Separator, electrochemical device, and electronic device
By embedding polymer particles into the inorganic coating in the separator of the electrochemical device and optimizing the structure of the inorganic coating and the bonding layer, the problem of poor kinetic performance of the existing separator under low temperature conditions is solved, and the electrical power is achieved Improvement of energy density and cycling performance of chemical devices.
Patent Information
- Application Number
- CN202411388090.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-22
AI Technical Summary
The separators of existing electrochemical devices have shortcomings in improving cycling performance and energy density, especially in low temperature conditions, which have poor kinetic performance and difficulty in maintaining good ion transport capabilities and bonding forces.
A separator is designed, including a substrate layer, an inorganic coating and an adhesive layer, and the polymer particles are embedded in the inorganic coating. The inorganic particles are optimized by adjusting the ratio of polymer particles to inorganic particles, the average diameter and the thickness of the bonding layer. The thickness of the coating and the selection of binder ensure that the diaphragm improves kinetics and cycling properties while maintaining good ion transport capabilities.
The energy density improvement of the electrochemical device, the kinetic performance and cycling performance improvement of the electrochemical device is achieved, especially the performance improvement under low temperature conditions, and the puncture resistance of the membrane and the transmission ability of the electrolyte are improved.
Smart Images

Figure CN119009359A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical energy storage, and in particular to a diaphragm, an electrochemical device using the diaphragm, and an electronic device using the electrochemical device. Background Art
[0002] As portable chemical energy sources, electrochemical devices (such as lithium-ion batteries) are widely used in consumer electronics (such as mobile phones, notebooks, cameras, etc.), energy storage products (such as home energy storage, energy storage power stations, UPS power supplies, etc.) and new energy vehicles due to their high energy density, high operating voltage platform, low self-discharge, long service life and environmental friendliness.
[0003] The diaphragm is an important component of the electrochemical device. The bonding force between the diaphragm and the positive and negative electrodes affects the cycle performance and energy density of the electrochemical device. Therefore, it is necessary to develop a diaphragm that can improve the cycle performance and energy density of the electrochemical device. Summary of the invention
[0004] The present application provides a diaphragm, an electrochemical device and an electronic device.
[0005] The first aspect of the present application provides a diaphragm, comprising a substrate layer, an inorganic coating and a bonding layer, wherein the inorganic coating is disposed between the substrate layer and the bonding layer, the inorganic coating comprises inorganic particles, the bonding layer comprises polymer particles, at least some of the polymer particles are embedded in the pores of the inorganic coating, and in a 2000x scanning electron microscope photograph of a cross section of the diaphragm, within an area of 11.6μm×7.6μm, the number of polymer particles embedded in the inorganic coating to a depth greater than or equal to 100nm is C, the total number of polymer particles in the cross section is D, and 0.5≤C / D<0.94.
[0006] In the diaphragm provided by the present application, part of the polymer is embedded in the inorganic coating, which reduces the thickness of the bonding layer and the inorganic coating on the surface of the substrate layer, and reduces the thickness of the entire diaphragm, thereby facilitating the improvement of the energy density of the electrochemical device. The applicant has found that when the number of polymer particles embedded in the inorganic coating is within a suitable range, the diaphragm maintains good ion transmission capability while also enabling the electrochemical device to have good kinetic performance, low temperature performance, and cycle performance.
[0007] More preferably, 0.71≤C / D<0.94 is satisfied, which can more effectively provide the diaphragm with good ion transmission ability, and further make the electrochemical device have better kinetic performance, low temperature performance and cycle performance.
[0008] Based on the first aspect, in some embodiments, the average diameter L of the polymer particles and the particle size Dv50 of the inorganic particles satisfy: 0.4≤L / Dv50≤0.8. This is beneficial to increase the embedding depth of the polymer particles into the inorganic coating and the number of polymer particles embedded in the inorganic coating, so that the polymer particles and the inorganic particles maintain good contact, improve the ion transport capacity of the separator in the electrochemical device, and further help the electrochemical device have good cycle performance, kinetic performance and low temperature performance.
[0009] Based on the first aspect, in some embodiments, the thickness of the inorganic coating is 0.5 μm to 5 μm, which is conducive to the embedding of polymer particles, and makes the separator have good energy density and good puncture resistance, and the separator also maintains good storage capacity and wettability for the electrolyte, which is conducive to improving the transmission of the electrolyte, thereby improving the cycle performance and low temperature performance of the electrochemical device.
[0010] Based on the first aspect, in some embodiments, the thickness of the inorganic coating is d 1 μm, C = 7.6d 1 + 7.4. The thickness of the inorganic coating and the number of polymer particles embedded in the inorganic coating satisfy the above relationship, which is more conducive to increasing the number of polymer particles embedded in the inorganic coating, and can further improve the ion transport capacity of the separator in the electrochemical device, thereby facilitating the improvement of the cycle performance, low temperature performance and kinetic performance of the electrochemical device.
[0011] Based on the first aspect, in some embodiments, the average diameter L of the polymer particles is 0.3 μm to 5 μm, which is conducive to a certain amount of polymer particles being embedded in the inorganic coating, improving the bonding force between the polymer particles and the inorganic coating and the interface bonding force between the polymer particles and the positive and negative electrodes, thereby improving the cycle performance of the electrochemical device.
[0012] Based on the first aspect, in some embodiments, the particle size Dv50 of the inorganic particles in the inorganic coating is 0.4 μm to 6.5 μm, and Dv90 is 0.8 μm to 8.7 μm. This is beneficial for embedding the polymer particles in the inorganic coating, and is also beneficial for improving the mechanical strength of the separator and improving the heat shrinkage resistance of the separator, thereby improving the cycle performance of the electrochemical device.
[0013] Based on the first aspect, in some embodiments, the thickness of the adhesive layer is 0.5 μm to 2 μm, which can improve the infiltration of the electrolyte along the thickness direction and the horizontal direction of the adhesive layer while maintaining a good energy density of the electrochemical device, thereby improving the dynamic performance of the electrochemical device. The coating weight per unit area of the adhesive layer is 0.5 mg / 5000 mm 2 Up to 3mg / 5000mm 2While maintaining good bonding between the bonding layer and the positive and negative electrode sheets and between the bonding layer and the inorganic coating, it also facilitates the infiltration of the electrolyte and improves the transmission of the electrolyte, thereby improving the kinetic performance and cycle performance of the electrochemical device.
