Thermally conductive silicone composition

By adding alkenyl organopolysiloxane, organohydrogen polysiloxane, surface-treated diamond particles and other components to the thermally conductive silicone composition, the contradiction between thermal conductivity and fluidity in the prior art is solved. It achieves a combination of high thermal conductivity and good fluidity, meeting the needs of improving the heat dissipation performance of electronic equipment.

CN119013361APending Publication Date: 2024-11-22HENKEL KGAA

Patent Information

Application Number
CN202280094493.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-04-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

While the existing thermal conductivity silicone compositions have limited fluidity while increasing the thermal conductivity, their fluidity is difficult to meet the demand for the increase in the heat dissipation performance of electronic equipment.

Method used

Compositions containing alkenyl organopolysiloxane, organohydrogen polysiloxane, surface-treated diamond particles, thermally conductive fillers in non-components, silane coupling agents and catalysts by specific proportions and treatment methods Improve the fluidity and thermal conductivity of the composition.

Benefits of technology

High thermal conductivity (greater than 10W/(m·K) and good fluidity (greater than 15g/min) during curing are achieved, ensuring efficient heat dissipation performance of electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005069004920000031
    Figure BDA0005069004920000031
  • Figure BDA0005069004920000041
    Figure BDA0005069004920000041
  • Figure BDA0005069004920000051
    Figure BDA0005069004920000051
Patent Text Reader

Abstract

The present invention provides a thermally conductive silicone composition. The composition comprises: (A) an organopolysiloxane comprising an alkenyl group; (B) an organohydrogenpolysiloxane having an average of at least two hydrogen atoms directly bonded to a silicon atom in a molecule; (C) surface-treated diamond particles having a D50 particle size greater than 70 [mu] m; (D) a thermally conductive filler that is not component (C); (E) a silane coupling agent; and (F) a catalyst characterized by an advantageous combination of properties including good flowability and high thermal conductivity upon curing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermally conductive silicone composition, and in particular to a thermally conductive silicone composition exhibiting good fluidity and high thermal conductivity when cured, a preparation method and use thereof. Background Art

[0002] In recent years, as the size of electronic devices has been reduced and the performance has been improved, the demand for heat dissipation compositions has increased. Thermally conductive silicone compositions that exhibit good fluidity and high thermal conductivity are widely used in electronic devices (especially telecommunication and data communication equipment, such as 5G stations, etc.).

[0003] Such a thermally conductive silicone composition can be exemplified by a thermally conductive silicone composition comprising an organopolysiloxane having a vinyl group, an organohydrogenpolysiloxane, a thermally conductive filler, an adhesion imparting agent selected from epoxysilane or alkyl titanate, and a platinum-type catalyst. In order to improve the thermal conductivity of a cured body obtained from such a thermally conductive silicone composition, the composition must be incorporated with a large amount of a thermally conductive filler. However, increasing the amount of such a filler impairs the fluidity of the composition.

[0004] JP 2003301189 A discloses an invention of a heat-dissipating silicone grease composition, and describes the use of a thermally conductive filler having an average particle size falling within the range of 0.1 to 100 μm, and preferably 1 to 20 μm.

[0005] JP 201013563 A discloses an invention of a thermally conductive silicone grease, and states that (A) the thermally conductive inorganic filler preferably has an average particle size falling within the range of 0.1 to 100 μm, particularly 1 to 70 μm. In the examples, B-1: zinc oxide powder (amorphous, average particle size: 1.0 μm), B-2: aluminum oxide powder (spherical, average particle size: 2.0 μm), and B-3: aluminum powder (amorphous, average particle size: 7.0 μm) were used.

[0006] US2018134938 A1 discloses a thermally conductive composition having good thermal conductivity, low viscosity and easy application, comprising: (A) a spherical thermally conductive filler and (B) an alkoxysilane compound or a dimethyl polysiloxane, wherein the spherical thermally conductive filler of component (A) is a mixture prepared with fillers having different average particle sizes in a specific ratio, wherein the mixture is prepared with 30% by mass or more of a spherical thermally conductive filler made of nitride having an average particle size of 50 μm or more.

