Temperature control polymer composite diaphragm as well as preparation method and application thereof

By using a negative electrical card material layer in the lithium-ion battery separator, using the combination of a three-dimensional ceramic skeleton and polar polymer material, the thermal runaway problem of lithium-ion batteries is solved, temperature regulation and high ionic conductivity are achieved, and battery safety is improved Sex and capacity.

CN119009356AActive Publication Date: 2024-11-22VKAN CERTIFICATION & TESTING
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411210354.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators will cause temperature rise when overcharging, mechanically extruded or short-circuited, causing heat out of control and explosion risks, and will not be able to cool down in real time to prevent the battery from overheating.

Method used

The negative electric card material layer consisting of a three-dimensional ceramic skeleton with negative electric card effect and polar polymer material is used to regulate the temperature layer, absorb heat during charging and discharging through dipole flip or offset, reduce the temperature of the diaphragm and battery, and increase the temperature of the diaphragm and battery Ion conductivity, preventing heat shrinkage and short circuit.

Benefits of technology

The temperature regulation and high ionic conductivity of lithium-ion batteries are achieved, the risk of thermal runaway is reduced, the battery safety and capacity is improved, the growth of lithium dendrites is inhibited, and the battery life is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020158910000111
    Figure BDA0005020158910000111
Patent Text Reader

Abstract

The invention discloses a temperature control polymer composite diaphragm which comprises a diaphragm substrate and a temperature control layer arranged on one side or two sides of the diaphragm substrate, the diaphragm substrate is a polymer film; the temperature regulation and control layer is a negative electrocaloric material layer, and the negative electrocaloric material layer is composed of a three-dimensional ceramic skeleton and a polar polymer material which both have a negative electrocaloric effect. The invention also discloses a preparation method of the temperature control polymer composite diaphragm and application of the temperature control polymer composite diaphragm in a lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a temperature-controlling polymer composite diaphragm and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have been widely used in portable electronic devices, large-scale energy storage systems, electric vehicles and other fields due to their high energy density, long cycle life and low self-discharge. However, thermal runaway of batteries in electric vehicles and fixed grid-scale energy storage systems is still the primary safety issue and one of the most urgent and challenging tasks. As one of the four key components of lithium-ion batteries, the separator can prevent the short circuit between the positive and negative electrodes and allow the Li + Free transmission is crucial to the safety and reliability of lithium-ion batteries. At present, porous and thin polyolefin membranes have become the most mainstream commercial separators due to their low cost, good mechanical properties and electrochemical stability; but unfortunately, when lithium-ion batteries are overcharged, mechanically squeezed or short-circuited, polyolefin membranes will shrink significantly at 130-150°C, resulting in direct contact between the anode and cathode, triggering complex chemical reactions, aggravating the temperature rise of the battery, and then severe heat accumulation causes severe redox reactions between the oxygen released by the cathode and the combustible materials in the battery, further leading to explosions and even fires.

[0003] The current technical research on lithium battery separators mainly includes enhancing their mechanical stability, improving their wettability to electrolytes, improving the porosity of separators, and improving the thermal stability of separators. In terms of thermal stability, reasonable doping and coating of separators can improve the thermal stability of separators to a certain extent, thereby improving the safety of lithium batteries, but it may affect the overall ionic conductivity of the battery, and it is impossible to cool the battery temperature during the battery charging and discharging process to prevent the battery temperature from being too high. For example, China's published patent CN112928389A obtains a separator with a thermostatic function by coating a phase change material, but the separator can only absorb battery heat to reduce the battery temperature when the phase change material undergoes a phase change, and the phase change temperature point of the phase change material is low, and it is impossible to suppress the thermal shrinkage of the separator in a high temperature state. For example, China's published patent CN114284640A prepares a thermal switch coating to melt the separator at a high temperature, blocking the migration of lithium ions, thereby suppressing the spread of heat. In summary, there is no separator material in the prior art that can reduce the temperature of the battery in real time during the charging and discharging process of a lithium-ion battery to ensure that the battery will not overheat and operate normally. Summary of the invention

[0004] One of the purposes of the present invention is to provide a temperature-controlling polymer composite diaphragm, which has a temperature control function and high ionic conductivity.

[0005] A second object of the present invention is to provide a method for preparing the above-mentioned temperature-controlling polymer composite diaphragm.

[0006] The third object of the present invention is to provide an application of the above-mentioned temperature-controlling polymer composite diaphragm.

[0007] The first object of the present invention is achieved through the following technical solutions.

[0008] A temperature-controlling polymer composite diaphragm, characterized in that it comprises a diaphragm substrate and a temperature-controlling layer arranged on one side or both sides thereof;

[0009] The diaphragm substrate is a polymer film;

[0010] The temperature regulating layer is a negative electrocaloric material layer, and the negative electrocaloric material layer is composed of a three-dimensional ceramic skeleton and a polar polymer material both having a negative electrocaloric effect.

[0011] The present invention adopts a three-dimensional ceramic skeleton and a polar polymer material both having a negative electrocaloric effect to form a negative electrocaloric material layer, that is, a temperature control layer, so that the temperature control polymer composite diaphragm has a temperature control function and high ionic conductivity. When the battery is charged and discharged (that is, when there is an external voltage), the dipoles inside the negative electrocaloric material layer flip or shift, and change from an ordered state to a disordered state; on the one hand, the disordered dipoles provide multiple migration channels for lithium ions, improve the mobility of lithium ions, that is, improve the ionic conductivity of the diaphragm; on the other hand, the dipoles change from an ordered state to a disordered state, which increases the entropy value of the negative electrocaloric material layer, absorbs environmental heat, helps to reduce the temperature of the diaphragm and the battery, and prevents the diaphragm from overheating and causing thermal shrinkage or curling, which causes the positive and negative electrodes of the battery to contact each other, thereby causing a short circuit and avoiding the thermal runaway of the battery. Further, the present invention fills the polar polymer material into the three-dimensional ceramic skeleton to form a whole, enhances the negative electrocaloric effect, produces a larger adiabatic temperature change, and can absorb higher heat when there is an external voltage, which is more conducive to regulating the temperature of the diaphragm and the battery. In addition, polar polymer materials have good flexibility and processability, and the three-dimensional ceramic skeleton has high hardness and thermal conductivity. The temperature regulating layer composed of the two is a diaphragm refrigeration material with good flexibility and high electrical conductivity.

