a uniform yellow transparent liquid. The obtained yellow transparent liquid was poured into a clean and flat polytetrafluoroethylene substrate, heated at 90°C on a heating table for 24 hours, and then placed in a vacuum oven at 90°C for vacuum drying for 24 hours to obtain a yellow transparent comb-like cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material.
[0047] Example 3
[0048] 0.348g of polyethylene glycol diamine particles and 0.1488g of poly(glycidyl methacrylate) powder were added to 5mL of dimethyl sulfoxide organic solvent, stirred at 50°C for 48 hours to fully crosslink to obtain a white transparent liquid, 0.812g of white crystalline particles of phosphotungstic acid were added to the white transparent liquid, and continued to stir at 60°C for 24 hours to obtain a uniform yellow transparent liquid. The obtained yellow transparent liquid was poured into a clean and flat polytetrafluoroethylene substrate, heated at 90°C on a heating table for 24 hours, and then placed in a vacuum oven at 90°C for vacuum drying for 24 hours to obtain a yellow transparent comb-like cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material.
[0049] Comparative Example 1
[0050] 0.348g of polyethylene glycol diamine particles and 0.0744g of poly(glycidyl methacrylate) powder were added to 5mL of dimethyl sulfoxide organic solvent, and stirred at 50°C for 48 hours to fully crosslink to obtain a white transparent liquid. The obtained white transparent liquid was poured into a clean and flat polytetrafluoroethylene substrate, heated at 90°C on a heating table for 24 hours, and then placed in a vacuum oven at 90°C for vacuum drying for 24 hours to obtain a white transparent comb-shaped cross-linked network polymer base film material.
[0051] Comparative Example 2
[0052] 0.348g of polyethylene glycol diamine particles and 0.0992g of poly(glycidyl methacrylate) powder were added to 5mL of dimethyl sulfoxide organic solvent, and stirred at 50°C for 48 hours to fully crosslink to obtain a white transparent liquid. The obtained white transparent liquid was poured into a clean and flat polytetrafluoroethylene substrate, heated at 90°C on a heating table for 24 hours, and then placed in a vacuum oven at 90°C for vacuum drying for 24 hours to obtain a white transparent comb-shaped cross-linked network polymer base film material.
[0053] Comparative Example 3
[0054] 0.348g of polyethylene glycol diamine particles and 0.1488g of poly(glycidyl methacrylate) powder were added to 5mL of dimethyl sulfoxide organic solvent, and stirred at 50°C for 48 hours to fully crosslink to obtain a white transparent liquid. The obtained white transparent liquid was poured into a clean and flat polytetrafluoroethylene substrate, heated at 90°C on a heating table for 24 hours, and then placed in a vacuum oven at 90°C for vacuum drying for 24 hours to obtain a white transparent comb-shaped cross-linked network polymer base film material.
[0055] Comparative Example 4
[0056] 0.348g of polyethylene glycol diamine particles and 0.1488g of poly(glycidyl methacrylate) powder were added to 5mL of dimethyl sulfoxide organic solvent, stirred at 50°C for 48 hours to fully crosslink to obtain a white transparent liquid, 0.522g of white crystalline particles of phosphotungstic acid were added to the white transparent liquid, and continued to stir at 60°C for 24 hours to obtain a uniform yellow transparent liquid. The obtained yellow transparent liquid was poured into a clean and flat polytetrafluoroethylene substrate, heated at 90°C on a heating table for 24 hours, and then placed in a vacuum oven at 90°C for vacuum drying for 24 hours to obtain a yellow transparent comb-like cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material.
[0057] Comparative Example 5
[0058] 1g chitosan with a number average molecular weight of 50,000 was fully stirred and dissolved in an acetic acid aqueous solution at 50°C to obtain a yellow transparent liquid. White crystalline particles of phosphotungstic acid were added to the yellow transparent liquid and stirred and mixed. The stirring was continued for 24 hours to obtain a uniform yellow transparent liquid. The obtained yellow transparent liquid was poured into a clean and flat polypropylene substrate, heated at 50°C on a heating table for 24 hours, and then placed in a vacuum oven for vacuum drying for 24 hours to obtain a yellow transparent chitosan-polymetallic oxygen cluster composite proton exchange membrane material.