[0007] However, the thermal conductivity of the above disclosed compositions does not exceed 10 W / (m·K), which cannot meet the increasing demand for heat dissipation performance.

[0008] In view of the above, an object of the present invention is to provide a thermally conductive silicone composition having an advantageous combination of properties including good flowability (greater than 15 g / min at 25°C) and high thermal conductivity (greater than 10 W / (m·K)) when cured. Summary of the invention

[0009] Disclosed herein is a thermally conductive silicone composition comprising:

[0010] (A) an organopolysiloxane containing an alkenyl group;

[0011] (B) an organohydrogenpolysiloxane having an average of at least two hydrogen atoms directly bonded to silicon atoms in the molecule;

[0012] (C)D 50 Surface treated diamond particles with a particle size greater than 70 μm;

[0013] (D) a thermally conductive filler other than component (C);

[0014] (E) a silane coupling agent; and

[0015] (F) Catalyst.

[0016] Also disclosed herein is a method of preparing the thermally conductive silicone composition according to the present invention.

[0017] Also disclosed herein is a cured product of the thermally conductive silicone composition according to the present invention.

[0018] Also disclosed herein is the use of the thermally conductive silicone composition and a cured product of the thermally conductive silicone composition according to the present invention in manufacturing electronic devices.

[0019] Other features and aspects of the subject matter are described in more detail below. DETAILED DESCRIPTION

[0020] It will be appreciated by those skilled in the art that the present invention is merely a description of an exemplary embodiment and is not intended to limit the broader aspects of the present invention. Each aspect so described may be combined with any one or more other aspects unless expressly indicated otherwise. In particular, any feature indicated as preferred or advantageous may be combined with any one or more other features indicated as preferred or advantageous.

[0021] Unless otherwise specified, in the context of the present invention, the terms used should be interpreted according to the following definitions.

[0022] As used herein, the terms "a," "an," "said," and "the" include both singular and plural referents unless otherwise specified.

[0023] As used herein, the terms "comprising," "including," and "including" are synonymous with "comprising," and are inclusive or open-ended and do not exclude additional, unrecited members, elements, or method steps.

[0024] The term "room temperature" as used herein refers to a temperature of about 20°C to about 25°C, preferably about 25°C.

[0025] Unless otherwise specified, recitations of numerical endpoints include all numbers and decimals subsumed within the corresponding ranges, as well as the recited endpoints.

[0026] All references cited in this specification are incorporated herein by reference in their entirety.

[0027] Unless otherwise defined, all terms (including technical and scientific terms) used in the present invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

[0028] In one aspect, the present disclosure generally relates to a thermally conductive silicone composition comprising:

[0029] (A) an organopolysiloxane containing an alkenyl group;

[0030] (B) an organohydrogenpolysiloxane having an average of at least two hydrogen atoms directly bonded to silicon atoms in the molecule;

[0031] (C)D 50 Surface treated diamond particles with a particle size greater than 70 μm;

[0032] (D) a thermally conductive filler other than component (C);

[0033] (E) a silane coupling agent; and

[0034] (F) Catalyst.

[0035] (A) Organopolysiloxane containing alkenyl groups

[0036] According to the present invention, the thermally conductive silicone composition includes (A) an organopolysiloxane including an alkenyl group.