[0012] The material of the three-dimensional ceramic skeleton can be selected from ceramic particles with relaxor ferroelectric or antiferroelectric effect, such as relaxor ferroelectric lead zirconate titanate or its dopants, potassium / sodium / silver-based niobate or its dopants, strontium titanate or its dopants. Preferably, the material of the three-dimensional ceramic skeleton of the present invention is a relaxor ferroelectric lead zirconate titanate dopant, more preferably a relaxor ferroelectric lead zirconate titanate dopant doped with tin, specifically Pb 0.97 La 0.02 Zr 0.91 Sn 0.05 TiO4.

[0013] The polar polymer material is at least one of poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene), poly(vinylidene fluoride-trifluoroethylene), polyurea aromatic linear dielectric polymer, perovskite relaxor ferroelectric polymer material, polyimide material, polyamide material, and polystyrene material; the present invention prefers poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene), hereinafter referred to as P(VDF-TrFE-CFE).

[0014] The material of the membrane substrate can be a conventional polymer for preparing a membrane, and can be specifically selected from at least one of polyacrylonitrile, polyethylene, polypropylene, polyvinylidene fluoride, polyvinyl pyrrolidone, poly(m-phenylene isophthalamide) and poly(methyl methacrylate).

[0015] Preferably, the thickness of the temperature-controlling polymer composite diaphragm is 30 to 200 μm; wherein the thickness ratio of the diaphragm substrate to the temperature-controlling layer is 5:1 to 30:1.

[0016] To achieve the second purpose of the present invention, the present invention provides a method for preparing the above-mentioned temperature-controlling polymer composite diaphragm, which is characterized in that it includes the following steps: preparing a three-dimensional ceramic skeleton by a sol-gel method; filling a polar polymer material into the three-dimensional ceramic skeleton, and then hot pressing to obtain a temperature-controlling layer; finally, hot-pressing and compounding the diaphragm base and the temperature-controlling layer to obtain the temperature-controlling polymer composite diaphragm.

[0017] As a specific embodiment, the method for preparing a three-dimensional ceramic skeleton of the present invention is: the raw materials for preparing the three-dimensional ceramic skeleton are evenly mixed with a solvent to obtain a sol; a polyurethane foam template is infiltrated in the sol, and then excess sol is squeezed out of the polyurethane foam template and dried at 35 to 65°C to obtain a precursor template; finally, the precursor template is sintered at 1000 to 1400°C for 1 to 3 hours (during this process, the polyurethane foam template is gasified and removed) to obtain a three-dimensional ceramic skeleton.

[0018] Preferably, the infiltration time is 15 to 20 minutes, more preferably 10 minutes.

[0019] Preferably, the solvent consists of 5-40 mL of ethanol, 1-10 mL of acetylacetone and 5-30 mL of glacial acetic acid; more preferably, it consists of 15 mL of ethanol, 5 mL of acetylacetone and 20 mL of glacial acetic acid.

[0020] Preferably, the raw materials for preparing the three-dimensional ceramic skeleton are PbO, La2O3, TiO2, ZrO2 and SnO2 to prepare the relaxor ferroelectric lead zirconate titanate dopant doped with tin. The mass ratio of the raw materials for preparing the three-dimensional ceramic skeleton to the solvent is 1:5 to 1:50.

[0021] Preferably, the precursor template is dried at 45° C., and the precursor template is sintered at 1200° C. for 2 h to obtain a three-dimensional ceramic skeleton.

[0022] As a specific embodiment, the method for preparing a temperature regulating layer of the present invention is: dissolving a polar polymer material to obtain a polar polymer material solution with a concentration of 5 to 35 wt%; then filling the polar polymer material solution into the three-dimensional ceramic skeleton prepared above, and then placing it in an oven at 40 to 80°C and heating it for 0.1 to 2 hours; repeating the above filling-heating operation several times until the three-dimensional ceramic skeleton is completely filled with the polar polymer material to obtain a composite material; drying the obtained composite material, and then hot pressing it at 0.1 to 1 MPa and 100 to 150°C for 10 to 25 minutes to convert the above composite material into a dense body to obtain a temperature regulating layer.

[0023] The concentration of the above-mentioned polar polymer material solution is obtained through a large number of experimental verifications; if there is too much polar polymer material in the temperature control layer, it will cause the lithium ion migration channel in the original diaphragm to be blocked, reduce the mobility of lithium ions, and thus affect the capacity of the battery; if there is too little polar polymer material in the temperature control layer, it will not have a cooling effect. During the battery charging and discharging process, it cannot play the role of reducing the battery temperature, which is not conducive to controlling the occurrence of battery thermal runaway.

[0024] Preferably, a polar polymer material solution with a concentration of 15 wt % is used; after the polar polymer material solution is filled into the three-dimensional ceramic skeleton, it is placed in an oven at 60° C. for 0.5 h.

