Internal packaging perovskite thin film, preparation method thereof and application of internal packaging perovskite thin film in solar cell
By using fluoropolyamic acid ester to form an internal packaging network structure in perovskite solar cells, the problems of aging and lead leakage in harsh environments are solved, and efficient and stable perovskite solar cells are achieved. Power conversion efficiency and stability are significantly improved.
Patent Information
- Application Number
- CN202411120037.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
Perovskite solar cells age faster in harsh environments, resulting in a decline in performance, and the prior art cannot effectively prevent lead leakage.
The internal encapsulation network structure is formed in the perovskite precursor solution by using fluoropolyamic acid ester (PAE) to form an internal encapsulation network structure, and the internal encapsulation perovskite film is prepared by solution spin coating method, and ultraviolet irradiation is used to promote the cross-linking reaction during the annealing process. A hydrophobic inner encapsulated perovskite layer is formed.
Significantly improves the power conversion efficiency and stability of perovskite solar cells, with PCE reaching 25.88%, maintaining 93% initial efficiency after continuous light in nitrogen environment and heating at 65°C, preventing lead leakage, and does not change color in deionized water. .
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solar cells, and in particular relates to an internally encapsulated perovskite film, a preparation method thereof, and an application thereof in a solar cell. Background Art
[0002] In recent decades, organic-inorganic halide perovskite solar cells (PSCs) have attracted extensive attention due to their rapid development, and their power conversion efficiency (PCE) has soared from 3.8% to 26.1%, offering great potential for the next-generation photovoltaic technology.
[0003] However, harsh external environmental conditions (such as water, oxygen, light, and thermal stress) can accelerate the aging of the perovskite layer, greatly reducing the performance of solar cells. To address this problem, the various functional layers of PSC (including perovskite layer, electron transport layer (ETL), hole transport layer (HTL), and counter electrode), as well as related interfaces and external encapsulation layers should be comprehensively considered and designed to meet the needs of practical applications. As the first line of defense against the external environment, the external encapsulation layer of the device has been proven to be one of the best ways to solve its stability and improve the life of the device. External physical encapsulation using high-performance encapsulation materials has been widely adopted. However, for the inside of the device, due to the various defects (such as vacancies, interstitials, and antisites), soft ionic lattices, and multiple interfaces of perovskite materials, it is also crucial to passivate defects, stabilize the structure, and enhance charge transfer through internal encapsulation of the device. The internal encapsulation of the perovskite layer is conducive to improving the stability of the perovskite and preventing lead leakage at the same time. Therefore, the internal encapsulation of perovskite has become one of the problems that need to be solved urgently.
[0004] Xu Ligang et al. (CN116113250A) disclosed a long-lasting and stable perovskite solar cell and its preparation method. By adding ammonium hexafluorophosphate (NH4PF6) to the anti-solvent to form a perovskite light absorption layer of the original perovskite / ion exchange perovskite / NH4PF6 in-situ protective layer, the stability of the device under various conditions is improved. Although the fluorine-containing structural additive improves the stability of the device to a certain extent, due to its small molecule structure, it cannot form an internal encapsulation network, thereby failing to prevent lead leakage. In view of the above background and problems, this invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a perovskite solar cell with an internal encapsulation network structure and a preparation method thereof. The present invention can not only improve the stability of the perovskite solar cell, but also prevent lead leakage.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions: In a first aspect, the present invention provides an internally encapsulated perovskite film and a method for preparing the same.
[0007] The internally encapsulated perovskite film provided by the present invention is prepared according to a method comprising the following steps: (1) Fluorinated polyamic acid ester (PAE), initiator, crosslinking agent and Cs 0.05 FA 0.95 The raw materials of the PbI3 perovskite precursor solution are dissolved in a solvent and stirred at room temperature in a glove box to form an internally encapsulated perovskite precursor solution; (2) The internal encapsulated perovskite film was prepared on the substrate by solution spin coating.
[0008] In step (1) of the above method, the fluorinated polyamic acid ester is a hydrophobic photosensitive polymer material containing polyfluorine, and its structure is shown in Formula I:
[0009] Among them, m1= 0.75, m2= 0.25, n = 15.