[0037] As used herein, "alkenyl" refers to a straight chain or branched hydrocarbon group ("C 2-40 In some embodiments, an alkenyl group has 2 to 30 carbon atoms (“C 2-30 In some embodiments, an alkenyl group has 2 to 20 carbon atoms (“C 2-20 In some embodiments, an alkenyl group has 2 to 10 carbon atoms (“C 2-10In some embodiments, an alkenyl group has 2 to 9 carbon atoms (“C 2-9 In some embodiments, an alkenyl group has 2 to 8 carbon atoms (“C 2-8 In some embodiments, an alkenyl group has 2 to 7 carbon atoms (“C 2-7 In some embodiments, an alkenyl group has 2 to 6 carbon atoms (“C 2-6 In some embodiments, an alkenyl group has 2 to 5 carbon atoms (“C 2-5 In some embodiments, an alkenyl group has 2 to 4 carbon atoms (“C 2-4 In some embodiments, an alkenyl group has 2 to 3 carbon atoms (“C 2-3 In some embodiments, an alkenyl group has 2 carbon atoms ("C2 alkenyl"). The one or more carbon-carbon double bonds can be internal (such as in 2-butenyl) or terminal (such as in 1-butenyl). 2-4 Examples of alkenyl groups include ethenyl (C2), 1-propenyl (C3), 2-propenyl (C3), 1-butenyl (C4), 2-butenyl (C4), butadienyl (C4), and the like. 2-6 Examples of the alkenyl group include the above-mentioned C 2-4 In some embodiments, alkenyl is an unsubstituted C 1-1, 1-dienyl, 1-hex ... 2-30 In certain embodiments, alkenyl is a substituted C 2-30 Alkenyl.

[0038] In some embodiments, the amount of alkenyl groups is in the range of 0.01 to 10 wt%, and preferably 0.1 to 5 wt%, based on the total weight of the organopolysiloxane. In addition, these alkenyl groups may be bonded to silicon atoms at the ends of the molecular chains, to non-terminal silicon atoms within the molecular chains, or to both types of silicon atoms; although from the perspective of ensuring a good curing rate of the composition and producing favorable physical properties of the cured product, the organopolysiloxane should contain at least alkenyl groups bonded to silicon atoms at the ends of the molecular chains, and preferably alkenyl groups bonded to silicon atoms at both ends of the molecular chains.

[0039] In some embodiments, the 25°C viscosity of component (A) is in the range of 10 to 1000 mPa·s, and preferably 10 to 500 mPa·s. If the 25°C viscosity is within the range defined above, the physical characteristics of the cured silicone rubber can be improved. When component (A) is a mixture of at least two alkenyl-containing organopolysiloxanes, the 25°C viscosity of component (A) refers to the calculated viscosity according to the following modified Gordon-Taylor equation (I), that is, these alkenyl-containing organopolysiloxanes as a whole have a calculated viscosity of 10 to 1000 mPa·s, and preferably 10 to 500 mPa·s, which means: alkenyl-containing organopolysiloxanes whose 25°C viscosity is not within the above range can be used, as long as the calculated viscosity as a whole is within the above range. In the present invention, the calculated viscosity of two or more alkenyl-containing organopolysiloxanes can be calculated according to the following modified Gordon-Taylor equation (I):

[0040] η=W1×η1+W2×η2+...W n ×η n (I)

[0041] wherein W1 is the weight percentage of the first alkenyl-containing organopolysiloxane based on the total weight of the alkenyl-containing organopolysiloxane, η1 is the viscosity of the first alkenyl-containing organopolysiloxane, W2 is the weight percentage of the second alkenyl-containing organopolysiloxane based on the total alkenyl-containing organopolysiloxane, and η2 is the viscosity of the second alkenyl-containing organopolysiloxane; W n is the weight percentage of the nth organopolysiloxane containing alkenyl groups based on the total organopolysiloxane containing alkenyl groups, η n is the viscosity of the nth organopolysiloxane containing an alkenyl group, and η is the calculated viscosity of the mixture of the first to nth organopolysiloxanes containing an alkenyl group.

[0042] There are no particular limitations on the molecular structure of component (A), including but not limited to a linear structure, a cyclic structure, a branched structure, a partially branched linear structure, and a three-dimensional network structure; although preferred are substantially linear diorganopolysiloxanes in which the main chain is formed by repeating diorganosiloxane units and both ends of the molecular chain are terminated with triorganosiloxy groups. In addition, component (A) may be a single polymer having this type of molecular structure, a copolymer having this type of molecular structure, or a mixture of different polymers having this type of molecular structure.

