Method for improving performance of sulfur-based composite solid electrolyte film by regulating skeleton structure

By adding polytetrafluoroethylene and acryloyl monomers to the sulfide solid electrolyte matrix, the supporting framework of the crosslinked structure is formed, which solves the cracks and thickness problems of the sulfide solid electrolyte sheet and improves its ionic conductivity and mechanical properties , realize the preparation of high-performance sulfur-based composite solid electrolyte film.

CN119009094APending Publication Date: 2024-11-22GUIZHOU MATERIAL IND TECH INSTITUE
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410998272.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The ceramic sheet made of direct cold pressing of sulfide solid electrolyte powder is prone to cracks and has a high thickness, which hinders the realization of high specific energy of solid lithium batteries. The existing sulfur-based solid electrolyte films have insufficient ionic conductivity and mechanical properties. Influence its application.

Method used

Polytetrafluoroethylene and acryloyl monomers are added to the sulfide solid electrolyte matrix, and multifunctional crosslinking agent and initiator are added to form a crosslinking structure through ball milling and rolling to prepare a high-performance flexible sulfur-based solid state Electrolyte film.

Benefits of technology

The room temperature ion conductivity of the sulfur-based composite solid electrolyte film is improved to 16.7 mS/cm, and its mechanical properties are enhanced, avoiding defects and short-circuit problems caused by pressure.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of electrode materials, in particular to a method for improving the performance of a sulfur-based composite solid electrolyte film by regulating and controlling a skeleton structure. According to the preparation method, an acryloyl monomer is polymerized to form a cross-linked structure, the cross-linked structure and polytetrafluoroethylene physically form a network interpenetrating supporting framework, a framework structure with the strength equal to that of a chemical bond is provided under the condition that chemical reaction with a sulfide matrix does not occur, and the framework structure is compounded with sulfide to prepare the high-performance sulfenyl composite solid electrolyte film; and the ionic conductivity at room temperature can be up to 16.7 mS / cm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrode materials, and in particular to a method for improving the performance of a sulfur-based composite solid electrolyte film by regulating a skeleton structure. Background Art

[0002] All-solid-state lithium batteries are regarded as the development direction of the next generation of energy storage batteries. By using a non-flammable solid electrolyte layer to replace the low-ignition-point organic electrolyte in traditional lithium-ion batteries, the safety performance of lithium batteries can be greatly improved. At the same time, it can also be paired with a lithium metal negative electrode to achieve a higher energy density and further develop the application potential of lithium batteries. Solid electrolytes are the core components of all-solid-state lithium batteries. Sulfide solid electrolytes have the advantages of high ionic conductivity and high ductility, and are a major development direction for solid electrolytes. When preparing larger-sized solid-state lithium batteries, ultra-thin solid electrolyte sheets need to be prepared. However, ceramic sheets made by direct cold pressing of sulfide solid electrolyte powders are prone to cracking and cannot be directly used; and the thickness is high, which hinders the realization of high specific energy of solid-state batteries.

[0003] The composite of sulfide and polymer to prepare a flexible sulfur-based solid electrolyte film with high ionic conductivity can improve its molding performance and reduce thickness while taking into account the high ionic conductivity of the sulfide matrix. The currently reported methods for preparing sulfur-based solid electrolyte films mainly include liquid phase method and solid phase method: the organic solvent used in the liquid phase method is easy to remain, and the sulfide will react with the polar solvent, resulting in low ionic conductivity of the prepared film; the solid phase method mainly adopts hot pressing, hot roller and other methods to directly press the mixture of polymer and sulfide into shape. Since it does not involve the addition of solvent, the ionic conductivity is relatively high. In 2019, Hippauf et al. (Hippauf F, Schumm et al. Overcoming binder limitations of sheet-type solid-state cathodes using a solvent-free dry-film approach [J]. Energy Storage Materials, 2019, 21: 390-8.) used fiber polytetrafluoroethylene (PTFE) and Li6PS5Cl to prepare a sulfur-based composite electrolyte membrane with a thickness of 150 μm, and the room temperature ionic conductivity was 2.7 mS / cm. However, the sulfur-based electrolyte film directly prepared by fiber polytetrafluoroethylene (PTFE) and sulfide solid electrolyte dry method not only has lower ionic conductivity than the matrix sulfide solid electrolyte, but also has poor mechanical properties. When it is matched with alloy or lithium metal negative electrode to assemble into a solid-state battery, it will produce defects due to pressure, and even cause the metal negative electrode to penetrate the electrolyte film and cause a short circuit, which seriously affects the practical application of solid electrolyte film. Summary of the invention

[0004] In order to solve the above technical problems existing in the prior art, the present invention provides a method for improving the performance of a sulfur-based composite solid electrolyte film by regulating the skeleton structure, which is specifically achieved through the following technical solutions.