[0010] The preparation method of PAE shown in formula I is as follows: hydroxyethyl methacrylate (HEMA), triethylamine (TEA), 4,4'-biphenyl ether dianhydride (ODPA) and 4,4'-(hexafluoroisopropylene) diphenyl anhydride (6FDA) are mixed and dissolved in N-methyl-2-pyrrolidone (NMP), and thionyl chloride (SOCl2) is added to carry out chlorination reaction; at 0~15°C, the mixture solution is slowly added dropwise to the NMP solution of 2,2'-bistrifluoromethyl-4,4'-diaminobiphenyl (TFDB), and then reacted at room temperature to generate a PAE solution, and then the solution is precipitated in deionized water, and after filtering, washing and drying, the PAE shown in formula I is obtained.
[0011] The initiator is at least one of benzophenone, dibenzyl ketone, 2-methylthioxanthone, 2,2'-diethoxyacetophenone, 1-phenyl-1,2-propanedione-2-(O-methoxycarbonyl)oxime and 1-phenyl-1,2-butanedione-2-(O-methoxycarbonyl)oxime; The crosslinking agent is at least one of 1,4-butanediol dimethacrylate, trimethylolpropane trimethacrylate, tetraethylene glycol dimethacrylate, ethylene glycol diethyl ether methacrylate, polyethylene glycol diacrylate and glycidyl methacrylate.
[0012] The concentration of the fluorinated polyamic acid ester (PAE) in the internally encapsulated perovskite precursor solution is 0.01-5 mg / mL, preferably 0.05-1 mg / mL.
[0013] The concentration of the initiator in the internally encapsulated perovskite precursor solution is 0.0001-1 mg / mL, preferably 0.001-0.01 mg / mL.
[0014] The concentration of the crosslinking agent in the internally encapsulated perovskite precursor solution is 0.001-0.1 mg / mL, preferably 0.01-0.05 mg / mL.
[0015] The preparation of Cs 0.05 FA 0.95 The raw materials of the PbI3 perovskite precursor solution include: formamidine hydroiodide (FAI), CsI, PbI2, and methylammonium chloride (MACl), and the mass ratios of the FAI, CsI, PbI2, and MACl are 13:1:40:1.8 respectively.
[0016] In step (1) of the above method, the solvent is a mixed solvent obtained by mixing DMF and DMSO in a volume ratio of 4:1 to 10:1.
[0017] In step (2) of the above method, the substrate may be an ITO glass substrate.
[0018] In step (2) of the above method, the method for preparing an inner-encapsulated perovskite film on a substrate by solution spin coating is specifically as follows: the inner-encapsulated perovskite precursor solution is spin coated on the substrate, and before the end of spin coating, the anti-solvent ether is dripped on the substrate, followed by annealing treatment, and after annealing, cooling to room temperature, an inner-encapsulated perovskite film is formed.
[0019] In the above method, the anti-solvent ether is added dropwise 10 to 20 seconds before the end of spin coating, preferably 20 seconds.
[0020] In the above method, an electron transport layer (such as a SnO2 layer) is also provided on the substrate.
[0021] According to one embodiment of the present invention, the inner encapsulated perovskite precursor solution (60 μL) was spin coated at 1000 rpm for 10 s and 5000 rpm for 30 s on the SnO2 electron transport layer of the ITO glass substrate, and 20 s from the end of the spin coating, ether (700 μL) was quickly dripped onto the substrate as an anti-solvent.
[0022] In the above method, the annealing temperature is 100-150° C., and the annealing time is 0.5-1.5 h, specifically annealing at 120° C. for 1 h.
[0023] During the annealing process, the film is irradiated with a 365 nm ultraviolet lamp for a period of time, and the irradiation time may be 1 to 300 s, preferably 30 to 200 s.
[0024] In a second aspect, the present invention provides the use of the internally encapsulated perovskite film described in the first aspect in the preparation of a perovskite solar cell.
[0025] In a third aspect, the present invention provides an inner-encapsulated perovskite solar cell comprising the inner-encapsulated perovskite film described in the first aspect of the present invention.
[0026] The internally encapsulated perovskite solar cell provided by the present invention comprises the above-mentioned internally encapsulated perovskite film of the present invention.
[0027] Furthermore, the structure of the inner-encapsulated perovskite solar cell includes, from bottom to top, a substrate, an electron transport layer, an inner-encapsulated perovskite layer, a hole transport layer, and a metal electrode.