[0043] Specific examples of component (A) include compounds represented by general formulae (i) to (v) shown below.

[0044]

[0045]

[0046] In the above formulas (i) to (v), R each independently represents a substituted or unsubstituted monovalent hydrocarbon group bonded to a silicon atom as described above, but excluding alkenyl; and it is preferably a methyl group or a phenyl group. In formulas (i) and (v), n is an integer from 0 to 5000. In formulas (ii) to (iv), n is an integer from 0 to 5000, m is an integer from 5 to 5000, and n+m ranges from 5 to 10000. In some embodiments, n ranges from as little as 0, 10, 50, 100, 200, 500, as much as 1000, 2000, 5000, or in any range defined between any two of the aforementioned values; and m ranges from 5, 10, 50, 200, or as much as 500, 1000, 2000, 5000, or in any range defined between any two of the aforementioned values. In addition, the range of n+m is as small as 5, 10, 30, 50, 100, 200, 500, or as large as 1000, 2000, 5000, 10000, or in any range defined between any two of the foregoing values, for example, in the range defined between 10 and 10000, and between 1000 and 5000.

[0047] In some embodiments, the unsubstituted or substituted monovalent hydrocarbon groups R in the above formulae (i) to (v) are each independently selected from: a straight chain alkyl group, preferably selected from methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, n-heptadecyl, n-octadecyl, n-nonadecyl and n-eicosyl; a branched chain alkyl group, preferably selected from isopropyl, tert-butyl, isobutyl, 2-methylundecane cyclopentyl, cyclohexyl and cyclododecyl; alkenyl, preferably selected from vinyl, allyl, butenyl, pentenyl and hexenyl; aryl, preferably selected from phenyl, tolyl and xylyl; aralkyl, preferably selected from benzyl, phenethyl and 2-(2,4,6-trimethylphenyl)propyl; and haloalkyl, preferably selected from 3,3,3-trifluoropropyl and 3-chloropropyl; preferably selected from linear alkyl, alkenyl and aryl; and more preferably selected from methyl, ethyl, vinyl and phenyl.

[0048] There is no particular limitation on the molecular weight of component (A), and it is preferably in the range of 3,000 to 20,000 g / mol.

[0049] Component (A) may be used either alone or in combination of two or more different compounds.

[0050] Such an alkenyl group-containing organopolysiloxane used as component (A) can be prepared by using a conventional known method. In a typical preparation method, the alkenyl group-containing organopolysiloxane is prepared by subjecting an organocyclic oligosiloxane and a hexaorganodisiloxane to an equilibrium reaction in the presence of a base or an acid catalyst.

[0051] Examples of commercially available products of component (A) include RH-Vi100E, RH-Vi322, RH-Vi323, and RH-Vi324, which can be obtained from Zhejiang Runhe Chemical New Material Co., Ltd.

[0052] According to the present invention, component (A) is present in an amount of 0.01 to 5% by weight, preferably 0.05 to 3% by weight, based on the total weight of the composition.

[0053] (B) An organohydrogenpolysiloxane having an average of at least two hydrogen atoms directly bonded to silicon atoms in the molecule

[0054] According to the present invention, the thermally conductive silicone composition further comprises (B) an organohydrogenpolysiloxane having an average of at least two hydrogen atoms directly bonded to silicon atoms in the molecule, which acts as a crosslinking agent for component (A) to form a silicone polymer matrix.

[0055] In one embodiment, the organohydrogenpolysiloxane has two or more -Si-H groups in one molecule. The -Si-H groups in component (B) and the alkenyl groups in component (A) are added by a hydrosilylation reaction promoted by the catalyst (F) described below to generate a three-dimensional network structure having a cross-linked structure.