[0025] Preferably, the obtained composite material is dried at 40-60°C for 8-12 hours, and then hot-pressed at 120°C for 15 minutes under a pressure of 0.5 MPa.

[0026] As a specific embodiment, the present invention places a temperature control layer on one side of the diaphragm substrate, performs hot pressing to obtain a polymer composite diaphragm, the hot pressing pressure is 0.5-1MPa, the temperature is 100-200°C, and the time is 1-10h; finally, the obtained polymer composite diaphragm is placed in a vacuum oven and annealed at 106°C for 10h to improve the crystallinity of the film to obtain the temperature-controlled polymer composite diaphragm. If the temperature control layer is set on both sides of the diaphragm substrate, the temperature control layer can be placed on both sides of the diaphragm substrate for hot pressing at the same time, or the temperature control layer can be placed on one side of the diaphragm substrate for hot pressing and then the other side is treated in the same way.

[0027] Preferably, the temperature-regulating layer and the diaphragm substrate are hot-pressed at a pressure of 0.5 MPa, a temperature of 110° C., and a time of 5 h.

[0028] Preferably, the preparation method of the diaphragm substrate is: mixing a polymer and N-methylpyrrolidone in a mass ratio of 1:10 to 1:50 to form a polymer solution; pouring the obtained polymer solution into a template, placing it in an oven at 40 to 60° C. for drying for 6 to 12 hours to obtain a diaphragm substrate.

[0029] Preferably, the polymer and N-methylpyrrolidone are stirred at 40-60° C. for 6-8 hours to obtain a polymer solution.

[0030] To achieve the third object of the present invention, the present invention provides the use of the above-mentioned temperature-controlling polymer composite diaphragm in a lithium-ion battery.

[0031] Preferably, the temperature control layer in the temperature control polymer composite separator is on the negative electrode side, which can further inhibit the growth of lithium dendrites.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The present invention composites a conventional polymer film with a negative charge card material layer (temperature control layer) to achieve regulation and control of the diaphragm temperature, so that the temperature-controlling polymer composite diaphragm has high ion conductivity and good electrolyte wettability.

[0034] When the battery is charged and discharged, that is, when there is an external voltage, the dipoles of the negatively charged card material inside the diaphragm change from an ordered state to a disordered state. The material absorbs the heat generated by the battery, lowers the battery temperature, and thus reduces the occurrence of thermal runaway of the battery. This can effectively ensure the safety of the battery and improve the thermal safety performance of the battery. At the same time, the disordered dipoles can provide more migration channels for lithium ions, promote lithium ion migration, and help increase the capacity of the battery.

[0035] When the temperature-controlling polymer composite diaphragm of the present invention is used, when the battery stops charging and discharging, that is, when the external electric field is removed, the temperature of the battery increases, which can reduce the polarization inside the battery, allowing lithium ions to migrate more, increasing the capacity of the battery, and inhibiting the growth of lithium dendrites. The temperature control layer in the temperature-controlling polymer composite diaphragm of the present invention is arranged on the negative electrode side, which can further inhibit the growth of lithium dendrites and reduce the battery capacity attenuation.

[0036] The temperature-controlling polymer composite diaphragm structure and preparation method of the present invention are simple. DETAILED DESCRIPTION

[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1 A temperature-controlled polymer composite membrane was prepared by the following steps:

[0039] S1: Pb 0.97 La 0.02 Zr 0.91 Sn 0.05 TiO4 material is prepared from PbO, La2O3, TiO2, ZrO2 and SnO2 with a purity greater than 99.0%, and the above raw materials are weighed according to the stoichiometric ratio; 15mL of ethanol, 5mL of acetylacetone and 20mL of glacial acetic acid are mixed to obtain a co-solvent, and then the above raw materials are dissolved in the co-solvent in turn and stirred to form a uniform solution, wherein the mass ratio of the raw materials of the three-dimensional ceramic skeleton to the co-solvent is 1:10, thereby obtaining a PLZST sol.

[0040] S2: The polyurethane foam template (TX704, ITW Texwipe) was soaked in the PLZST sol for 10 min; then the excess sol was squeezed out from the polyurethane foam template and dried at 45 °C to obtain the PLZST precursor template; finally, the PLZST precursor template was sintered at 1200 °C for 2 h to obtain a three-dimensional ceramic skeleton.

[0041] S3: P(VDF-TrFE-CFE) (62.1 / 30.1 / 7.8 mol%, Piezotech, France) was dissolved in DMF and stirred for 10 h to obtain a uniform P(VDF-TrFE-CFE) solution with a concentration of 15 wt%.

[0042] S4: The three-dimensional ceramic skeleton is placed on a PTFE mold with a length, width and height of 40x40x20 mm, and then the P(VDF-TrFE-CFE) solution obtained in S3 is filled into the three-dimensional ceramic skeleton, and then placed in an oven at 60°C for 0.5 h. The above filling-heating process is repeated several times until the three-dimensional ceramic skeleton is completely filled with P(VDF-TrFE-CFE) to obtain a composite material.

[0043] S5: The obtained composite material was dried at 50° C. for 10 h to remove excess solvent, and then the material was converted into a dense body by hot pressing at 0.5 MPa and 120° C. for 15 min to obtain a temperature regulating layer.

[0044] S6: Put polyethylene powder and NMP in a mass ratio of 1:20 into a glass container and stir them at 50°C for 6 hours to obtain a polymer solution; pour the polymer solution into a PTFE template and put it into an oven for drying at a temperature of 50°C for 8 hours to obtain a diaphragm substrate.