[0028] Specifically, the substrate may be an ITO glass substrate; the electron transport layer may be a SnO2 electron transport layer, and its thickness may be 20~30 nm; the thickness of the inner encapsulation perovskite layer may be 600~700 nm; the hole transport layer may be a 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) layer, and its thickness may be 90~120 nm; the metal electrode may be Au, and its thickness may be 80~100 nm.
[0029] In a fourth aspect, the present invention provides a method for preparing the internally encapsulated perovskite solar cell of the third aspect of the present invention.
[0030] The method for preparing the internally encapsulated perovskite solar cell provided by the present invention comprises the following steps: (a) preparing an electron transport layer on a substrate; (b) Spin coating on the electron transport layer to prepare the inner encapsulated perovskite film; (c) preparing a hole transport layer on the inner encapsulated perovskite film; (d) Preparing a metal electrode on the hole transport layer to obtain the perovskite solar cell.
[0031] In step (a) of the above method, the substrate is an ITO glass substrate, which needs to be treated as follows before use: the ITO glass is ultrasonically cleaned with water, acetone and isopropanol for 15 minutes in sequence, blown dry with a nitrogen gun after cleaning, and then placed in a plasma cleaner for ultraviolet ozone treatment for 10 minutes.
[0032] In step (a) of the above method, a SnO2 electron transport layer can be prepared on an ITO glass substrate. According to one embodiment of the present invention, the specific preparation method is as follows: a SnO2 colloidal aqueous solution (15 wt.%) is spin-coated on the treated ITO glass at a speed of 4000 rpm for 30 s, and annealed on a hot stage at 150 ° C for 30 min to form a SnO2 electron transport layer.
[0033] In step (b) of the above method, the method for preparing the internal encapsulation perovskite film by spin coating on the electron transport layer can be carried out according to the method described in the first aspect of the present invention.
[0034] After step (b) and before step (c), the method further includes a step of passivating the inner encapsulated perovskite film prepared in step (b), specifically, spin coating the MeO-PEAI solution on the inner encapsulated perovskite film, and then annealing the inner encapsulated perovskite film at 100° C. for 5 min to passivate the perovskite film.
[0035] According to an embodiment of the present invention, 4-MeOPEAI was dissolved in isopropanol (3 mg / mL); the 4-MeOPEAI solution (100 μL) was spin coated on the inner encapsulated perovskite film at 4000 rpm for 30 s, and then the inner encapsulated perovskite film was annealed at 100° C. for 5 min to passivate the perovskite film.
[0036] In step (c) of the above method, the hole transport layer is a 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) layer. According to one embodiment of the present invention, the specific preparation method is as follows: a Spiro-OMeTAD solution of a certain concentration is spin-coated on the inner encapsulated perovskite film at a speed of 4000 rpm for 30 seconds to form a Spiro-OMeTAD hole transport layer.
[0037] In step (d) of the above method, a metal electrode is prepared on the hole transport layer by vacuum evaporation.
[0038] In the inner-encapsulated perovskite solar cell, the fluorinated polyamic acid ester in the perovskite layer is photosensitive, undergoes a cross-linking reaction after being exposed to ultraviolet light, and forms an inner-encapsulated perovskite layer, which contains a hydrophobic polyfluorine structure, thereby improving the power conversion efficiency and stability of the battery, and its PCE can reach 25.88%. After continuous illumination and heating at 65°C in a glove box filled with nitrogen, it can still maintain 93% and 88% of the initial efficiency. At the same time, it can prevent lead leakage, and the inner-encapsulated perovskite solar cell can remain in deionized water for 1 minute without changing color.
[0039] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention forms an inner encapsulation network structure by adding fluorinated polyamic acid ester (PAE) into the perovskite precursor solution, thereby significantly improving the power conversion efficiency and stability of the battery.
[0040] (2) The PCE of the inner-encapsulated perovskite solar cell prepared by the present invention can reach 25.88%, and it can still maintain 93% and 88% of the initial efficiency after continuous illumination and heating at 65°C in a glove box filled with nitrogen. At the same time, it can prevent lead leakage, and the inner-encapsulated perovskite solar cell can remain in deionized water for 1 minute without changing color.
[0041] (3) The present invention provides a new idea for preparing high-efficiency and long-lasting perovskite solar cells. Compared with the existing technology, the preparation cost is low, the power conversion efficiency and stability are significantly improved, reaching the world's first-class level, and it has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 is the structural formula of the fluorinated polyamic acid ester described in the present invention.