[0014] Based on the first aspect, in some embodiments, the thickness of the substrate layer is d2, satisfying: 0.05≤d1 / d2≤1. The thickness of the inorganic coating and the thickness of the separator satisfy the above relationship, which not only allows the polymer particles to be embedded in the inorganic coating, but also helps the electrochemical device maintain a good energy density.
[0015] In some embodiments, the inorganic particles include at least one of aluminum oxide, aluminum oxide, silicon dioxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zirconium oxide, zinc oxide, calcium oxide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The above-mentioned inorganic particles can improve the mechanical strength of the diaphragm, and at the same time, it is also beneficial to improve the wetting effect of the diaphragm on the electrolyte and improve the cycle performance of the electrochemical device. The inorganic coating also includes a binder, and the binder includes at least one of acrylic acid, methyl methacrylate, butyl acrylate, octyl acrylate, isooctyl acrylate, butadiene or acrylonitrile. The above-mentioned binder is beneficial to improve the bonding force between the inorganic particles in the inorganic coating and the bonding force between the inorganic coating and the substrate layer, and is beneficial to improve the interface bonding force between the inorganic coating and the substrate layer, which is beneficial to lithium ion transmission and improves the cycle performance of the electrochemical device.
[0016] Based on the mass of the inorganic coating, the mass percentage of the inorganic particles is 85% to 95%. When the mass percentage of the inorganic particles is within the above range, the electrochemical device can have good kinetics and improve the thermal safety of the electrochemical device.
[0017] Based on the first aspect, in some embodiments, the polymer particles in the bonding layer are selected from the following at least two monomers: butadiene, methyl acrylate, methyl methacrylate, styrene, butyl methacrylate, isooctyl acrylate, ethylene, propylene or vinylidene fluoride. The polymer particles formed by the polymerization of the above monomers have good bonding force and wetting ability, and provide a certain bonding force for the bonding layer. In some embodiments, the polymer particles also include at least one of acrylic acid, acrylonitrile or butadiene. The addition of the above substances can further improve the bonding force between the bonding layer and the inorganic coating, so that the bonding layer has good bonding force and wetting ability, which is conducive to improving the kinetic performance of the electrochemical device.
[0018] Based on the first aspect, in some embodiments, the porosity of the separator is 30% to 50%, which can improve the liquid retention capacity of the separator, reduce the transmission impedance of lithium ions, and improve the transmission capacity of lithium ions, thereby improving the cycle performance of the electrochemical device.
[0019] Based on the first aspect, in some embodiments, under a scanning electron microscope of the diaphragm at a magnification of 10,000 times, within an area of 11.6 μm×7.6 μm, the surface of each polymer particle has a plurality of protrusions, and the number of protrusions is 5 to 50. The protrusions on the surface of the bonding layer can be formed by the monomers of some polymers being polymerized, swelling in the electrolyte and protruding from the surface. The applicant found that when the protrusions on the surface of the bonding layer meet the appropriate number in the above-mentioned area, the first aspect increases the contact sites between the polymer particles and the positive and negative electrode sheets, and increases the bonding force between the polymer particles and the positive and negative electrode sheets; secondly, when the diaphragm is applied to an electrochemical device, the above-mentioned protrusions are also more conducive to being embedded in the active material layer of the positive electrode sheet or the negative electrode sheet, further improving the bonding force between the separator and the positive electrode sheet or the negative electrode sheet, thereby facilitating the improvement of the cycle performance and energy density of the electrochemical device; thirdly, the protrusions in the above-mentioned polymer particles are also more conducive to improving the electrolyte retention capacity, improving the conduction of lithium ions, and improving the cycle performance and kinetic performance of the electrochemical device.
[0020] Based on the first aspect, in some embodiments, the diaphragm includes two bonding layers, one bonding layer is located on the surface of the inorganic coating layer away from the substrate layer, and the other bonding layer is located on the surface of the substrate layer away from the inorganic coating layer. The bonding layer containing the inorganic coating layer is close to the positive electrode sheet, and the inorganic coating layer can prevent the damage to the diaphragm caused by crystallization on the positive electrode sheet, thereby improving the safety of the electrochemical device. The bonding layers are included on both sides of the diaphragm, which is conducive to improving the bonding force between the diaphragm and the positive electrode sheet and the negative electrode sheet, reducing the possibility of deformation of the electrochemical device during the cycle, and also helping to improve the ion transmission capacity of the diaphragm and improve the cycle performance of the electrochemical device.
[0021] The second aspect of the present application also provides an electrochemical device, wherein the electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is located between the positive electrode sheet and the negative electrode sheet. The electrochemical device includes the above-mentioned separator, and the number of polymer particles embedded in the inorganic coating in the separator meets appropriate conditions, which can improve the energy density and cycle performance of the electrochemical device.
[0022] A third aspect of the present application provides an electronic device, which includes an electrochemical device. The electrochemical device has good energy density and cycle performance, and can further improve the service life of the electronic device. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0024] Figure 1 This is a scanning electron microscope image of the cross section of the diaphragm provided in Example 1 of the present application at a magnification of 2000.
[0025] Figure 2 for Figure 1 Scanning electron microscopy of a cross section of a diaphragm at 10,000x magnification.
[0026] Figure 3 This is a scanning electron microscope image of the surface of the diaphragm prepared in Example 1. DETAILED DESCRIPTION
[0027] The technical scheme in the embodiment of the present application is described clearly and in detail below. Obviously, the described embodiment is a part of the embodiment of the present application, rather than all the embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present application. The terms used in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application.
[0028] As used herein, amounts, ratios and other numerical values are sometimes presented herein in a range format. It should be understood that such a range format is used for convenience and brevity, and should be flexibly construed to include not only the values explicitly specified as range limits, but also all individual values or sub-ranges encompassed within the range, as if each value and sub-range were explicitly specified.
[0029] The present application provides a diaphragm, comprising a substrate layer, an inorganic coating and a bonding layer, wherein the inorganic coating is disposed between the substrate layer and the bonding layer, the inorganic coating comprises inorganic particles, the bonding layer comprises polymer particles, at least some of the polymer particles are embedded in the pores of the inorganic coating, and in a scanning electron microscope photograph of a cross section of the diaphragm at a magnification of 2000 times, within an area of 11.6 μm×7.6 μm, the number of polymer particles embedded in the inorganic coating to a depth greater than or equal to 100 nm is C, the total number of polymer particles in the cross section is D, and 0.5≤C / D<0.94.