[0005] A method for improving the performance of a sulfur-based composite solid electrolyte film by regulating the skeleton structure comprises the following steps:

[0006] (1) adding 0.1-6 wt % of polytetrafluoroethylene (PTFE) and 0.1-6 wt % of acryl monomer to a sulfide solid electrolyte matrix;

[0007] (2) adding 0.01-0.03 wt % of a multifunctional crosslinking agent and 0.02-0.05 wt % of an initiator to the mixture obtained in step (1);

[0008] (3) the mixture obtained in step (2) is ball-milled at medium speed using a planetary ball mill; and then rolled using a double-roll mill at a temperature of 80-130° C. to form a film with a thickness of 30-120 μm;

[0009] (4) The film is polymerized by an initiator to induce acryl monomers to form a cross-linked structure, which forms a network interpenetrating support skeleton with polytetrafluoroethylene, thereby preparing a high-performance flexible sulfur-based solid electrolyte film.

[0010] Furthermore, the sulfide solid electrolyte matrix is ​​Li6-xPS5-xCl1+x or Li9.6-0.2xSi3-4.2xP4.8xS12-xClx.

[0011] Furthermore, the acryl monomer is butyl acrylate, methyl acrylate, acryl or other acryl monomers.

[0012] Furthermore, the multifunctional cross-linking agent is ethylene glycol dimethacrylate or N,N-methylenebisacrylamide.

[0013] Furthermore, the initiator is a photoinitiator or a thermal initiator.

[0014] The thermal initiator may be azobisisobutyronitrile or dimethyl azobisisobutyrate. The photoinitiator may be 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone.

[0015] Furthermore, the medium-speed ball milling is specifically ball milling at 150-300 rpm for 30 min.

[0016] Furthermore, the rolling pressure of the roller machine is 3T.

[0017] Furthermore, the initiator, specifically a photoinitiator or a thermal initiator, is used under light or heating conditions, and specific light and heating parameters are adjusted according to different initiators.

[0018] Compared with the prior art, the technical effects created by the present invention are embodied in:

[0019] The present application utilizes the polymerization of acryl monomers to form a cross-linked structure, physically forming a network interpenetrating support skeleton with polytetrafluoroethylene, providing a skeleton structure with strength equivalent to that of a chemical bond without chemically reacting with the sulfide matrix, and preparing a high-performance sulfur-based composite solid electrolyte film in combination with sulfides, with a room temperature ionic conductivity of up to 16.7 mS / cm. DETAILED DESCRIPTION

[0020] The technical solution of the present invention is further defined below in conjunction with specific implementation methods, but the scope of protection required is not limited to the description.

[0021] Example 1

[0022] (1) Weigh 98 wt% of Li 5.5 PS 4.5 C 1.5 Solid electrolyte (9.8 g), 1 wt% polytetrafluoroethylene (0.1 g) and 1 wt% butyl acrylate (0.1 g);

[0023] (2) adding azobisisobutyronitrile (0.02 g) and ethylene glycol dimethacrylate (0.02 g) to the mixture obtained in step (1);

[0024] (3) The mixture obtained in step (2) was mixed by medium-speed ball milling (250 rpm, 30 min) in a planetary ball mill, then heated to 90° C., and rolled multiple times to form a dense film of 120 μm;

[0025] (4) The film is heated to 100°C and kept at this temperature for 6 hours to thermally initiate polymerization of the acryl monomer to form a cross-linked structure, which physically forms a network interpenetrating support skeleton structure with polytetrafluoroethylene to prepare a sulfur-based composite electrolyte film.

[0026] Example 2

[0027] (1) Weigh 99 wt% Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 Solid electrolyte (9.9 g), 0.5 wt% polytetrafluoroethylene (0.05 g) and 0.5 wt% butyl acrylate (0.05 g);

[0028] (2) adding azobisisobutyronitrile (0.01 g) and ethylene glycol dimethacrylate (0.01 g) to the mixture obtained in step (1);

[0029] (3) The mixture obtained in step (2) was mixed by medium-speed ball milling (250 rpm, 30 min) in a planetary ball mill, and then the powder was heated to 100° C. and rolled multiple times to form a dense film of 60 μm;

[0030] (4) The film is heated to 120° C. and kept at this temperature for 6 hours to thermally initiate polymerization of the acryl monomer to form a cross-linked structure, which physically forms a network interpenetrating support skeleton structure with polytetrafluoroethylene to prepare a sulfur-based composite electrolyte film.

[0031] Example 3

[0032] (1) Weigh 98 wt% of L i5.5 PS 4.5 Cl 1.5 Solid electrolyte (9.8 g), 1 wt% polytetrafluoroethylene (0.1 g) and 1 wt% butyl acrylate (0.1 g);

[0033] (2) adding azobisisobutyronitrile (0.02 g) and N,N-methylenebisacrylamide (0.02 g) to the mixture obtained in step (1);

[0034] (3) The mixture obtained in step (2) was mixed by medium-speed ball milling (250 rpm, 30 min) in a planetary ball mill, then heated to 100° C., and rolled multiple times to form a dense film of 60 μm;

[0035] (4) The film is heated to 120° C. and kept at this temperature for 6 hours to thermally initiate polymerization of the acryl monomer to form a cross-linked structure, which physically forms a network interpenetrating support skeleton structure with polytetrafluoroethylene to prepare a sulfur-based composite electrolyte film.