[0043] Figure 2 This is a scanning electron microscope cross-sectional view of the internally encapsulated perovskite solar cell prepared in Example 1 of the present invention.
[0044] Figure 3 JV curves of the standard perovskite solar cell prepared in Comparative Example 1 of the present invention and the internally encapsulated perovskite solar cell prepared in Example 1.
[0045] Figure 4 This is a comparison chart of the thermal stability of the standard perovskite solar cell prepared in Comparative Example 1 of the present invention and the internally encapsulated perovskite solar cell prepared in Example 1.
[0046] Figure 5 This is a comparison chart of the photostability of the standard perovskite solar cell prepared in Comparative Example 1 of the present invention and the internally encapsulated perovskite solar cell prepared in Example 1.
[0047] Figure 6 This is a comparison chart of the X-ray photoelectron spectra of the internally encapsulated perovskite film prepared by PAE in the present invention and Example 1.
[0048] Figure 7 This is a comparison diagram of the water drop contact angles of the standard perovskite film prepared in Comparative Example 1 of the present invention and the internal encapsulation perovskite film prepared in Example 1.
[0049] Figure 8 Scanning electron microscope surface images of the standard perovskite film prepared in Comparative Example 1 of the present invention and the internal encapsulation perovskite film prepared in Example 1.
[0050] Fig. 9 This is a comparison chart of the standard perovskite film prepared in comparative example 1 of the present invention and the internal encapsulation perovskite film prepared in example 1 after being immersed in water for one minute.
[0051] Fig.10 This is a JV curve diagram of the internally encapsulated perovskite solar cell prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0052] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.
[0053] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.
[0054] The PAE structure used in the following examples is shown in Formula I:
[0055] Among them, m1= 0.75, m2= 0.25, n = 15.
[0056] The preparation method is as follows: In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer, a thermometer and a nitrogen protection device, 26.03 g of 2-hydroxyethyl methacrylate (HEMA), 15.82 g of pyridine, 7.76 g (0.025 mol) of 4,4'-biphenyl ether dianhydride (ODPA), 33.32 g (0.075 mol) of 4,4'-(hexafluoroisopropylene) diphenyl anhydride (6FDA) and 200 g of N-methyl-2-pyrrolidone (NMP) were added in sequence and stirred at room temperature for 4 h. The above solution was reacted with 23.79 g of thionyl chloride (SOCl2) at 0°C for 2 h. After cooling the temperature to below 0°C, the solution was slowly added dropwise to a solution of 280 g of NMP containing 32.02 g (0.1 mol) of 2,2'-bistrifluoromethyl-4,4'-diaminobiphenyl (TFDB), and the reaction was carried out at room temperature for 5 h; the reaction solution was poured into 5 L of deionized water, the solid was precipitated, filtered, washed, and vacuum dried to obtain PAE.
[0057] Comparative Example 1 (1) The ITO glass was ultrasonically cleaned with water, acetone and isopropanol for 15 min in sequence, blown dry with a nitrogen gun after cleaning, and then placed in a plasma cleaner for UV-ozone treatment for 10 min.
[0058] (2) The SnO2 colloidal aqueous solution was mixed with ultrapure water in a volume ratio of 1:2, and the mixed solution was spin-coated on the ITO glass at a speed of 4000 rpm for 30 s. The mixture was then annealed on a hot stage at 150 °C for 30 min to form a SnO2 electron transport layer.
[0059] (3) The prepared SnO2 electron transport layer was transferred to a nitrogen environment glove box. FAI (240.76 mg), CsI (18.19 mg), PbI2 (728.40 mg) and MACl (33.08 mg) powders were dissolved in DMF (888 μL) and DMSO (111 μL) and stirred at room temperature for 6 h to form a standard perovskite precursor solution. The perovskite precursor solution (60 μL) was spin-coated at 1000 rpm for 10 s and 5000 rpm for 30 s on the SnO2 electron transport layer. 20 s from the end of spin coating, 700 μL of ether was quickly dropped onto the substrate as an anti-solvent. The perovskite precursor film was then annealed at 120 °C and 25% RH for 1 h to form a standard perovskite film.
[0060] (4) 4-MeOPEAI was dissolved in isopropanol (3 mg / mL). The 4-MeOPEAI solution (100 μL) was spin-coated on the standard perovskite film at 4000 rpm for 30 s, and then the perovskite film was annealed at 100 °C for 5 min to passivate the perovskite film.