[0030] In the diaphragm provided by the present application, part of the polymer is embedded in the inorganic coating, which reduces the thickness of the bonding layer and the inorganic coating on the surface of the substrate layer, and reduces the thickness of the entire diaphragm, thereby facilitating the improvement of the energy density of the electrochemical device. The applicant has found that when the proportion of the number of polymer particles embedded in the inorganic coating is within an appropriate range, the diaphragm maintains good ion transmission capacity, thereby also enabling the electrochemical device to have good kinetic performance, low temperature performance and cycle performance.
[0031] In some embodiments, 0.71≤C / D<0.94. The kinetic performance, low temperature performance and cycle performance of the electrochemical device can be better improved.
[0032] In some embodiments, 0.6≤C / D≤0.8, which can further improve the kinetic performance, low temperature performance and cycle performance of the electrochemical device.
[0033] See also Figure 1 and Figure 2 ,exist Figure 2 Along the thickness direction of the substrate layer, according to the different colors and shapes in the figure, from top to bottom, it can be divided into a bonding layer, a substrate layer, an inorganic coating layer and a bonding layer, and both sides of the substrate layer are provided with bonding layers. Figure 2 The inorganic coating is formed by square-shaped particles, the polymer particles in the bonding layer are spherical in structure, and some of the polymer particles are embedded in the pores of the inorganic coating.
[0034] In some embodiments, the ratio of C / D can be 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.94 or any value within the range formed by any two of the above values.
[0035] If the C / D ratio is less than 0.5, the number of polymer particles embedded in the inorganic coating is small, and most of the polymer particles are bonded to the surface of the inorganic coating, which reduces the ion transmission capacity and is not conducive to improving the kinetic performance, low temperature performance and cycle performance of the electrochemical device.
[0036] In some embodiments, the average diameter L of the polymer particles and the particle size Dv 50 of the inorganic particles satisfy: 0.4≤L / Dv 50≤0.8. The average diameter of the polymer particles and the particle size of the inorganic particles satisfy the above conditions, which is conducive to increasing the embedding depth of the polymer particles embedded in the inorganic coating and the number of polymer particles embedded in the inorganic coating, so that the polymer particles can be fully embedded in the pores of the inorganic coating, such as between multiple adjacent inorganic particles, so that the polymer particles and the inorganic particles maintain good contact, improve the ion transmission capacity of the diaphragm in the electrochemical device, and further help the electrochemical device have good kinetic performance, low temperature performance and cycle performance.
[0037] If the ratio of L / Dv 50 is small, such as less than 0.4, the particle size Dv50 of the inorganic particles is large or the average diameter L of the polymer particles is small, the polymer particles may be completely embedded in the gaps between the inorganic particles, which may reduce the bonding force between the inorganic coating and the bonding layer, affect the interface stability between the diaphragm and the positive and negative electrodes in the electrochemical device, and affect the cycle performance of the electrochemical device. If the ratio of L / Dv 50 is large, such as greater than 0.8, the average diameter L of the polymer particles is close to the particle size Dv50 of the inorganic particles, which is not conducive to the embedding of the polymer particles in the pores of the inorganic coating, and is not conducive to improving the ion transmission capacity of the diaphragm in the electrochemical device, thereby improving the kinetic performance, low temperature performance and cycle performance of the electrochemical device. In some embodiments, the ratio of L / Dv50 can be 0.4, 0.5, 0.6, 0.7, 0.8 or any value within the range composed of any two of the above values.
[0038] Among them, D V 50 is also called the "median diameter", which means the particle diameter at which the volume of the inorganic particles is 50% measured from the smallest particle diameter in the volume-based particle size distribution.
[0039] In some embodiments, the thickness of the inorganic coating is 0.5 μm to 5 μm. The thickness of the inorganic coating is within the above range, which is conducive to the embedding of polymer particles, and enables the diaphragm to have good energy density while also having good puncture resistance, and the diaphragm also maintains good storage capacity and wettability for the electrolyte, which is conducive to improving the transmission of the electrolyte, thereby facilitating the improvement of the cycle performance and low temperature performance of the electrochemical device. And the thickness of the above-mentioned inorganic coating is within the above range, which is also conducive to reducing the self-discharge rate of the electrochemical device and improving the stability of the electrochemical device. In some embodiments, the thickness of the inorganic coating can be 0.5 μm, 0.8 μm, 1 μm, 1.5 μm, 1.8 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm or any value within the range composed of any two of the above values.
[0040] In some embodiments, the thickness of the inorganic coating is d 1 μm, C = 7.6d 1 + 7.4. The thickness of the inorganic coating and the number of polymer particles embedded in the inorganic coating satisfy the above relationship, which is more conducive to increasing the number of polymer particles embedded in the inorganic coating, and can further improve the ion transport capacity of the separator in the electrochemical device, thereby helping to improve the cycle performance, low temperature performance and kinetic performance of the electrochemical device.
[0041] In some embodiments, the average diameter L of the polymer particles is 0.3 μm to 5 μm. The average diameter L of the polymer is within the above range, which is conducive to a certain amount of polymer particles being embedded in the inorganic coating, improving the bonding force between the polymer particles and the inorganic coating and the interfacial bonding force between the polymer particles and the positive and negative electrodes, thereby facilitating the improvement of the cycle performance of the electrochemical device. If the average diameter L of the polymer particles is small, such as less than 0.3 μm, the number of polymer particles is large, which will slow down the transmission of the electrolyte on the surface of the bonding layer and reduce the cycle performance of the electrochemical device. If the average diameter L of the polymer particles is large, such as greater than 5 μm, the number of polymer particles embedded in the inorganic coating will be reduced, reducing the ion transmission capacity of the diaphragm in the electrochemical device, thereby reducing the cycle performance and kinetic performance of the electrochemical device. In some embodiments, the average diameter L of the polymer particles is 0.3 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm or any value within the range composed of any two of the above values.
[0042] In some embodiments, the particle size Dv50 of the inorganic particles in the inorganic coating is 0.4 μm to 7 μm, and Dv90 is 0.8 μm to 9 μm. The particle sizes Dv50 and Dv90 of the inorganic particles meet the above ranges, which is conducive to embedding the polymer particles in the inorganic coating, and is also conducive to improving the mechanical strength of the diaphragm and improving the heat shrinkage resistance of the diaphragm, thereby improving the cycle performance of the electrochemical device. The particle size Dv50 of the inorganic particles can be 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm or any value within the range composed of any two of the above values. The particle size Dv90 of the inorganic particles can be 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2.3 μm, 2.7 μm, 3.2 μm, 3.7 μm, 4 μm, 4.2 μm, 4.5 μm, 4.8 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm or any value within the range formed by any two of the above values. V 90 indicates the particle size at which 90% of the volume accumulation is achieved from the smallest particle size in the volume-based particle size distribution of the inorganic particles.