[0045] S7: Place the temperature regulating layer on one side of the diaphragm substrate and perform hot pressing at a pressure of 0.5 MPa, a temperature of 110°C, and a time of 5 hours; finally, the obtained polymer composite diaphragm is annealed in a vacuum oven at 106°C for 10 hours to improve the crystallinity of the membrane, and a temperature-controlled polymer composite diaphragm is obtained with a thickness of 38 μm, wherein the thickness ratio of the diaphragm substrate to the temperature regulating layer is 8:1.

[0046] Example 2 A temperature-controlled polymer composite diaphragm was prepared by the following steps:

[0047] S1: Pb 0.97 La 0.02 Zr 0.91 Sn 0.05 TiO4 material is prepared from PbO, La2O3, TiO2, ZrO2 and SnO2 with a purity greater than 99.0%, and the above raw materials are weighed according to the stoichiometric ratio; 13mL of ethanol, 7mL of acetylacetone and 15mL of glacial acetic acid are mixed to obtain a co-solvent, and then the above raw materials are dissolved in the co-solvent in turn and stirred to form a uniform solution, wherein the mass ratio of the raw materials of the three-dimensional ceramic skeleton to the co-solvent is 1:7, thereby obtaining a PLZST sol.

[0048] S2: The polyurethane foam template (TX704, ITW Texwipe) was soaked in the PLZST sol for 10 min; then the excess sol was squeezed out of the polyurethane foam template and dried at 45 °C to obtain the PLZST precursor template; finally, the PLZST precursor template was sintered at 1100 °C for 2 h to obtain a three-dimensional ceramic skeleton.

[0049] S3: P(VDF-TrFE-CFE) (62.1 / 30.1 / 7.8 mol%, Piezotech, France) was dissolved in DMF and stirred for 10 h to obtain a homogeneous P(VDF-TrFE-CFE) solution with a concentration of 28 wt%.

[0050] S4: Place the three-dimensional ceramic skeleton on a PTFE mold with a length, width and height of 40x40x20 mm; then fill the three-dimensional ceramic skeleton with the P(VDF-TrFE-CFE) solution obtained in S3, and then heat it in an oven at 60°C for 0.5h. Repeat the above filling-heating process several times until the three-dimensional ceramic skeleton is completely filled with P(VDF-TrFE-CFE) to obtain a composite material.

[0051] S5: The obtained composite material was dried at 50° C. for 10 h to remove excess solvent, and then the material was converted into a dense body by hot pressing at 0.5 MPa and 120° C. for 15 min to obtain a temperature regulating layer.

[0052] S6: Put polyethylene powder and NMP in a mass ratio of 1:10 into a glass container and stir them at 50°C for 6 hours to obtain a polymer solution; pour the polymer solution into a PTFE template and put it into an oven for drying at a temperature of 50°C for 8 hours to obtain a diaphragm substrate.

[0053] S7: Place the temperature control layer material on one side of the diaphragm substrate and perform hot pressing at a pressure of 0.5 MPa, a temperature of 110°C, and a time of 5 hours; finally, the obtained polymer composite diaphragm is annealed in a vacuum oven at 106°C for 10 hours to improve the crystallinity of the membrane, and a temperature-controlling polymer composite diaphragm is obtained with a thickness of 48 μm, wherein the thickness ratio of the diaphragm substrate to the temperature control layer is 13:1.

[0054] Example 3 A temperature-controlled polymer composite membrane was prepared by the following steps:

[0055] S1: Pb 0.97 La 0.02 Zr 0.91 Sn 0.05 TiO4 material is prepared from PbO, La2O3, TiO2, ZrO2 and SnO2 with a purity greater than 99.0%, and the above raw materials are weighed according to the stoichiometric ratio; 10 mL of ethanol, 7 mL of acetylacetone and 10 mL of glacial acetic acid are mixed to obtain a co-solvent, and then the above raw materials are dissolved in the co-solvent in turn and stirred to form a uniform solution, wherein the mass ratio of the raw materials of the three-dimensional ceramic skeleton to the co-solvent is 1:20, thereby obtaining a PLZST sol.

[0056] S2: The polyurethane foam template (TX704, ITW Texwipe) was soaked in the PLZST sol for 10 min. Then the excess sol was squeezed out of the polyurethane foam template and dried at 45 °C to obtain the PLZST precursor template. Finally, the PLZST precursor template was sintered at 1100 °C for 2 h to obtain a three-dimensional ceramic skeleton.

[0057] S3: P(VDF-TrFE-CFE) (62.1 / 30.1 / 7.8 mol%, Piezotech, France) was dissolved in DMF and stirred for 10 h to obtain a uniform P(VDF-TrFE-CFE) solution with a concentration of 26 wt%.

[0058] S4: Place the three-dimensional ceramic skeleton on a PTFE mold with a length, width and height of 40x40x20 mm; then fill the three-dimensional ceramic skeleton with the P(VDF-TrFE-CFE) solution obtained in S3, and then heat it in an oven at 60°C for 0.5 h. Repeat the above filling-heating process several times until the three-dimensional ceramic skeleton is completely filled with the polymer matrix to obtain a composite material.

[0059] S5: The obtained composite material was dried at 50° C. for 10 h to remove excess solvent, and then the material was converted into a dense body by hot pressing at 0.5 MPa and 120° C. for 15 min to obtain a temperature regulating layer.

[0060] S6: Put polyethylene powder and NMP in a mass ratio of 1:15 into a glass container and stir them at 50°C for 6 hours to obtain a polymer solution; pour the polymer solution into a PTFE template and put it into an oven for drying at 50°C for 8 hours to obtain a diaphragm substrate.