[0061] (5) Spiro-OMeTAD (72.3 mg) was dissolved in 1000 μL chlorobenzene, and Li-TFSI solution (260 mg / mL) (17.5 μL) and TBP (28.8 μL) were added. The Spiro-OMeTAD mixed solution (50 μL) was spin-coated on the perovskite film at 4000 rpm for 30 s, and the prepared sample was oxidized in a desiccator for 10 h.
[0062] (6) Finally, in the vacuum coating machine, thermal evaporation (<2.5×10 -4 A standard perovskite solar cell was obtained by depositing 80 nm Au electrodes on a 400 nm Au electrode (Pa).
[0063] Embodiment 1, The difference between this embodiment and comparative example 1 lies in step (3), and the remaining steps are the same as those of comparative example 1.
[0064] (1) The ITO glass was ultrasonically cleaned with water, acetone and isopropanol for 15 min in sequence, blown dry with a nitrogen gun after cleaning, and then placed in a plasma cleaner for UV-ozone treatment for 10 min.
[0065] (2) The SnO2 colloidal aqueous solution was mixed with ultrapure water in a volume ratio of 1:2, and the mixed solution was spin-coated on the ITO glass at a speed of 4000 rpm for 30 s. The mixture was then annealed on a hot stage at 150 °C for 30 min to form a SnO2 electron transport layer.
[0066] (3) The prepared SnO2 electron transport layer was transferred into a nitrogen environment glove box. FAI (240.76 mg), CsI (18.19 mg), PbI2 (728.40 mg), MACl (33.08 mg), PAE (0.1 mg), 1-phenyl-1,2-propanedione-2-(O-methoxycarbonyl)oxime (0.005 mg) and ethylene glycol diethyl ether methacrylate (0.04 mg) powder were dissolved in DMF (888 μL) and DMSO (111 μL) and stirred at room temperature for 6 h to form an inner encapsulated perovskite precursor solution. The inner encapsulated perovskite precursor solution (60 μL) was spin-coated at 1000 rpm for 10 s and 5000 rpm for 30 s on the SnO2 electron transport layer. 20 s after the spin coating, 700 μL of ether was quickly dropped onto the substrate as an anti-solvent. The inner encapsulated perovskite precursor film was then annealed at 120 °C and 25% RH for 1 h, and irradiated with a 365 nm ultraviolet lamp for 30 s. After annealing, the inner encapsulated perovskite film was formed after cooling to room temperature.
[0067] (4) 4-MeOPEAI was dissolved in isopropanol (3 mg / mL). The 4-MeOPEAI solution (100 μL) was spin-coated on the inner encapsulated perovskite film at 4000 rpm for 30 s, and then the inner encapsulated perovskite film was annealed at 100 °C for 5 min to passivate the perovskite film.
[0068] (5) Spiro-OMeTAD (72.3 mg) was dissolved in 1000 μL chlorobenzene, and Li-TFSI solution (260 mg / mL) (17.5 μL) and TBP (28.8 μL) were added. The Spiro-OMeTAD mixed solution (50 μL) was spin-coated on the perovskite film at 4000 rpm for 30 s, and the prepared sample was oxidized in a desiccator for 10 h.
[0069] (6) Finally, in the vacuum coating machine, thermal evaporation (<2.5×10-4 The 80 nm Au electrode was deposited on a 400 nm Au-coated perovskite solar cell (PSC).
[0070] The performance of the internally encapsulated perovskite solar cell prepared in this embodiment was compared with that of the standard perovskite solar cell prepared in Comparative Example 1. The results are shown in Table 1 and Table 2. Figure 3 As shown. It can be seen that the PCE of the prepared inner package device is significantly improved.
[0071] Table 1 Performance comparison of standard devices and internal packaged devices
[0072] See also Figure 2 , is a scanning electron microscope cross-sectional view of the internally encapsulated perovskite solar cell prepared in Example 1. It can be seen that the perovskite layer has a uniform and dense morphology and few grain boundaries.
[0073] See also Figure 4 , which is a comparison chart of the thermal stability of the standard perovskite solar cell prepared in Comparative Example 1 and the internally encapsulated perovskite solar cell prepared in Example 1. It can be seen that under continuous heating at 65 °C in a N2 environment, the internally encapsulated perovskite solar cell can still maintain 88% of the initial efficiency after 500 h, while the standard internally encapsulated cell can only maintain 57%.