[0043] In some embodiments, the particle size Dv10 of the inorganic particles in the inorganic coating is 0.2 μm to 0.6 μm. In some embodiments, the particle size Dv10 of the inorganic particles can be 0.2 μm, 0.3 μm, 0.4 μm, 0.4 μm, 0.6 μm or any value within the range formed by any two of the above values.
[0044] In some embodiments, the thickness of the bonding layer is 0.5 μm to 2 μm. When the thickness of the bonding layer is within the above-mentioned suitable range, the electrolyte can be improved in the thickness direction and the horizontal direction of the bonding layer while maintaining a good energy density of the electrochemical device, which is beneficial to improving the kinetic performance of the electrochemical device. In some embodiments, the thickness of the bonding layer can be 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2 μm, or any value within the range formed by any two of the above values.
[0045] The coating weight per unit area of the adhesive layer is 0.5 mg / 5000 mm 2 Up to 3mg / 5000mm 2 The coating weight per unit area of the adhesive layer is within the above range. While maintaining good adhesion between the adhesive layer and the positive and negative electrode sheets and between the adhesive layer and the inorganic coating, it is also conducive to the infiltration of the electrolyte and improves the transmission of the electrolyte, thereby improving the kinetic performance and cycle performance of the electrochemical device. In some embodiments, the coating weight per unit area of the adhesive layer is 0.5 mg / 5000 mm 2 , 1mg / 5000mm 2 , 1.5mg / 5000mm 2 , 2mg / 5000mm 2 , 2.5mg / 5000mm 2 、3mg / 5000mm 2 Or any value within the range formed by any two of the above values.
[0046] In some embodiments, the thickness of the substrate layer is d2, and the separator satisfies: 0.05≤d1 / d2≤1.0. The thickness of the inorganic coating layer and the thickness of the substrate layer satisfy the above relationship, which not only satisfies the embedding of polymer particles in the inorganic coating layer, but also helps the electrochemical device maintain a good energy density. In some embodiments, the ratio of d1 / d2 can be 0.05, 0.1, 0.2, 0.3, 0.5, 0.8, 0.9, 1 or any value within the range of any two of the above values.
[0047] In some embodiments, the inorganic particles include at least one of aluminum oxide, aluminum oxide, silicon dioxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zirconium oxide, zinc oxide, calcium oxide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The above inorganic particles can improve the mechanical strength of the diaphragm, and are also conducive to improving the wetting effect of the diaphragm on the electrolyte and improving the cycle performance of the electrochemical device.
[0048] The inorganic coating also includes a binder, which includes at least one of acrylic acid, methyl methacrylate, butyl acrylate, octyl acrylate, isooctyl acrylate, butadiene or acrylonitrile. The above-mentioned binder is beneficial to improving the bonding force between inorganic particles in the inorganic coating and the bonding force between the inorganic coating and the substrate layer, and is beneficial to improving the interfacial bonding force between the inorganic coating and the substrate layer, which is beneficial to lithium ion transmission and improves the cycle performance of the electrochemical device. Based on the mass of the inorganic coating, the mass percentage of the binder is 5% to 15%. The mass percentage of the binder is within the above range, which can make the inorganic coating and the substrate layer have good bonding force. In some embodiments, based on the mass of the inorganic coating, the mass percentage of the binder can be 5%, 7%, 8%, 9%, 10%, 12%, 13%, 14%, 15% or any value within the range composed of any two of the above values.
[0049] Based on the mass of the inorganic coating, the mass percentage of the inorganic particles is 85% to 95%. The mass percentage of the inorganic particles within the above range can improve the thermal safety of the electrochemical device on the basis of good kinetics. In some embodiments, based on the mass of the inorganic coating, the mass percentage of the inorganic particles can be 85%, 87%, 89%, 90%, 92%, 93%, 94%, 95% or any value within the range of any two of the above values.
[0050] In some embodiments, the polymer particles in the bonding layer are selected from at least two of the following monomers: butadiene, methyl acrylate, methyl methacrylate, styrene, butyl methacrylate, isooctyl acrylate, ethylene, propylene or vinylidene fluoride. The polymer particles formed by the polymerization of the above monomers have good bonding force and wetting ability, and provide a certain bonding force for the bonding layer.
[0051] In some embodiments, the polymer particles further include at least one of acrylic acid, acrylonitrile or butadiene. The addition of the above substances can further improve the bonding force between the bonding layer and the inorganic coating, so that the bonding layer has good bonding force and wetting ability, which is beneficial to improving the kinetic performance of the electrochemical device.
[0052] In some embodiments, the porosity of the diaphragm is 30% to 50%. The porosity of the diaphragm within the above range can not only improve the liquid retention capacity of the diaphragm, but also reduce the transmission impedance of lithium ions and improve the transmission capacity of lithium ions, thereby improving the cycle performance and kinetic performance of the electrochemical device. In some embodiments, the porosity of the diaphragm can be 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50% or any value within the range composed of any two of the above values. Preferably, the porosity of the diaphragm is 35% to 45%.
[0053] In some embodiments, under a scanning electron microscope of the diaphragm at a magnification of 10,000 times, the number of polymer particles in an area of 11.6 μm × 7.6 μm is 10 to 60. If the number of polymer particles is small, the bonding force between the bonding layer and the positive electrode sheet and the negative electrode sheet will be reduced. If the number of polymer particles is large, the rate performance of the electrochemical device may be reduced. In some embodiments, the number of polymer particles is 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60 or any value within the range of any two of the above values.