[0061] S7: Place the temperature control layer material on one side of the diaphragm substrate and perform hot pressing at a pressure of 0.5 MPa, a temperature of 110°C, and a time of 5 hours; finally, the obtained polymer composite diaphragm is annealed in a vacuum oven at 106°C for 10 hours to improve the crystallinity of the membrane, and a temperature-controlling polymer composite diaphragm is obtained with a thickness of 42 μm, wherein the thickness ratio of the diaphragm substrate to the temperature control layer is 11:1.

[0062] Example 4 A temperature-controlled polymer composite diaphragm was prepared by the following steps:

[0063] S1: Pb 0.97 La 0.02 Zr 0.91 Sn 0.05 TiO4 material is prepared from PbO, La2O3, TiO2, ZrO2 and SnO2 with a purity greater than 99.0%, and the above raw materials are weighed according to the stoichiometric ratio; 10 mL of ethanol, 3 mL of acetylacetone and 10 mL of glacial acetic acid are mixed to obtain a co-solvent, and then the above raw materials are dissolved in the co-solvent in turn and stirred to form a uniform solution, wherein the mass ratio of the raw materials of the three-dimensional ceramic skeleton to the co-solvent is 1:30, thereby obtaining a PLZST sol.

[0064] S2: The polyurethane foam template (TX704, ITW Texwipe) was soaked in the PLZST sol for 10 min; then the excess sol was squeezed out from the polyurethane foam template and dried at 45 °C to obtain the PLZST precursor template; finally, the PLZST precursor template was sintered at 1100 °C for 2 h to obtain a three-dimensional ceramic skeleton.

[0065] S3: P(VDF-TrFE-CFE) (62.1 / 30.1 / 7.8 mol%, Piezotech, France) was dissolved in DMF and stirred for 10 h to obtain a uniform P(VDF-TrFE-CFE) solution with a concentration of 30 wt%.

[0066] S4: The three-dimensional ceramic skeleton is placed on a PTFE mold with a length, width and height of 40x40x20 mm, and then the P(VDF-TrFE-CFE) solution obtained in S3 is filled into the three-dimensional ceramic skeleton, and then placed in an oven at 60°C for 0.5 h. The above filling-heating process is repeated several times until the three-dimensional ceramic skeleton is completely filled with P(VDF-TrFE-CFE) to obtain a composite material.

[0067] S5: The obtained composite material was dried at 50° C. for 10 h to remove excess solvent, and then the material was converted into a dense body by hot pressing at 0.5 MPa and 110° C. for 15 min to obtain a temperature regulating layer.

[0068] S6: Put polyethylene powder and NMP in a mass ratio of 1:8 into a glass container and stir them at 50°C for 6 hours to obtain a polymer solution; pour the polymer solution into a PTFE template and put it into an oven for drying at a drying temperature of 50°C for 8 hours to obtain a diaphragm substrate.

[0069] S7: Place the temperature regulating layer on one side of the diaphragm substrate and perform hot pressing at a pressure of 0.5 MPa, a temperature of 110°C, and a time of 5 hours; finally, the obtained polymer composite diaphragm is annealed in a vacuum oven at 106°C for 10 hours to improve the crystallinity of the membrane, and a temperature-controlled polymer composite diaphragm is obtained with a thickness of 52 μm, wherein the thickness ratio of the diaphragm substrate to the temperature regulating layer is 16:1.

[0070] Example 5 A temperature-controlled polymer composite membrane was prepared by the following steps:

[0071] S1: Pb 0.97 La 0.02 Zr 0.91 Sn 0.05 TiO4 material is prepared from PbO, La2O3, TiO2, ZrO2 and SnO2 with a purity greater than 99.0%, and the above raw materials are weighed according to the stoichiometric ratio; 6 mL of ethanol, 3 mL of acetylacetone and 10 mL of glacial acetic acid are mixed to obtain a co-solvent, and then the above raw materials are dissolved in the co-solvent in turn and stirred to form a uniform solution, wherein the mass ratio of the raw materials of the three-dimensional ceramic skeleton to the co-solvent is 1:22, thereby obtaining a PLZST sol.

[0072] S2: The polyurethane foam template (TX704, ITW Texwipe) was soaked in the PLZST sol for 10 min; then the excess sol was squeezed out from the polyurethane foam template and dried at 45 °C to obtain the PLZST precursor template; finally, the PLZST precursor template was sintered at 1100 °C for 2 h to obtain a three-dimensional ceramic skeleton.

[0073] S3: P(VDF-TrFE-CFE) (62.1 / 30.1 / 7.8 mol%, Piezotech, France) was dissolved in DMF and stirred for 10 h to obtain a uniform P(VDF-TrFE-CFE) solution with a concentration of 24 wt%.

[0074] S4: The three-dimensional ceramic skeleton is placed on a PTFE mold with a length, width and height of 40x40x20 mm, and then the P(VDF-TrFE-CFE) solution obtained in S3 is filled into the three-dimensional ceramic skeleton, and then placed in an oven at 60°C for 0.5 h. The above filling-heating process is repeated several times until the three-dimensional ceramic skeleton is completely filled with P(VDF-TrFE-CFE) to obtain a composite material.

[0075] S5: The obtained composite material was dried at 50° C. for 10 h to remove excess solvent, and then the material was converted into a dense body by hot pressing at 0.5 MPa and 110° C. for 15 min to obtain a temperature regulating layer.

[0076] S6: Put polyethylene powder and NMP in a mass ratio of 1:13 into a glass container and stir them at 50°C for 6 hours to obtain a polymer solution; pour the polymer solution into a PTFE template and put it into an oven for drying at a temperature of 50°C for 8 hours to obtain a diaphragm substrate.