[0074] See also Figure 5 , which is a comparison chart of the photostability of the standard perovskite solar cell prepared in Comparative Example 1 and the internally encapsulated perovskite solar cell prepared in Example 1. It can be seen that under continuous irradiation at AM 1.5 light intensity in N2 environment, the internally encapsulated perovskite solar cell can still maintain 93% of the initial efficiency after 500 h, while the standard perovskite solar cell can only maintain 75%.
[0075] See also Figure 6 , which is a comparison of the X-ray photoelectron spectra of the inner encapsulated perovskite film prepared by PAE and Example 1. It can be seen that compared with pure PAE, the F 1s peak of the inner encapsulated perovskite film moves toward the high binding energy direction, indicating that F and uncoordinated Pb 2+ The interaction between them passivates the defects.
[0076] See also Figure 7 , which is a comparison diagram of the water drop contact angle of the standard perovskite film prepared in Comparative Example 1 and the inner encapsulated perovskite film prepared in Example 1. It can be seen that the water contact angle of the inner encapsulated perovskite film (73.0°) is significantly larger than the water contact angle of the standard perovskite film (56.2°), indicating that the formation of the inner encapsulation structure enhances the hydrophobicity of the perovskite film, which is beneficial to improving the stability of the device.
[0077] See also Figure 8, which is a scanning electron microscope surface image of the standard perovskite film prepared in comparative example 1 and the inner encapsulated perovskite film prepared in example 1. It can be seen that the grain size of the inner encapsulated perovskite film is significantly larger than that of the standard perovskite film, and there is no residual PbI2.
[0078] See also Fig. 9 , which is a comparison chart of the standard perovskite film prepared in comparative example 1 and the inner encapsulation perovskite film prepared in example 1 immersed in water for one minute. It can be seen that the standard perovskite film has completely turned yellow and degraded, while the color of the inner encapsulation perovskite film has hardly changed, indicating that the inner encapsulation strategy can prevent lead leakage.
[0079] Example 2 The difference between this embodiment and embodiment 1 is that: The concentrations of PAE in step (3) were adjusted to 0.05, 0.10 and 0.20 mg / mL, respectively. That is, the amounts of PAE were adjusted to 0.05 mg, 0.10 mg and 0.20 mg, respectively. The remaining steps were the same as in Example 1.
[0080] The performance of the prepared internally encapsulated perovskite solar cells with different PAE concentrations was compared, and the results are shown in Table 2 and Fig.10 As shown, it can be seen that when the PAE concentration is 0.10 mg / mL, the performance of the prepared encapsulated device is the best.
[0081] Table 2 Performance comparison of internal packaged devices with different PAE concentrations
[0082] In summary, in the inner-encapsulated perovskite solar cell proposed by the present invention, the fluorinated polyamic acid ester in the perovskite layer is photosensitive, undergoes a cross-linking reaction after being exposed to ultraviolet light, forms an inner-encapsulated perovskite layer, and contains a hydrophobic polyfluorine structure, so that the power conversion efficiency and stability of the battery are improved, and its PCE can reach 25.88%. After continuous illumination and heating at 65°C in a glove box filled with nitrogen, it can still maintain 93% and 88% of the initial efficiency. At the same time, it can prevent lead leakage, and the inner-encapsulated perovskite solar cell can remain in deionized water for 1 min without changing color.
[0083] The present invention has been described in detail above. It will be apparent to those skilled in the art that the present invention may be implemented in a wide range under equivalent parameters, concentrations and conditions without departing from the spirit and scope of the present invention and without the need for unnecessary experimentation. Although the present invention provides specific embodiments, it should be understood that further improvements may be made to the present invention. In short, according to the principles of the present invention, this application intends to include any changes, uses or improvements to the present invention, including changes made by conventional techniques known in the art that depart from the scope disclosed in this application. Applications of some of the basic features may be made within the scope of the following appended claims.
Claims
1. A method for preparing an internally encapsulated perovskite film, comprising the following steps: (1) Fluorinated polyamic acid ester (PAE), initiator, crosslinking agent and Cs 0.05 FA 0.95 The raw materials of the PbI3 perovskite precursor solution are dissolved in a solvent and stirred at room temperature to form an inner encapsulated perovskite precursor solution; (2) The internal encapsulated perovskite film was prepared on the substrate by solution spin coating.