[0054] Each polymer particle has a plurality of protrusions on its surface. In a 10,000-fold scanning electron microscope photograph of the separator, the number of protrusions is 5 to 50 in an area of 11.6 μm×7.6 μm, as shown in FIG. Figure 3 . The protrusions on the surface of the bonding layer can be formed by the monomers of some polymers being polymerized, swelling in the electrolyte and protruding from the surface. The applicant found that when the protrusions on the surface of the bonding layer meet the appropriate number in the above-mentioned area, on the one hand, the contact sites between the polymer particles and the positive and negative electrode sheets are increased, and the bonding force between the polymer particles and the positive and negative electrode sheets is increased; on the second hand, when the diaphragm is used in an electrochemical device, the above-mentioned protrusions are also conducive to being embedded in the active material layer of the positive electrode sheet or the negative electrode sheet, further improving the bonding force between the polymer particles and the positive electrode sheet or the negative electrode sheet, thereby helping to improve the cycle performance and energy density of the electrochemical device; on the third hand, the protrusions in the above-mentioned polymer particles are also more conducive to improving the electrolyte retention capacity, helping to improve the conduction of lithium ions, and improving the cycle performance and kinetic performance of the electrochemical device. In some embodiments, within an area of 11.6 μm×7.6 μm, the number of protrusions may be 5, 8, 10, 12, 14, 16, 18, 20, 24, 28, 30, 32, 34, 38, 40, 44, 48, 50 or any value within the range formed by any two of the above values.
[0055] The number of the above-mentioned polymer particles is related to the material (monomer type) of the polymer particles, the coating weight per unit area, the particle size of the polymer particles, and the coating morphology. By adjusting at least one of the above factors, the number of polymer particles in the above region can be changed. The number of protrusions on the surface of the above-mentioned polymer particles is related to the material (monomer type) of the polymer particles, the cross-linking degree of the polymer particles, and the ratio of the core-shell structure of the polymer particles formed by the polymerization of the polymer monomers. By adjusting the above factors, the number of protrusions in the above region can be changed.
[0056] In some embodiments, the diaphragm includes two adhesive layers, one adhesive layer is located on the surface of the inorganic coating layer away from the substrate layer, and the other adhesive layer is located on the surface of the substrate layer away from the inorganic coating layer. The adhesive layer containing the inorganic coating layer is close to the positive electrode sheet, and the inorganic coating layer can prevent the damage to the diaphragm caused by crystallization on the positive electrode sheet, thereby improving the safety of the electrochemical device. The inclusion of adhesive layers on both sides of the diaphragm is conducive to improving the bonding force between the diaphragm and the positive electrode sheet and the negative electrode sheet, reducing the possibility of deformation of the electrochemical device during the cycle, and also helping to improve the ion transmission capacity of the diaphragm and improve the cycle performance of the electrochemical device.
[0057] In the present application, the number of polymer particles embedded in the inorganic coating, that is, the ratio of C / D, is adjusted by regulating the particle size Dv 50 of the inorganic particles in the inorganic coating, the thickness of the inorganic coating, the coating weight per unit area of the bonding layer, or the average diameter L of the polymer particles.
[0058] In one embodiment of the present application, an electrochemical device is also provided, including a housing, an electrode assembly, and an electrolyte, wherein the battery cell and the electrolyte are located in the housing. The housing may be a packaging bag obtained by packaging with a packaging film (such as an aluminum-plastic film), such as when the electrochemical device is a soft-pack secondary battery. In other embodiments, the electrochemical device may also be a steel shell battery, an aluminum shell battery, and the like.
[0059] The electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is located between the positive electrode sheet and the negative electrode sheet. The electrode assembly may be a laminated structure, which is formed by stacking the positive electrode sheet, the separator and the negative electrode sheet. In other embodiments, the electrode assembly may also be a wound structure, which is formed by stacking the positive electrode sheet, the separator and the negative electrode sheet and then winding them.
[0060] Positive electrode
[0061] The positive electrode plate includes a positive current collector and a positive active layer disposed on the positive current collector. The positive current collector may be aluminum foil or nickel foil, etc., or may be any composite current collector disclosed in the prior art, such as but not limited to the current collector formed by combining the aforementioned conductive foil and the polymer substrate. The positive active layer contains a positive active material, and the positive active material includes a compound that reversibly embeds and deintercalates lithium ions (i.e., a lithiated intercalation compound). In some embodiments, the positive active material may include a lithium transition metal composite oxide. The lithium transition metal composite oxide contains lithium and at least one element selected from cobalt, manganese and nickel. In some embodiments, the positive active material may include but is not limited to lithium cobaltate, lithium nickel manganese cobaltate, lithium nickel manganese aluminum, lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, lithium manganese silicate, spinel lithium manganese oxide, spinel lithium nickel manganese oxide and lithium titanate.
[0062] The positive electrode active layer also includes a binder to bond the positive electrode active material particles to facilitate the formation of a film layer, and at the same time, it can also improve the bonding force between the positive electrode active layer and the positive electrode current collector. In some embodiments, the binder may include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylic (ester) styrene butadiene rubber, epoxy resin or nylon, etc. At least one of the above.
[0063] The positive electrode active layer may also include a conductive material, including but not limited to a carbon-based material, a metal-based material, a conductive polymer, or any combination thereof. In some embodiments, the carbon-based material may include but is not limited to natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, the metal-based material may include but is not limited to metal powder or metal fiber, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.
[0064] Diaphragm
[0065] The material and shape of the diaphragm used in the electrochemical device of the present application are not particularly limited, and it can be any technology disclosed in the prior art. In some embodiments, the diaphragm includes a polymer or inorganic substance formed of a material that is stable to the electrolyte of the present application. In the present application, the diaphragm described above is used.
[0066] For example, the substrate layer is a non-woven fabric, film or composite film with a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, polypropylene porous film, polyethylene porous film, polypropylene non-woven fabric, polyethylene non-woven fabric or polypropylene-polyethylene-polypropylene porous composite film can be selected.
[0067] Electrolyte
[0068] According to some embodiments of the present application, the electrolyte includes an organic solvent, a lithium salt, and optional additives.
[0069] The organic solvent in the electrolyte of the present application may be any organic solvent known in the prior art that can be used as a solvent for the electrolyte. The electrolyte used in the electrolyte according to the present application is not limited, and it can be any electrolyte known in the prior art. The additive of the electrolyte according to the present application can be any additive known in the prior art that can be used as an electrolyte additive. In some embodiments, the organic solvent includes, but is not limited to: ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC) or ethyl propionate.
[0070] In some embodiments, the organic solvent includes an ether solvent, for example, at least one of 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME). In some embodiments, the lithium salt includes at least one of an organic lithium salt or an inorganic lithium salt. In some embodiments, the lithium salt includes, but is not limited to: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), bistrifluoromethanesulfonyl imide lithium LiN(CF3 SO2)2 (LiTF SI), bis(fluorosulfonyl)imide lithium Li(N(SO2F)2)(LiF SI), lithium bis(oxalate borate) LiB(C2O4)2 (LiB OB) or lithium difluorooxalate borate LiBF2(C2O4) (LiDFOB). In some embodiments, the additive includes at least one of fluoroethylene carbonate and adiponitrile.