[0077] S7: Place the temperature control layer on one side of the diaphragm substrate and perform hot pressing at a pressure of 0.5 MPa, a temperature of 110°C, and a time of 5 hours; finally, the obtained polymer composite diaphragm is annealed in a vacuum oven at 106°C for 10 hours to improve the crystallinity of the membrane, and a temperature-controlled polymer composite diaphragm is obtained with a thickness of 41 μm, wherein the thickness ratio of the diaphragm substrate to the temperature control layer is 12.5:1.

[0078] Example 6 The temperature-controlled polymer composite membrane was prepared by the following steps:

[0079] S1: Pb 0.97 La 0.02 Zr 0.91 Sn 0.05 TiO4 material is prepared from PbO, La2O3, TiO2, ZrO2 and SnO2 with a purity greater than 99.0%, and the above raw materials are weighed according to the stoichiometric ratio; 6 mL of ethanol, 3 mL of acetylacetone and 10 mL of glacial acetic acid are mixed to obtain a co-solvent, and then the above raw materials are dissolved in the co-solvent in turn and stirred to form a uniform solution, wherein the mass ratio of the raw materials of the three-dimensional ceramic skeleton to the co-solvent is 1:18, thereby obtaining a PLZST sol.

[0080] S2: The polyurethane foam template (TX704, ITW Texwipe) was soaked in the PLZST sol for 10 min; then the excess sol was squeezed out from the polyurethane foam template and dried at 45 °C to obtain the PLZST precursor template; finally, the PLZST precursor template was sintered at 1100 °C for 2 h to obtain a three-dimensional ceramic skeleton.

[0081] S3: P(VDF-TrFE-CFE) (62.1 / 30.1 / 7.8 mol%, Piezotech, France) was dissolved in DMF and stirred for 10 h to obtain a uniform P(VDF-TrFE-CFE) solution with a concentration of 32 wt%.

[0082] S4: The three-dimensional ceramic skeleton is placed on a PTFE mold with a length, width and height of 40x40x20 mm, and then the P(VDF-TrFE-CFE) solution obtained in S3 is filled into the three-dimensional ceramic skeleton, and then placed in an oven at 60°C for 0.5 h. The above filling-heating process is repeated several times until the three-dimensional ceramic skeleton is completely filled with P(VDF-TrFE-CFE) to obtain a composite material.

[0083] S5: The obtained composite material was dried at 50° C. for 10 h to remove excess solvent, and then the material was converted into a dense body by hot pressing at 0.5 MPa and 110° C. for 15 min to obtain a temperature regulating layer.

[0084] S6: Put polyethylene powder and NMP in a mass ratio of 1:11 into a glass container and stir them at 50°C for 6 hours to obtain a polymer solution; pour the polymer solution into a PTFE template and put it into an oven for drying at a temperature of 50°C for 8 hours to obtain a diaphragm substrate.

[0085] S7: Place the temperature control layer on one side of the diaphragm substrate and perform hot pressing at a pressure of 0.5 MPa, a temperature of 110°C, and a time of 5 hours; finally, the obtained polymer composite diaphragm is annealed in a vacuum oven at 106°C for 10 hours to improve the crystallinity of the membrane, and a temperature-controlled polymer composite diaphragm is obtained with a thickness of 55 μm, wherein the thickness ratio of the diaphragm substrate to the temperature control layer is 18:3.

[0086] Comparative Example 1

[0087] The difference between this comparative example and Example 1 is that the concentration of the P(VDF-TrFE-CFE) solution is 2wt%, and the remaining steps are the same as Example 1; the thickness of the diaphragm obtained in this comparative example is 38μm, wherein the thickness ratio of the diaphragm substrate to the temperature regulating layer is 40:1.

[0088] Comparative Example 2

[0089] The difference between this comparative example and Example 1 is that the concentration of the P(VDF-TrFE-CFE) solution is 50wt%, and the remaining steps are the same as Example 1; the thickness of the diaphragm obtained in this comparative example is 200μm, wherein the thickness ratio of the diaphragm substrate to the temperature regulating layer is 2:3.

[0090] Comparative Example 3

[0091] A conventional polymer diaphragm was prepared by hot pressing without a temperature control layer; specifically, polyethylene powder and NMP were charged into a glass container at a mass ratio of 1:20 and stirred at 50°C for 6 hours, followed by hot pressing at a pressure of 0.5 MPa, a temperature of 110°C, and a time of 5 hours to obtain a conventional polymer diaphragm with a thickness of 40 μm.

[0092] Comparative Example 4

[0093] The polymer membrane of this embodiment is a commercially available polyolefin membrane.

[0094] Test Example 1: Diaphragm ion conductivity and battery temperature test

[0095] 1) The diaphragms of Example 1 and Comparative Examples 1 to 4 were respectively assembled with stainless steel sheets into symmetrical cells, and the ionic conductivity of the diaphragms was tested at a voltage of 5 mV and a frequency of 0.01 Hz to 1 MHz;

[0096] 2) The separators of Example 1 and Comparative Examples 1 to 4 were respectively used with the LFP positive electrode and the graphite negative electrode to assemble into full batteries, and the batteries were set to perform constant current charge and discharge at 0.1C at room temperature, with a charge and discharge voltage range of 2.5V to 3.8V, and the battery temperature was tested; at the same time, the batteries were also placed in a 130°C incubator, set to perform constant current charge at 0.1C, with a charge and discharge voltage range of 2.5V to 3.8V, and the battery temperature was tested.

