Method for resource utilization of lithium battery negative electrode waste coating slurry
By using sulfuric acid, hydrogen peroxide and ozone in the production of lithium-ion batteries to destroy the dispersion system of waste coating slurry, the efficient solid-liquid separation of waste coating slurry of lithium battery negative electrode is achieved, and the problems of resource waste and environmental pollution are solved. , promoting the recycling and clean production of the lithium battery industry.
Patent Information
- Application Number
- CN202310548532.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-22
AI Technical Summary
The negative electrode waste coating slurry produced in the production process of lithium-ion batteries is difficult to treat harmlessly and utilize resources in a resource waste and environmental pollution due to its high moisture content, fine particles and strong dispersion stability.
An oxidation system constructed with sulfuric acid, hydrogen peroxide and ozone is used to adjust the pH value or add oxidants to destroy the colloidal dispersion system of waste coating slurry and achieve efficient solid-liquid separation. The resulting solid can be used in the production of industrial activated carbon.
It realizes efficient solid-liquid separation of waste coated slurry, reduces energy consumption and costs, improves filtration performance, has significant environmental and economic benefits, and promotes resource recycling and clean production in the lithium battery industry.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of recycling of lithium battery material resources, and in particular relates to a method for recycling waste coating slurry of lithium battery negative electrodes. Background Art
[0002] As an environmentally friendly new energy source, lithium-ion batteries have been widely used in consumer electronics, electric vehicles, energy storage and other fields with their outstanding advantages such as high voltage, high specific energy, long cycle life and good safety performance. The main manufacturing process of lithium-ion battery pole pieces is: slurry stirring → coating → drying → rolling → winding, in which the lithium battery negative electrode slurry is composed of adhesive, conductive agent, graphite carbon powder, etc. The two processes of lithium-ion battery slurry stirring and coating have a significant impact on the performance of lithium-ion batteries. Waste coating slurry is inevitably generated during the slurry stirring and coating process. Waste coating slurry has a high moisture content (over 90%), fine particles (tens to hundreds of nanometers), and strong migration fluidity. It contains organic adhesives and metals. If improperly disposed of, it will not only cause serious waste of resources, but also cause serious ecological and environmental safety.
[0003] In the manufacturing process of lithium-ion battery electrodes, only when graphite and carbon black particles are evenly dispersed in the slurry and the pole piece can the lithium-ion battery show good performance, which requires the negative electrode slurry to have excellent mixing uniformity. However, because both graphite and carbon black particles are hydrophobic and non-polar on the surface, they aggregate in water without additives and cannot be dispersed. Therefore, CMC (sodium carboxymethyl cellulose) is usually added during the slurry mixing process to thicken and disperse, and SBR (styrene-butadiene rubber) plays a bonding role during the pole piece coating process. Qualified negative electrode coating slurry is a viscous colloidal dispersion system with strong dispersion stability and is difficult to filter directly. In summary, solvents such as CMC and SBR bring highly uniform and stable dispersion to the coating slurry, while superimposing the problem of solid-liquid separation of the slurry. Therefore, efficient separation of the solid-liquid two phases of waste coating slurry is the key to its treatment and disposal and resource utilization.
[0004] At present, a large number of studies are mainly focused on the treatment and resource utilization of waste lithium-ion batteries, and no research has focused on the treatment and resource recovery of pollutants in its production process. Waste negative electrode slurry contains carbon materials such as graphite and carbon black. Resource recovery of carbon materials can reduce the environmental hazards of waste negative electrode slurry and realize the recycling of resources. For the separation of colloidal dispersion systems, studies have used degumming agents, high temperature, high shear force devices (homogenizers or high-pressure screw pumps, etc.) to destroy the stability of the colloidal dispersion system and achieve solid-liquid separation of the system. The addition of degumming agents will introduce impurities, which will affect the separation and purification of subsequent products. High temperature and high shear force have problems such as high energy consumption and strict equipment requirements. The present invention develops an efficient separation technology for lithium battery negative electrode waste coating slurry based on the basic characteristics of waste negative electrode slurry. The technology uses an oxidation system constructed by sulfuric acid, hydrogen peroxide, ozone, etc. to affect the solubility of CMC and the stability of SBR in the negative electrode waste coating slurry to destroy the stable colloidal dispersion system of the waste coating slurry and achieve its efficient solid-liquid separation. The separated carbon material can be used as industrial activated carbon. The specific principle of this technology is that CMC and SBR organic additives are highly sensitive to pH, which is manifested in that the dissociation degree of CMC decreases with the decrease of pH value, thereby reducing the content of ionized CMC in the waste slurry, resulting in a decrease in the electrostatic repulsion of the waste slurry dispersion system, and ultimately destroying the stability of the bridged dispersion system formed by CMC and SBR, and causing particles to flocculate and agglomerate. Compared with the prior art, the present invention has the remarkable characteristics of strong operability, low energy consumption and low cost. Summary of the invention
[0005] The waste negative electrode coating slurry generated in the lithium battery production process has a high moisture content, fine particles, strong dispersion stability, and is difficult to be harmlessly treated and recycled. The present invention provides a method for recycling waste negative electrode coating slurry of lithium batteries based on the dispersion characteristics of waste negative electrode coating slurry of lithium batteries. By destroying the dispersion stability of waste negative electrode coating slurry of lithium batteries, efficient solid-liquid separation is achieved, and the obtained solid product can be used as industrial activated carbon and carbon black products. This method solves the problem of harmless disposal and resource utilization of waste coating slurry generated in the stirring and coating process of negative electrode slurry in lithium battery production. It effectively controls the emission of pollutants in the lithium battery production process and is one of the effective ways to promote resource recycling in the lithium battery industry and promote clean production.