[0071] According to some embodiments of the present application, the electrochemical device of the present application includes, but is not limited to: a lithium-ion battery.
[0072] The present application also applies the electrochemical device to the electronic device, and the electrochemical device supplies power to the load of the electronic device. In the above electronic device, the electrochemical device has good kinetic performance and cycle performance, which is conducive to improving the service life and charging efficiency of the electronic device.
[0073] Among them, electronic devices may include but are not limited to laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini CDs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.
[0074] The present application is described below by specific examples and comparative examples. Those skilled in the art should understand that the preparation methods described in the present application are only examples, and any other suitable preparation methods are within the scope of the present application.
[0075] Example 1
[0076] Preparation of battery separator:
[0077] A substrate is provided. An inorganic ceramic coating is coated on one surface of the substrate layer. The inorganic ceramic coating comprises boehmite and an acrylic binder. Based on the mass of the inorganic ceramic coating, the mass proportion of the boehmite is 90%.
[0078] Add 90g of polymer particles (weight average molecular weight of 600,000, polymer monomers including 5% by weight of methyl acrylate, 78% by weight of styrene, 2% by weight of butadiene and 15% by weight of isobutyl acrylate) into a blender, add 10g of sodium carboxymethyl cellulose, stir and mix evenly, add 5g of wetting agent dimethylsiloxane, and then add deionized water and stir, adjust the viscosity of the slurry to 2000mPa·s~5000mPa·s, and the solid content to 5%, to obtain a bonding layer slurry.
[0079] Then, the bonding layer slurry was evenly coated on the surface of the inorganic ceramic coating layer and the substrate layer by screen printing, with a coating weight of 1 mg / 5000 mm 2 , and then dried in an oven to form a bonding layer, thereby obtaining a diaphragm, wherein the porosity of the diaphragm is 42.5%, the thickness of the bonding layer is 0.5 μm, and the thickness ratio of the inorganic coating layer to the substrate layer is 0.4.
[0080] Preparation of negative electrode sheet:
[0081] The negative electrode active materials artificial graphite, acetylene black, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in a mass ratio of 96:1:1.5:1.5, and then deionized water is added as a solvent to prepare a negative electrode slurry with a solid content of 70%, and then a vacuum mixer is used to stir evenly. The negative electrode slurry is evenly coated on one surface of a copper foil with a thickness of 8 μm, dried at 110°C, and cold pressed to obtain a negative electrode sheet coated with a 150 μm negative electrode active material layer on one side, and then the above coating steps are repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet coated with a negative electrode active material layer on both sides. The negative electrode sheet is cut into a specification of 74 mm × 867 mm and welded to the pole ear for standby use.
[0082] <Preparation of positive electrode sheet>
[0083] The positive electrode active materials lithium cobalt oxide, acetylene black, and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then N-methylpyrrolidone (NMP) is added as a solvent to prepare a positive electrode slurry with a solid content of 75%, and then a vacuum mixer is used to stir evenly. The positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, dried at 90°C, and cold pressed to obtain a positive electrode sheet coated with a 100μm thick positive electrode active material layer on one side, and then the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet coated with a positive electrode active material layer on both sides. The positive electrode sheet is cut into a specification of 74mm×867mm and welded to the pole ear for standby use.
[0084] <Preparation of Electrolyte>
[0085] In an environment with a water content of less than 10ppm, non-aqueous organic solvents of ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), propyl propionate (PP), and vinylene carbonate (VC) are mixed in a mass ratio of 20:30:20:28:2, and then lithium hexafluorophosphate (LiPF6) is added to the non-aqueous organic solvent to dissolve and mix evenly to obtain an electrolyte. Based on the total mass of the electrolyte, the mass content of LiPF6 is 8%.
[0086] <Preparation of Secondary Battery>
[0087] The positive electrode sheet, battery separator and negative electrode sheet prepared above are stacked in order, so that the separator is located between the positive electrode sheet and the negative electrode sheet to play a role of isolation, wherein one surface of the separator containing the inorganic ceramic coating faces the positive electrode sheet and contacts the positive electrode sheet, and then wound to obtain an electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, and the moisture is removed at 80°C, and the prepared electrolyte is injected, and a secondary battery is obtained through vacuum packaging, standing, formation, shaping and other processes.
[0088] Related performance test methods of diaphragm:
[0089] (1) Number of polymer particles C value and D value
[0090] In the scanning electron microscope of the cross section of the diaphragm, at a magnification of 2K times, the image statistics method was used to count the particle sizes of the polymer particles in the area of 11.6μm×7.6μm, and the particle size of the single particle was used as the standard. The secondary particles formed by multiple particles were excluded, and the C value and D value of the polymer particles were recorded.
[0091] (2) Average diameter of polymer particles L
[0092] In the scanning electron microscope of the diaphragm, the image statistics method was used to count the particle size of the polymer particles in the area of 11.6μm×7.6μm, and the particle size of the single particle was taken as the standard. The secondary particles formed by multiple particles were excluded, and the diameter of the polymer particles was recorded. The diameters of 32 polymer particles were randomly selected and their average value L was calculated.
[0093] (3) Particle size Dv50 and Dv90 of inorganic particles
[0094] Use laser particle size analyzer Malvern 3000 for measurement. Add 50ml water to the beaker, add about 2g of material (inorganic particles), stir the solution to make the material fully dispersed; after the equipment is cleaned, add more than 2 / 3 of DI water, adjust the speed to 2800±50. Click "Initialize Instrument" and wait for the instrument to complete initialization. Click "Measure Background". The laser intensity is required to be higher than 70%, and the background light intensity must be lower than 100. After the background test is completed, add the test sample. When the laser shading reaches the specified range of 10-12%, wait for 5-8S, click "Test Sample" to automatically generate the value after the test is completed, and record the three sets of test data Dv 10, Dv50, and Dv90; Equipment parameter settings: refractive index 1.765, absorptivity 0.1, density 1.05.
[0095] (4) Thickness of bonding layer, inorganic coating and diaphragm
[0096] The test was performed using a VL 500,000 caliper, which included pressing the "▼" button to make the measuring head close to the test platform, and pressing the "zero" button to reset the thickness gauge. Press the "▲" button to raise the measuring head, pick up the diaphragm and place it flat on the test platform, so that the diaphragm at the measuring position remains flat on the test platform and the measuring position is aligned with the measuring head. Press the "▼" button until the measuring head is still. When the data remains stable, record the data in a table; measure 16 points evenly in the horizontal direction (1 point is tested every 20 mm; measure 16 points evenly in the width, and then calculate the average value of the 32 points measured in the horizontal and width directions. Similarly, the bonding layer and inorganic coating are measured in the same way.