[0056] Component (B) may have an average of at least two, and preferably three or more -Si-H groups per molecule, and these -Si-H groups may be located at the terminal, non-terminal position, or both of the molecular chains.

[0057] In one embodiment, the organohydrogenpolysiloxane is linear or branched, and in a preferred embodiment, the organohydrogenpolysiloxane may be represented by the general formula (vi):

[0058]

[0059] In the above formula (vi), R' independently represents a hydrogen atom or an unsubstituted or substituted monovalent hydrocarbon group other than an aliphatic unsaturated bond, and at least two R' groups are hydrogen atoms. The subscript e represents an integer of 1 or more.

[0060] Suitable examples of the unsubstituted or substituted monovalent hydrocarbon radicals in the general formula (vi) are each independently selected from: straight-chain alkyl groups, preferably selected from methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, n-heptadecyl, n-octadecyl, n-nonadecyl and n-eicosyl; branched-chain alkyl groups, preferably selected from isopropyl, tert-butyl, isobutyl, 2-methylundecyl and 1-hexyl; cyclopentyl, cyclohexyl and cyclododecyl; alkenyl, preferably selected from vinyl, allyl, butenyl, pentenyl and hexenyl; aryl, preferably selected from phenyl, tolyl and xylyl; aralkyl, preferably selected from benzyl, phenethyl and 2-(2,4,6-trimethylphenyl)propyl; and haloalkyl, preferably selected from 3,3,3-trifluoropropyl and 3-chloropropyl; preferably selected from linear alkyl, alkenyl and aryl; and more preferably selected from methyl, ethyl, vinyl and phenyl.

[0061] The functionality content of -Si-H groups in component (B) is preferably in the range of 0.1 to 10.0 mmol / g, more preferably 0.1 to 5.0 mmol / g.

[0062] In a preferred embodiment, the amount of the number of moles of the -Si-H groups contained in the component (B) is preferably 0.1 to 5.0 times the number of moles of the alkenyl groups derived from the component (A).

[0063] Specific examples of component (B) include, but are not limited to, 1,1,3,3-tetramethyldisiloxane, methylhydrogencyclopolysiloxane, a cyclic copolymer of methylhydrogensiloxane and dimethylsiloxane, methylhydrogenpolysiloxane terminated at both ends with trimethylsiloxy groups, a copolymer of dimethylsiloxane and methylhydrogensiloxane terminated at both ends with trimethylsiloxy groups, a dimethylpolysiloxane terminated at both ends with dimethylhydrogensiloxane, a copolymer of dimethylpolysiloxane and methylhydrogensiloxane terminated at both ends with dimethylhydrogensiloxane, a copolymer of methylhydrogensiloxane and diphenylsiloxane terminated at both ends with trimethylsiloxy groups, a copolymer of methylhydrogensiloxane, diphenylsiloxane and dimethylsiloxane terminated at both ends with trimethylsiloxy groups, and a copolymer of methylhydrogensiloxane, dimethylsiloxane and diphenylsiloxane terminated at both ends with dimethylhydrogensiloxane groups.

[0064] Component (B) can be prepared by using conventional known methods. In a typical preparation method, octamethylcyclotetrasiloxane and / or tetramethylcyclodisiloxane, and compounds (e.g., hexamethyldisiloxane) to form terminal groups or compounds incorporating 1,1'-dihydro-2,2',3,3'-tetramethyldisiloxane units are balanced in the presence of a catalyst (e.g., sulfuric acid, trifluoromethanesulfonic acid or methanesulfonic acid) at a temperature of -10°C to 40°C. Commercially available products can also be obtained. Examples of commercially available products of component (B) include RH-H86, RH-H502, RH-H503, which can be obtained from Zhejiang Runhe Chemical New Materials Co., Ltd.

[0065] According to the present invention, component (B) is present in an amount of 0.01 to 5% by weight, preferably 0.05 to 3% by weight, based on the total weight of the composition.