[0036] The ionic conductivity of each embodiment was measured, and the specific results are as follows:

[0037] The ionic conductivity of the composite electrolyte film prepared in each embodiment was measured, and the experimental method was as follows:

[0038] The prepared composite electrolyte film was cut into 10 mm diameter discs using a cutting mold and placed in a mold. The discs were pressurized to 360 MPa and maintained for 5 min. Then, a Gamry Interface 1010 electrochemical workstation was used to measure the pressure at 10 6 Hz~10 -2 The film resistance R is obtained by electrochemical impedance spectroscopy (EIS) testing in the HZ frequency range, and then the ionic conductivity is calculated.

[0039] The ionic conductivity (σ) is calculated as follows: σ = L / RS, where L is the thickness, S is the area, and R is the resistance.

[0040] Table 1 Thickness and ionic conductivity (25°C) parameters of the sulfur-based composite solid electrolyte films prepared in Examples 1-3

[0041] Film thickness (μm) Ionic conductivity (mS / cm) Example 1 120 16.7 Example 2 60 10.9 Example 3 60 9.8

[0042] Finally, it should be pointed out that the above embodiments are only representative examples of the present invention. Obviously, the technical solution of the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by ordinary technicians in this field should be considered as the protection scope of the present invention.

Claims

1. A method for improving the performance of a sulfur-based composite solid electrolyte film by regulating the skeleton structure, characterized in that: The following steps are involved: (1) adding 0.1-6 wt % of polytetrafluoroethylene and 0.1-6 wt % of acryl monomer to a sulfide solid electrolyte matrix; (2) adding 0.01-0.03 wt % of a multifunctional crosslinking agent and 0.02-0.05 wt % of an initiator to the mixture obtained in step (1); (3) The mixture obtained in step (2) is milled at medium speed using a planetary ball mill for 1-2 hours at a speed of 200-350 rpm; after being mixed evenly, the mixture is taken out from the ball mill, heated to 80-130° C., and rolled using a double roller mill to form a film with a thickness of 30-120 μm; (4) placing the film under the reaction conditions required by the initiator for a reaction of 6-20 hours to promote the polymerization and cross-linking of the acryl monomers to form an interpenetrating structural support skeleton with polytetrafluoroethylene, thereby preparing a high-performance flexible sulfur-based solid electrolyte film.

2. The method for improving the performance of sulfur-based composite solid electrolyte film by regulating the skeleton structure according to claim 1, characterized in that: The sulfide solid electrolyte matrix is ​​Li 6-x PS 5-x Cl x or Li 9.6-0.2x Si 3-4.2x P 4.8x S 12- x Cl x .

3. The method for improving the performance of sulfur-based composite solid electrolyte film by regulating the skeleton structure according to claim 1, characterized in that: The acryl monomer units are butyl acrylate, methyl acrylate and acrylamide.

4. The method for improving the performance of sulfur-based composite solid electrolyte film by regulating the skeleton structure according to claim 1, characterized in that: The multifunctional cross-linking agent is ethylene glycol dimethacrylate or N,N-methylenebisacrylamide.

5. The method for improving the performance of sulfur-based composite solid electrolyte film by regulating the skeleton structure according to claim 1, characterized in that: The initiator is a photoinitiator or a thermal initiator.

6. The method for improving the performance of sulfur-based composite solid electrolyte film by regulating the skeleton structure according to claim 5, characterized in that: The thermal initiator is azobisisobutyronitrile or dimethyl azobisisobutyrate.

7. The method for improving the performance of sulfur-based composite solid electrolyte film by regulating the skeleton structure according to claim 5, characterized in that: The photoinitiator is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

8. The method for improving the performance of sulfur-based composite solid electrolyte film by regulating the skeleton structure according to claim 1, characterized in that: The medium-speed ball mill is specifically 150-300 rpm.

9. The method for improving the performance of sulfur-based composite solid electrolyte film by regulating the skeleton structure according to claim 1, characterized in that: The rolling pressure of the roller machine is 3T.

10. The method for improving the performance of sulfur-based composite solid electrolyte film by regulating the skeleton structure according to claim 1, characterized in that: The initiator is specifically a photoinitiator or a thermal initiator, and the specific lighting and heating parameters are adjusted according to the different initiators under lighting or heating conditions.

Citation Information

Cited By

  • Sulfide solid electrolyte membrane and preparation method and application thereof

    CN120149520A

  • A sulfide solid electrolyte membrane and its preparation method and application

    CN120149520B