[0059] Structural characterization:
[0060] 1. Fourier transform infrared spectroscopy test
[0061] Fourier transform infrared spectroscopy is one of the powerful means to characterize the composition and internal structure of materials. It uses the infrared characteristic absorption peaks of chemical bonds within molecules to obtain information on the internal composition of materials and the existing interactions. Figure 3 The infrared absorption spectra of Example 1, Comparative Example 1 and poly(glycidyl methacrylate) are shown. In Comparative Example 1, the characteristic peak of the epoxy group of poly(glycidyl methacrylate) disappears, indicating that most of the epoxy side groups are successfully cross-linked; and four characteristic peaks of phosphotungstic acid are observed in Example 1, indicating that phosphotungstic acid is successfully introduced into the polymer network. It is also observed that the four characteristic peaks of phosphotungstic acid in Example 1 also shift significantly, confirming the existence of hydrogen bond interaction between phosphotungstic acid and polyethylene glycol diamine polymer.
[0062] 2. Small-angle X-ray scattering (SAXS)
[0063] Because of the sensitivity of X-rays to heavy metal ions with high electron density, we can obtain the distribution state of phosphotungstic acid molecular clusters in the polymer matrix with the help of small-angle X-ray scattering technology, including the shape factor related to its bulk shape and the structure factor reflecting the interaction and distribution state between phosphotungstic acid molecular clusters. Figure 4 The following are small angle X-ray scattering test curves of Example 1, Comparative Example 1, poly(glycidyl methacrylate), phosphotungstic acid and polyethylene glycol diamine. As can be seen from Comparative Example 1, the crystallization peak of polyethylene glycol diamine disappears after crosslinking, indicating that the crystallization region is broken, wherein the shape factor characteristic peak in the high Q region of the small angle X-ray scattering curve in Example 1 is highly consistent with the theoretical fitting curve of the phosphotungstic acid molecular cluster model, indicating that the polyacid molecular cluster maintains its structural integrity in the polymer substrate.
[0064] Mechanical properties characterization:
[0065] 1. Tensile performance test
[0066] Tensile testing is one of the important methods for testing the mechanical properties of materials. It can obtain the elastic modulus and elongation at break of the material, and then evaluate the mechanical properties and toughness of the material. The tensile rate during this test is 10mm / min. Figure 5 and Figure 6The tensile test curves of the comb-like cross-linked network polymer-based composite membrane materials of Comparative Examples 1 to 3 and Examples 1 to 3 respectively show that the elastic modulus of the material in Comparative Examples 1 to 3 increases with the increase of the cross-linking ratio, which are 1.15MPa, 1.49MPa, and 1.83MPa, respectively. And in Examples 1 to 3, with the addition of phosphotungstic acid, the elastic modulus and elongation at break of the multimetallic oxygen cluster composite proton exchange membrane material further increase, which are 1.72MPa, 16.6MPa, and 17.3MPa, respectively, indicating that the addition of multimetallic oxygen clusters can significantly enhance the mechanical strength and mechanical properties of the composite proton exchange membrane material.