[0097] Table 1 Performance study results of Example 1 and its comparative example

[0098]

[0099]

[0100] It can be seen from Example 1 and Comparative Examples 1 to 4 that Example 1 has good ionic conductivity of 8.88 mS / cm, Comparative Example 1 is 1.65 mS / cm, Comparative Example 2 is 0.12 mS / cm, Comparative Example 3 is 0.15 mS / cm, and Comparative Example 4 is 0.58 mS / cm; it can be seen that the composite diaphragm modified by the negative charge card material layer has good ionic conductivity, and during the charging and discharging process, it can reduce the temperature of the battery, keep the battery temperature near room temperature, and prevent the battery temperature from further increasing. When the battery is in the charging process, due to external factors, such as the phenomenon of the ambient temperature rising due to fire, which is higher than the melting point temperature of the conventional polyolefin membrane of 130°C, the temperature-controlling polymer composite membrane of the present invention can absorb the ambient temperature, reduce the temperature of the battery, and effectively avoid the occurrence of thermal runaway of the battery; as shown in the battery temperature in the rightmost column of Table 1, when the battery is charging and discharging, the ambient temperature is higher than 130°C. At this time, the temperature of the battery in Example 1 can still be maintained at 50°C, with a very good temperature control effect, while the battery temperature of the comparative example has long been higher than the ambient temperature, which will further cause the battery to explode.

[0101] Test Example 2

[0102] Test ①: The temperature-controlled polymer composite diaphragms prepared in Example 2 and Comparative Example 4 were cut into 19 mm discs, assembled with the positive electrode material lithium iron phosphate into half-cells for electrical performance testing, and cycled 300 times at 2C rate at room temperature;

[0103] The temperature-controlled composite diaphragm prepared in Example 3 was cut into 19 mm discs and assembled with graphite into a half-cell for electrical performance testing. The half-cell was cycled 150 times at room temperature at a rate of 4C.

[0104] The results are shown in Table 2.

[0105] Table 2 Charge and discharge test results of the half-cell assembled with the diaphragms of Examples 2 to 3

[0106] Example magnification Capacity retention rate Discharge specific capacity (mAh / g) Example 2 2C 99.9% 155 Example 3 4C No obvious attenuation No obvious attenuation Comparative Example 4 2C 95.6% 132

[0107] As shown in Table 2, the half-cell assembled in Example 2 is charged and discharged at a rate of 2C, with a good capacity retention rate of 99.9% and a discharge specific capacity of 155 mAh / g. The graphite half-cell in Example 3 is charged and discharged at a rate of 4C without obvious attenuation, indicating that the diaphragm has good electrical properties. After the 2C charge and discharge test, the half-cell assembled from the commercial polyolefin diaphragm of Comparative Example 4 was found to have lower capacity retention rate and discharge specific capacity than that of Example 2, proving that the temperature-controlled polymer composite diaphragm of the present invention has good electrical properties.

[0108] Test ②: The temperature-controlling polymer composite diaphragm prepared in Example 4 was cut into 19 mm discs and assembled with lithium sheets into a lithium-lithium symmetric battery (where the temperature-controlling layer of the diaphragm was located on the negative electrode side) for electrical performance testing. At room temperature, at 2 mA / cm 2 Cycle 4000 times.

[0109] The electrical performance test results show that the lithium-lithium symmetrical battery assembled with the temperature-controlled polymer composite diaphragm of Example 4 has a high 2 After cycling 4000 times at a current density of , the polarization voltage exhibited was 0.2V, that is, the battery still exhibited a small polarization voltage after 4000 cycles, indicating that the battery has a strong ability to inhibit lithium dendrites; while with the conventional polyolefin separator, the migration of lithium ions is affected by internal impurities during charging and discharging, and the migration speed is slow, which is more likely to block the pores of the separator, causing the internal resistance of the battery to increase. Lithium loss and increased internal resistance will cause the battery capacity to plummet, and the number of cycles will be seriously reduced, and it will not reach 4000 cycles at all.

[0110] At the same time, the results also show that when the charge and discharge are terminated and the electric field is removed, the temperature increase of the lithium-lithium symmetrical battery assembled using the temperature-controlled polymer composite diaphragm of Example 4 can reduce the internal polarization, effectively reduce the internal resistance of the battery, and increase the capacity of the battery. Taking charging as an example, conventional polyolefin separators do not have a temperature regulating function and cannot quickly eliminate the concentration polarization inside the lithium-ion battery, which ultimately results in the lithium ions not being completely embedded in the negative electrode. The lithium ions released from the positive electrode will form lithium monomers or lithium compounds, or even dead lithium, on the surface of the negative electrode, which will cause the growth of lithium dendrites, thereby causing the battery capacity to decay. The further growth of lithium dendrites may even pierce the separator, causing the positive and negative electrodes of the battery to contact, thereby causing thermal runaway. However, in the present invention, the temperature-controlling polymer composite separator with a negative electrocaloric effect can further increase the temperature after the electric field is removed, thereby promoting the rapid migration of lithium ions, reducing internal concentration polarization, and making the lithium ions almost 100% embedded in the negative electrode without staying on the surface of the negative electrode. In addition, the temperature-controlling layer with a certain rigidity facing the negative electrode is also conducive to inhibiting the formation of lithium dendrites, thereby significantly improving the battery capacity.

[0111] Test ③: The temperature-controlled polymer composite diaphragm prepared in Example 5 was cut into rectangular pieces of 25 mm x 30 mm and loaded with 20 mg / cm 2 The lithium iron phosphate and the loading is 8mg / cm 2 The electrical performance of the graphite assembled soft-pack battery was tested, and the charge and discharge test was carried out at room temperature and 1C rate.

[0112] The test results show that the battery assembled with the temperature-controlled polymer composite diaphragm of Example 5 can be charged and discharged normally, and the temperature of the battery can be maintained below 40°C; if the battery is unfortunately in a high temperature environment greater than 130°C, the battery can also be "cooled" during charging and discharging, effectively avoiding further thermal runaway of the battery.