2. The preparation method according to claim 1, characterized in that: In the step (1), the fluorinated polyamic acid ester is a hydrophobic photosensitive polymer material containing polyfluorine, and its structure is shown in Formula I: Where, m1 = 0.75, m2 = 0.25, n = 15; And / or, the initiator is at least one of benzophenone, dibenzyl ketone, 2-methylthioxanthone, 2,2'-diethoxyacetophenone, 1-phenyl-1,2-propanedione-2-(O-methoxycarbonyl)oxime and 1-phenyl-1,2-butanedione-2-(O-methoxycarbonyl)oxime; And / or, the cross-linking agent is at least one of 1,4-butanediol dimethacrylate, trimethylolpropane trimethacrylate, tetraethylene glycol dimethacrylate, ethylene glycol diethyl ether methacrylate, polyethylene glycol diacrylate and glycidyl methacrylate; and / or, the concentration of the fluorinated polyamic acid ester in the inner packaged perovskite precursor solution is 0.01 to 5 mg / mL, preferably 0.05 to 1 mg / mL; and / or, the concentration of the initiator in the internally encapsulated perovskite precursor solution is 0.0001 to 1 mg / mL, preferably 0.001 to 0.01 mg / mL; And / or, the concentration of the cross-linking agent in the internally encapsulated perovskite precursor solution is 0.001-0.1 mg / mL, preferably 0.01-0.05 mg / mL.
3. The preparation method according to claim 1 or 2, characterized in that: In the step (1), the preparation of Cs 0.05 FA 0.95 The raw materials of the PbI3 perovskite precursor solution include: formamidine hydroiodide (FAI), CsI, PbI2, methylammonium chloride (MACl), and the mass ratios of FAI, CsI, PbI2, and MACl are 13:1:40:1.8 respectively; And / or, in the step (1), the solvent is a mixed solvent obtained by mixing DMF and DMSO in a volume ratio of 4:1 to 10:
1.
4. The preparation method according to claim 1-3, characterized in that: In the step (2), the method for preparing an inner-encapsulated perovskite film on a substrate by solution spin coating is specifically as follows: the inner-encapsulated perovskite precursor solution is spin coated on the substrate, and before the end of spin coating, the anti-solvent ether is dripped on the substrate, followed by annealing treatment, and after annealing, cooling to room temperature to form an inner-encapsulated perovskite film.
5. The preparation method according to claim 4, characterized in that: The anti-solvent ether is added dropwise 10 to 20 seconds before the end of spin coating, preferably 20 seconds; And / or, the annealing temperature is 100-150° C., and the annealing time is 0.5-1.5 h; And / or, during the annealing process, a 365 nm ultraviolet irradiation lamp is used to irradiate the film for 1 to 300 s, preferably for 30 to 200 s.
6. An internally encapsulated perovskite film prepared by the method according to any one of claims 1 to 5.
7. An internally encapsulated perovskite solar cell, comprising the internally encapsulated perovskite film described in claim 6.
8. The internally encapsulated perovskite solar cell according to claim 7, characterized in that: The structure of the inner-encapsulated perovskite solar cell includes, from bottom to top, a substrate, an electron transport layer, the inner-encapsulated perovskite layer described in claim 6, a hole transport layer, and a metal electrode.
9. The internally encapsulated perovskite solar cell according to claim 8, characterized in that: The substrate is an ITO glass substrate; The electron transport layer is a SnO2 electron transport layer, and its thickness is 20-30 nm; The thickness of the inner encapsulated perovskite layer is 600-700 nm; The hole transport layer is a 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) layer having a thickness of 90-120 nm; The metal electrode is Au, and its thickness is 80-100 nm.
10. The method for preparing the internally encapsulated perovskite solar cell according to claim 8 or 9, comprising the following steps: (a) preparing an electron transport layer on a substrate; (b) preparing an internal encapsulated perovskite film by spin coating on the electron transport layer according to the method described in any one of claims 1 to 5; (c) preparing a hole transport layer on the inner encapsulated perovskite film; (d) Preparing a metal electrode on the hole transport layer to obtain the perovskite solar cell.
Citation Information
Cited By
Perovskite thin film with three-dimensional interpenetrating network structure and preparation method and application thereof