[0067] Electrochemical characterization:
[0068] 1. Conductivity test
[0069] The conductivity of the material at different temperatures was measured using an electrochemical workstation. Figure 7 The temperature dependence curve of the conductivity of the composite proton exchange membrane materials prepared in Examples 1 to 3 shows that the conductivity increases with the increase of temperature. The composite proton exchange membrane materials prepared in Examples 1-3 all effectively achieve proton conduction under anhydrous conditions, among which the proton conductivity of Example 1 at 130°C is close to 10 -3 S cm -1 , the anhydrous proton conductivity is the best. The conductivity test results of Comparative Examples 4 and 5 show that they cannot achieve proton conduction under anhydrous conditions or the anhydrous proton conduction level is poor. As shown in the table:
[0070] Test items Proton conductivity / 130℃(S / cm) Example 1 <![CDATA[8.45×10 -4 ]]> Example 2 <![CDATA[2.13×10 -4 ]]> Example 3 <![CDATA[7.45×10 -5 ]]> Comparative Example 4 <![CDATA[4.49×10 -5 ]]> Comparative Example 5 <![CDATA[7.45×10 -7 ]]>
[0071] The production process of the comb-shaped cross-linked network polymer-based polyoxometalate composite proton exchange membrane material disclosed in the embodiment of the present invention is simple and easy. It only needs to dissolve a certain proportion of polyethylene glycol diamine, poly(glycidyl methacrylate) polymer and phosphotungstic acid in an organic solvent, dimethyl sulfoxide, heat and stir to mix evenly, then cast and lay the membrane, and heat and dry the organic solvent to obtain the composite proton exchange membrane material. The product production process is simple and has less pollution.
[0072] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material, It is characterized in that It is mainly prepared from polyethylene glycol diamine, poly(glycidyl methacrylate) and molecular clusters; the molecular cluster is a polymetallic oxygen cluster, specifically one of Keggin-type polymetallic oxygen clusters, Dawson-type polymetallic oxygen clusters or Anderson-type polymetallic oxygen clusters.
2. The comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material according to claim 1, It is characterized in that The number average molecular weight of the polyethylene glycol diamine is 1000 to 10000; The number average molecular weight of the polyglycidyl methacrylate is 2,000 to 20,000.
3. The comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material according to claim 1, It is characterized in that The molecular cluster is a Keggin type polymetallic oxygen cluster, and its molecular formula is Y n [XM 12 O 40 ] n- ·mH 2 O, X = P, Si, Co or Al; M = W, Mo or Nb; n = 3, 4 or 6; wherein X represents the central atom, M represents the coordinated polyatom, Y is called the counter ion, Y = H, Li, Na or K; n is the number of charges carried by the polyanion, and m is the number of crystal waters.
4. The comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material according to claim 3, It is characterized in that The Keggin type polymetallic oxygen cluster has a molecular formula of Y n [XM 12 O 40 ] n- ·mH 2 O, wherein X is a P or Si atom, M is a W or Mo atom, n=3 or 4, and Y is a H or Na atom.
5. The comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material according to claim 1, It is characterized in that The mass ratio of the polyethylene glycol diamine, polyglycidyl methacrylate and polyoxymetallic clusters is (1-8): (0.2-4): (2-15).
6. The comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material according to claim 5, It is characterized in that The mass ratio of the polyethylene glycol diamine, polyglycidyl methacrylate and polymetallic oxygen cluster is (1.5-6): (0.5-3): (3-13).
7. The comb-shaped cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material according to claim 5, It is characterized in that The mass ratio of the polyethylene glycol diamine, polyglycidyl methacrylate and polymetallic oxide cluster is (2-5): (0.8-1.5): (5-11).
8. A method for preparing the comb-like cross-linked network polymer-based multi-metal oxide cluster composite proton exchange membrane material according to any one of claims 1 to 7, Features The following steps are involved: Polyethylene glycol diamine and poly(glycidyl methacrylate) are stirred evenly in a solvent to make them fully cross-linked, and then polyoxometalates are added and stirred evenly to obtain a composite solution; the composite solution is dried to form a film to obtain a composite proton exchange membrane, that is, the comb-like cross-linked network polymer-based polyoxometalates composite proton exchange membrane material.
9. The preparation method according to claim 8, It is characterized in that The mass fraction of the polymetallic oxygen cluster in the complex solution is 40-70%; The solvent includes at least one of a furan solvent, an alcohol solvent, dimethyl sulfoxide, and dimethylacetamide; After adding the polyoxometalate, the mixture is stirred uniformly at 40° C. to 100° C. to obtain a complex solution.
10. Use of the comb-like cross-linked network polymer-based multi-metal oxygen cluster composite proton exchange membrane material according to any one of claims 1 to 7 in hydrogen and oxygen fuel cells.