[0113] Test ④: The temperature-controlling polymer composite diaphragm prepared in Example 6 was cut into rectangular pieces of 25 mm x 30 mm and loaded with 20 mg / cm 2 The lithium iron phosphate and the loading is 8mg / cm 2 The electrical performance of the graphite assembled soft-pack battery was tested, and the charge and discharge test was carried out at room temperature and 6C rate.

[0114] The test results show that when the battery assembled with the temperature-controlled polymer composite diaphragm of Example 6 is charged and discharged under fast charging conditions, the battery temperature can still be controlled within 35°C, which indicates that the diaphragm can be effectively used in the field of battery fast charging and has good application prospects.

Claims

1. A temperature-controlling polymer composite diaphragm, It is characterized in that It includes a diaphragm substrate and a temperature regulating layer arranged on one side or both sides thereof; The diaphragm substrate is a polymer film; The temperature regulating layer is a negative electrocaloric material layer, and the negative electrocaloric material layer is composed of a three-dimensional ceramic skeleton and a polar polymer material both having a negative electrocaloric effect.

2. The temperature-controlling polymer composite diaphragm according to claim 1, It is characterized in that The material of the three-dimensional ceramic skeleton is a relaxor ferroelectric lead zirconate titanate dopant doped with tin; The polar polymer material is at least one of poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene), poly(vinylidene fluoride-trifluoroethylene), polyurea aromatic linear dielectric polymer, perovskite relaxor ferroelectric polymer material, polyimide material, polyamide material, and polystyrene material.

3. The temperature-controlling polymer composite diaphragm according to claim 2, It is characterized in that The polar polymer material is poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene).

4. The temperature-controlling polymer composite diaphragm according to claim 3, It is characterized in that The material of the diaphragm substrate is selected from at least one of polyacrylonitrile, polyethylene, polypropylene, polyvinylidene fluoride, polyvinyl pyrrolidone, poly(m-phenylene isophthalamide) and poly(methyl methacrylate).

5. A method for preparing the temperature-controlling polymer composite diaphragm according to claims 1 to 4, It is characterized in that The following steps are involved: A three-dimensional ceramic skeleton is prepared by a sol-gel method; a polar polymer material is filled into the three-dimensional ceramic skeleton, and then hot-pressed to obtain a temperature-regulating layer; finally, the diaphragm substrate and the temperature-regulating layer are hot-pressed and composited to obtain the temperature-controlling polymer composite diaphragm.

6. The method for preparing the temperature-controlling polymer composite diaphragm according to claim 5, It is characterized in that The method for preparing a three-dimensional ceramic skeleton is as follows: the raw materials for preparing the three-dimensional ceramic skeleton are evenly mixed with a solvent to obtain a sol; a polyurethane foam template is infiltrated in the sol, and then excess sol is squeezed out of the polyurethane foam template and dried at 35 to 65° C. to obtain a precursor template; finally, the precursor template is sintered at 1000 to 1400° C. for 1 to 3 hours to obtain a three-dimensional ceramic skeleton.

7. The method for preparing the temperature-controlling polymer composite diaphragm according to claim 6, It is characterized in that The infiltration time is 15 to 20 minutes; the solvent is composed of 5 to 40 mL of ethanol, 1 to 10 mL of acetylacetone and 5 to 30 mL of glacial acetic acid; the mass ratio of the raw materials for preparing the three-dimensional ceramic skeleton to the solvent is 1:5 to 1:

50.

8. The method for preparing the temperature-controlling polymer composite diaphragm according to claim 7, It is characterized in that The method for preparing the temperature regulating layer is as follows: dissolving the polar polymer material to obtain a polar polymer material solution with a concentration of 5 to 35 wt%; then filling the polar polymer material solution into the three-dimensional ceramic skeleton prepared above, and then placing it in an oven at 40 to 80°C and heating it for 0.1 to 2 hours; repeating the above filling-heating operation several times until the three-dimensional ceramic skeleton is completely filled with the polar polymer material to obtain a composite material; drying the obtained composite material at 40 to 60°C for 8 to 12 hours, and then hot pressing at 0.1 to 1 MPa and 100 to 150°C for 10 to 25 minutes to convert the above composite material into a dense body to obtain the temperature regulating layer.

9. The method for preparing the temperature-controlling polymer composite diaphragm according to claim 8, It is characterized in that Placing a temperature control layer on one side of the diaphragm substrate and performing hot pressing to obtain a polymer composite diaphragm, wherein the hot pressing pressure is 0.5-1 MPa, the temperature is 100-200° C., and the time is 1-10 hours; finally, annealing the obtained polymer composite diaphragm in a vacuum oven at 106° C. for 10 hours to improve the crystallinity of the film, thereby obtaining the temperature control polymer composite diaphragm; The preparation method of the diaphragm substrate is as follows: a polymer and N-methylpyrrolidone are mixed in a mass ratio of 1:10 to 1:50 to form a polymer solution; the obtained polymer solution is poured into a template, and placed in an oven for drying at 40 to 60° C. for 6 to 12 hours to obtain a diaphragm substrate.

10. Use of the temperature-controlling polymer composite diaphragm according to claims 1 to 4 in lithium-ion batteries.

Citation Information

Patent Citations

  • Lithium ion secondary battery

    CN110419127A

  • Lithium battery composite diaphragm as well as preparation method and application thereof

    CN114883747A

  • Secondary battery and electric device

    CN115911757A

  • Foamed ceramic loaded perovskite composite material for water treatment and preparation method thereof

    CN116571233A

  • Adhesive heat-resistant diaphragm

    CN215119155U