[0006] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a method for resource utilization of waste coating slurry of lithium battery negative electrode, comprising:
[0007] A certain amount of sulfuric acid is added to the waste coating slurry of the lithium battery negative electrode, the pH value is adjusted to 1-4, the mixture is stirred for a period of time, the solid and liquid are separated, and the obtained solid is dried and crushed to obtain industrial activated carbon;
[0008] or
[0009] Ozone is added to the waste coating slurry of the negative electrode of lithium battery, or hydrogen peroxide and ozone are added, reacted for a period of time, solid-liquid separation is performed, and the obtained solid is dried and crushed to obtain industrial activated carbon.
[0010] Preferably, a certain amount of sulfuric acid is added to the waste coating slurry of the lithium battery negative electrode, the pH value is adjusted to 1-4, and the reaction is stirred for more than 30 minutes.
[0011] Preferably, ozone is added to the waste coating slurry of the lithium battery negative electrode and the reaction is carried out for more than 2 hours.
[0012] Preferably, hydrogen peroxide and ozone are added to the waste coating slurry of the lithium battery negative electrode and reacted for more than 30 minutes.
[0013] Preferably, ozone is added to the waste coating slurry of the lithium battery negative electrode, and the amount of ozone added is 0.5-12g per liter of slurry.
[0014] Preferably, 30 wt % of hydrogen peroxide and ozone are added to the waste coating slurry of the lithium battery negative electrode, and the mass ratio of hydrogen peroxide to ozone is 0.3:1 to 3:1, preferably 1 to 1.5:1.
[0015] Compared with the existing gel breaking and separation invention, the present invention has the following significant advantages:
[0016] (1) The present invention achieves debonding of the colloidal dispersion system by adjusting the pH value of the waste coating slurry or adding a small amount of oxidant to destroy the solubility and stability of the dispersant and adhesive therein. This technology does not require the investment of special debonding agents and high-energy-consuming special equipment, and has the technical advantages of strong operability and low overall cost.
[0017] (2) Based on the degumming of waste coating slurry, the present invention greatly improves the filtering performance of waste slurry, which can not only filter and separate the waste slurry efficiently, but also recycle the carbon materials therein, thus having significant environmental and economic benefits. DETAILED DESCRIPTION
[0018] In order to better illustrate the present invention, specific embodiments are given below to describe the present invention in more detail. The protection scope of the present invention is not limited to the examples given.
[0019] The present invention starts from the basic characteristics of waste negative electrode slurry, combines the properties of CMC and SBR organic additives therein, and develops an efficient separation technology for lithium battery negative electrode waste coating slurry. This technology uses an oxidation system constructed by sulfuric acid, hydrogen peroxide / ozone, etc. to affect the solubility of CMC and the stability of SBR in the negative electrode waste coating slurry, so as to destroy the stable colloidal dispersion system of the waste coating slurry and achieve its efficient solid-liquid separation. The separated carbon material can be used as industrial activated carbon. Compared with the prior art, the present invention has the remarkable characteristics of strong operability, low energy consumption and cost.
[0020] The waste negative electrode coating slurry No. 1 and the waste negative electrode coating slurry No. 2 involved in the embodiment come from a lithium battery production enterprise, wherein the moisture content of the waste negative electrode coating slurry No. 1 is 88%, and the moisture content of No. 2 is 95%. The different moisture contents of the slurries do not affect the specific implementation process.