[0097] (5) Coating weight per unit area of adhesive layer
[0098] The samples before and after the substrate layer is coated with the adhesive layer are punched into strips of 50*100mm, and the weight is measured with a 4-decimal electronic balance. m1 and m2 are recorded. Six test points are taken before and after coating to find the average value and calculate the coating weight per unit area.
[0099] (6) Porosity of the diaphragm
[0100] Cut the membrane sample into discs with a diameter of 10 mm, and put the punched membrane sample into the sample cup. Place the sample cup into the sample chamber, close the sample chamber, and use the gas exchange method of the true density meter to test. Record the test results, test each membrane sample 3 times and take the average value.
[0101] (7) Number of polymer particles and protrusions
[0102] In the scanning electron microscope of the diaphragm, the image statistics method was used to count the particle sizes of the polymer particles in the area of 11.6μm×7.6μm, and the particle size of the single particle was taken as the standard, and the secondary particles formed by multiple particles were excluded, and the number of polymer particles was recorded; at a magnification of 10,000 times the SEM, a single particle was selected to count the number of protrusions on the particle, and the number of protrusions of 32 polymer particles was counted and the average value was taken.
[0103] Performance test of lithium-ion battery:
[0104] Adhesion test between diaphragm and electrode plate:
[0105] The national standard GB / T 2790-1995, i.e., the 180° peel test standard, was adopted to test the bonding force between the diaphragm and the positive electrode sheet or the negative electrode sheet. The diaphragm and the positive electrode sheet or the negative electrode sheet were cut into 54.2 mm × 72.5 mm samples. The diaphragm and the positive electrode sheet or the negative electrode sheet were compounded and hot pressed using a hot press. The hot pressing conditions were: temperature 85°C, pressure 1 MPa, and hot pressing time 85 s (seconds). The compounded samples were cut into 15 mm × 54.2 mm strips. The bonding force between the diaphragm and the positive electrode sheet or the negative electrode sheet was tested according to the 180° peel test standard.
[0106] Low temperature capacity retention test:
[0107] At 25°C, the lithium-ion battery is charged to 4.53V at 0.5C constant current, charged to 0.02C at constant voltage, and then discharged to 2.5V at 0.2C at constant current, and the discharge capacity of the lithium-ion battery at 25°C is recorded; then, the lithium-ion battery is charged to 4.53V at 0.5C constant current, charged to 0.02C at constant voltage, and then the lithium-ion battery is placed at -20°C and discharged to 2.5V at 0.2C constant current, and the discharge capacity of the lithium-ion battery at -20°C is recorded. Calculate the capacity retention rate of the lithium-ion battery at -20°C, low temperature capacity retention rate = (final discharge capacity of the secondary battery at -20°C / discharge capacity of the first cycle of the secondary battery at 25°C) × 100%.
[0108] High temperature (45°C) cycle performance test:
[0109] At 45°C, the lithium-ion battery is charged to 4.35V at 3C constant current and to 1.8C at constant voltage, and then discharged to 3.0V at 0.7C to complete a cycle, which is recorded as the first cycle. Then, the above steps are repeated for 800 cycles, and the capacity retention rate after 800 cycles is calculated. The capacity retention rate after 800 cycles = (discharge capacity after 800 cycles / discharge capacity after the first cycle) × 100%.
[0110] Rate performance test:
[0111] At 25°C, the lithium-ion battery is charged to 4.47V at 0.5C constant current, and charged to 0.05C at constant voltage, and then rests for 5 minutes, and then discharged to 3.0V at 0.2C constant current, and then rests for 5 minutes, and then charged to 4.47V at 0.5C constant current, and then charged to 0.05C at constant voltage, and then rests for 5 minutes, and then discharged to 3.0V at 0.5C constant current, and the capacity D1 is recorded, and then rests for 5 minutes, and then, discharged to 3.0V at 2C constant current, and the capacity D2 is recorded. Rate performance = D2 / D1*100%.
[0112] Energy density test:
[0113] The lithium-ion battery was charged to 4.47V at a constant current of 0.5C, charged to 0.05C at a constant voltage, rested for 5 minutes, and then discharged to 3.0V at a constant current of 0.2C. The capacity D of the lithium-ion battery was recorded. The volume V of the lithium-ion battery was calculated based on the size of the lithium-ion battery. The energy density of the lithium-ion battery = D / V.
[0114] Self-discharge rate K value of lithium-ion battery:
[0115] The initial voltage V1 of the lithium-ion battery is tested. After the lithium-ion battery is left to stand for 48 hours, the voltage V2 of the lithium-ion battery is tested. K value = (V1-V2) / 48.
[0116] Example 2 to Example 6
[0117] The relevant parameters in Table 1 were obtained by adjusting the coating weight per unit area of the bonding layer and the number of polymer particles embedded in the inorganic coating layer. The rest was the same as in Example 1.
[0118] Comparative Example 1 to Comparative Example 3
[0119] The relevant parameters in Table 1 and Table 2 are obtained by adjusting the particle sizes Dv50 and Dv90 of the inorganic particles in the inorganic coating, and the rest are the same as in Example 1.
[0120] Example 7 to Example 13
[0121] The particle size Dv50 and the thickness of the inorganic coating were changed to obtain the relevant parameters in Table 3 and Table 4, and the rest were the same as in Example 1.
[0122] Example 14 to Example 25
[0123] The thickness of the inorganic coating layer is adjusted, or the average diameter of the polymer particles and the thickness of the bonding layer are adjusted to obtain the relevant parameters in Table 5 and Table 6. The rest is the same as in Example 1.
[0124] Example 26 to Example 32
[0125] The porosity and the ratio of d1 / d2 of the diaphragm were adjusted to obtain the relevant parameters in Table 7 and Table 8. The rest was the same as in Example 1.
[0126] Example 33 to Example 36
[0127] The content relationship of the components in the polymer monomer is adjusted, or the number of protrusions is adjusted to obtain the relevant parameters in Table 9 and Table 10, and the rest is the same as Example 1.
[0128] Table 1
[0129]
[0130] Table 2
[0131]
[0132] It can be seen from Tables 1 and 2 above that when the C / D ratio of the number of embedded polymer particles is greater than or equal to 0.5, it can improve the K value, energy density, rate performance, low temperature performance and high temperature cycle performance of the lithium-ion battery.