[0021] Example 1
[0022] Take 1 L of No. 1 waste negative electrode coating slurry, add 20 mL of sulfuric acid to the slurry, adjust the pH value to 2.0, place the slurry with adjusted pH value in a stirred reactor and stir at room temperature for 30 min. After the reaction is completed, the waste slurry is successfully filtered, and a carbon-containing filter residue with a moisture content of 46.97% is obtained through laboratory filtration equipment. The moisture content of the untreated waste coating slurry is reduced by 41.03%, and the transmittance is increased by 54%. The filter residue is dried and ground to obtain industrial activated carbon. The activated carbon has an adsorption capacity of 435 mg / g for methylene blue in wastewater, a removal rate of 89.2% for water COD, and a removal rate of 54% for Cr. 6+ The removal rate is 52%. The above indicators meet the requirements of LY / T3279-2021 "Technical Indicators of Activated Carbon for Industrial Water Treatment".
[0023] Example 2
[0024] 500 mL of No. 2 waste negative electrode coating slurry was placed in a reactor, and 5 g of ozone was introduced into the reactor for 4 h. After the reaction, the laboratory filtration equipment successfully filtered the waste coating slurry, and the moisture content of the filter residue dropped to 64.21%, which was 30.79% lower than that of the untreated waste coating slurry, and the transmittance increased by 38%. The filter residue was dried and ground to obtain industrial activated carbon. The activated carbon has an adsorption capacity of 450 mg / g for methylene blue in wastewater, a removal rate of 90.2% for water COD, and a removal rate of 90.2% for Cr. 6+ The removal rate is 60.4%. The above indicators meet the requirements of LY / T3279-2021 "Technical Indicators of Activated Carbon for Industrial Water Treatment".
[0025] Example 3
[0026] 500 mL of No. 1 waste negative electrode coating slurry was placed in a reactor, 2 g of ozone was introduced, 4.5 g of 30 wt% hydrogen peroxide was added, and the reaction was continued for 45 min. After the reaction was completed, the waste slurry was successfully filtered through a laboratory filtration device. The moisture content of the filter residue was 61.81%, which was 26.19% lower than that of the untreated waste coating slurry, and the transmittance was increased by 32%. The filter residue was dried and ground to obtain industrial activated carbon. The activated carbon has an adsorption capacity of 450 mg / g for methylene blue in wastewater, a removal rate of 92.4% for water COD, and a removal rate of 92.4% for Cr. 6+The removal rate is 64.6%. The above indicators meet the requirements of LY / T3279-2021 "Technical Indicators of Activated Carbon for Industrial Water Treatment".
[0027] Example 4
[0028] Take 500 mL of No. 1 waste negative electrode coating slurry, add 5 mL of sulfuric acid to the slurry, adjust the pH value to 5.0, place the slurry with adjusted pH value in a stirred reactor and stir at room temperature for 30 min. After the reaction is completed, transfer the waste slurry to a filtration device. No filter cake is formed in the device, and the waste coating slurry fails to achieve solid-liquid separation.
[0029] Example 5
[0030] Take 500 mL of No. 1 or No. 2 waste negative electrode coating slurry, add 5 g of 30 wt% hydrogen peroxide, stir and react for 2.5 h. After the reaction, transfer the waste slurry to the filtration device. No filter cake is formed in the device, and the waste coating slurry cannot achieve solid-liquid separation.
[0031] The above is a preferred embodiment of the present invention, but does not limit the scope of protection of the present invention. Technicians in this field may make some non-essential improvements to the present invention based on the above invention content, which still fall within the scope of protection of the present invention.
Claims
1. A method for resource utilization of waste coating slurry of lithium battery negative electrode, characterized in that: include: A certain amount of sulfuric acid is added to the waste coating slurry of the lithium battery negative electrode, the pH value is adjusted to 1-4, the mixture is stirred for a period of time, the solid and liquid are separated, and the obtained solid is dried and crushed to obtain industrial activated carbon; or Ozone is added to the waste coating slurry of the negative electrode of lithium battery, or hydrogen peroxide and ozone are added, reacted for a period of time, solid-liquid separation is performed, and the obtained solid is dried and crushed to obtain industrial activated carbon.
2. The method according to claim 1, characterized in that Add a certain amount of sulfuric acid to the waste coating slurry of the lithium battery negative electrode, adjust the pH value to 1-4, and stir the reaction for more than 30 minutes.
3. The method according to claim 1, characterized in that Add ozone to the waste coating slurry of the lithium battery negative electrode and react for more than 2 hours.
4. The method according to claim 1, characterized in that Add hydrogen peroxide and ozone to the waste coating slurry of lithium battery negative electrode and react for more than 30 minutes.
5. The method according to claim 1, characterized in that Ozone is added to the waste coating slurry of the lithium battery negative electrode, with the amount of ozone added being 0.5~12g per liter of slurry.
6. The method according to claim 1, wherein: Hydrogen peroxide and ozone are added to the lithium battery negative electrode waste coating slurry, and the mass ratio of hydrogen peroxide to ozone is 0.3:1 to 3:1, preferably 1 to 1.5:1.