[0133] Table 3
[0134]
[0135]
[0136] Table 4
[0137]
[0138] It can be seen from Tables 3 and 4 above that by changing the particle size Dv50 of the inorganic coating and the thickness of the inorganic coating in Examples 7 to 13, the ratio of the number of polymer particles embedded is within an appropriate range, and the lithium ion batteries prepared by the assembly thereof have good lithium ion battery K value, high temperature cycle performance, low temperature performance and rate performance.
[0139] Table 5
[0140]
[0141] Table 6
[0142]
[0143] It can be seen from Tables 5 and 6 above that in Examples 14 to 19 and Examples 24 and 25, the thickness of the inorganic coating is changed. When the thickness of the inorganic coating is within an appropriate range, the lithium ion batteries prepared therefrom have good lithium ion battery K value, low temperature performance and rate performance.
[0144] In Examples 20 to 24, the average diameter of the polymer particles and the thickness of the bonding layer are adjusted within a suitable range, and the lithium-ion batteries prepared by assembling them have good high-temperature cycle performance, low-temperature performance and rate performance.
[0145] Table 7
[0146]
[0147] Table 8
[0148]
[0149] In Table 7 and Table 8, in Example 26 to Example 28, the porosity of the diaphragm is changed. When the porosity of the diaphragm meets the appropriate range, the lithium ion battery assembled therefrom has good high temperature cycle performance, low temperature performance and rate performance.
[0150] In Examples 28 to 32, the ratio of the thickness d1 of the inorganic coating layer to the thickness d2 of the substrate layer is changed. Within a suitable range, the lithium-ion battery has good energy density, high-temperature cycle performance and rate performance.
[0151] Table 9
[0152]
[0153] In Table 9, in Example 28 and Examples 33 to 34, in different polymer monomers, the obtained polymer particles are applied to the diaphragm, and the diaphragm has good adhesion to the positive / negative electrode sheets, and the lithium-ion batteries assembled therefrom have good energy density, high temperature cycle performance and rate performance.
[0154] Table 10
[0155]
[0156] From the above Table 10, changing the mass proportion of methyl acrylate in the polymer monomer can change the number of protrusions on the surface of the polymer particles. The number of protrusions is within an appropriate range, which is beneficial to making the separator have good adhesion with the positive electrode sheet / negative electrode sheet, and is beneficial to improving the high temperature cycle performance of the lithium-ion battery.
[0157] The above disclosure is only a preferred implementation mode of the present application, and certainly cannot be used to limit the present application. Therefore, equivalent changes made according to the present application are still within the scope covered by the present application.
Claims
1. A diaphragm, characterized in that: It includes a substrate layer, an inorganic coating and a bonding layer, wherein the inorganic coating is arranged between the substrate layer and the bonding layer, the inorganic coating includes inorganic particles, the bonding layer includes polymer particles, at least part of the polymer particles are embedded in the pores of the inorganic coating, in a 2000-fold scanning electron microscope photograph of the cross section of the diaphragm, within a 11.6μm×7.6μm area, the number of polymer particles embedded in the inorganic coating to a depth greater than or equal to 100nm is C, the total number of polymer particles in the cross section is D, and 0.5≤C / D<0.
94.
2. The diaphragm according to claim 1, characterized in that 0.71≤C / D<0.
94.
3. The diaphragm according to claim 1, characterized in that The average diameter L of the polymer particles and the particle size Dv50 of the inorganic particles satisfy: 0.4≤L / Dv50≤0.
8.
4. The diaphragm according to claim 1, characterized in that The diaphragm satisfies at least one of the following conditions: (1) The thickness of the inorganic coating is 0.5 μm to 5 μm; (2) The thickness of the inorganic coating is d 1 μm, C = 7.6d 1 + 7.4; (3) The average diameter L of the polymer particles is 0.3 μm to 5 μm; (4) The particle size Dv50 of the inorganic particles is 0.4 μm to 6.5 μm, and Dv90 is 0.8 μm to 8.7 μm; (5) The thickness of the adhesive layer is 0.5 μm to 2 μm, and the coating weight per unit area of the adhesive layer is 0.5 mg / 5000 mm 2 Up to 3mg / 5000mm 2 ; (6) The thickness of the inorganic coating layer is d1, the thickness of the substrate layer is d2, and 0.05≤d1 / d2≤1.
0.
5. The diaphragm according to claim 1, characterized in that The inorganic particles include at least one of aluminum oxide, aluminum oxide, silicon dioxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zirconium oxide, zinc oxide, calcium oxide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate; The inorganic coating further comprises a binder, wherein the binder comprises at least one of acrylic acid, methyl methacrylate, butyl acrylate, octyl acrylate, isooctyl acrylate, butadiene or acrylonitrile; Based on the mass of the inorganic coating, the mass percentage of the inorganic particles is 85% to 95%.
6. The diaphragm according to claim 1, characterized in that The polymer particles in the bonding layer are selected from at least two of the following monomers: butadiene, methyl acrylate, methyl methacrylate, styrene, butyl methacrylate, isooctyl acrylate, isobutyl acrylate, ethylene, propylene or vinylidene fluoride; The polymer particles also include at least one of acrylic acid, acrylonitrile or butadiene.
7. The diaphragm according to claim 1, characterized in that The porosity of the separator is 30% to 50%.
8. The diaphragm according to claim 1, characterized in that The surface of the polymer particle has a plurality of protrusions. In a 10,000-fold scanning electron microscope photograph of the separator, the number of the protrusions in each polymer particle is 5 to 50 within an area of 11.6 μm×7.6 μm.
9. The diaphragm according to claim 1, characterized in that The separator comprises two bonding layers, one bonding layer is located on the surface of the inorganic coating layer facing away from the substrate layer, and the other bonding layer is located on the surface of the substrate layer facing away from the inorganic coating layer.
10. An electrochemical device, comprising an electrode assembly, wherein the electrode assembly comprises a positive electrode sheet and a negative electrode sheet, characterized in that: The electrode assembly further comprises a separator as claimed in any one of claims 1 to 9, wherein the separator is located between the positive electrode sheet and the negative electrode sheet.
11. An electronic device, characterized in that: Comprising the electrochemical device as claimed in claim 10.
Citation Information
Cited By
Lithium ion secondary battery
CN119542509A
Composite separator, method for manufacturing the same, and secondary battery
CN120728170B