[0066] (C) Surface treated diamond particles

[0067] According to the present invention, the thermally conductive silicone composition comprises (C)D 50 Surface treated diamond particles with a particle size greater than 70 μm.

[0068] In this paper, the “D 50 The “particle size” refers to the median diameter in a volume-based particle size distribution curve obtained by measurement with a laser diffraction particle size analyzer.

[0069] In some embodiments, component (C) has D 50 The particle size is greater than 90 μm, preferably greater than 100 μm. In a preferred embodiment, component (C) has a D 50 The particle size is greater than 70 μm to 200 μm, preferably greater than 90 μm to 200 μm, more preferably greater than 100 μm to 200 μm, even more preferably 110 μm to 150 μm.

[0070] There is no particular restriction on the shape of component (C) used in the present invention. They may have a spherical, tetrahedral, hexahedral, octahedral, polyhedral or irregular shape. In this specification, the term "spherical" refers to a shape in which the entire surface is formed by a convex smooth surface. In diamond particles, the spheroidicity is, for example, 0.5 or greater, preferably 0.55 or greater, and more preferably 0.6 or greater. Spheroidality refers to an index in which the closer the spheroidality is to 1, the closer the index is to a sphere; and when the spheroidality is high, for example, in a polyhedral shape, it increases the contact surface and is therefore easy to dissipate heat; and in addition, when the spheroidality is close to 1, the diamond particles become easy to be dispersed in the silicone polymer matrix. There is no particular restriction on the upper limit of the spheroidality, which is 1.

[0071] According to the present invention, component (C) should have a surface treatment, preferably a silane surface treatment. By surface treating the diamond particles, the diamond particles become easy to conform to the silicon matrix, and a large number of diamond particles become easy to be evenly dispersed in the silicone polymer matrix. The diamond particles are surface treated with a surface treatment agent (e.g., a silane compound, an organic titanium compound, an organic aluminum compound, or a phosphate compound), and preferably with a silane compound.

[0072] In a preferred embodiment, the amount of the surface treatment agent adhered to the diamond particles is, for example, 0.01 wt% to 2 wt%, preferably 0.02 wt% to 1.5 wt%, more preferably 0.03 wt% to 1 wt%, relative to the weight of the diamond particles. If the content of the surface treatment agent is within the above defined range, the diamond particles will have improved compatibility with other thermal particles.

[0073] The silane compound to be used for surface treatment is not particularly limited, and examples thereof include alkoxysilane and chlorosilane; and alkoxysilane is preferred. When the diamond particles are surface-treated with a silane compound, they are easily adapted to the silicon polymer matrix, so that the amount of diamond particles blended in the thermally conductive composition is easily increased.

[0074] Examples of alkoxysilanes include alkoxysilanes having a reactive group and alkoxysilanes having no reactive group. The reactive group of the alkoxysilane having a reactive group is selected from, for example, an epoxy group, a (meth)acryloyl group, an amino group, a vinyl group, a urea group, a mercapto group, and an isocyanate group.

[0075] Examples of alkoxysilanes having an epoxy group include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane. Examples of alkoxysilanes having a (meth)acryloyl group include 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and 3-(meth)acryloxypropyltriethoxysilane. The example of the silane compound with amino group includes: alkoxysilane, such as N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and N-phenyl-3-aminopropyltrimethoxysilane. The example of the silane compound with vinyl group includes vinyltrimethoxysilane and vinyltriethoxysilane. The example of the alkoxysilane with mercapto group includes 3-mercaptopropyltrimethoxysilane and 3-mercaptopropylmethyldimethoxysilane. The example of the alkoxysilane with urea group includes 3-ureapropyltrimethoxysilane. The example of the alkoxysilane with isocyanate group includes 3-isocyanatepropyltriethoxysilane. In addition, examples of alkoxysilanes without reactive groups include: trialkoxysilanes, such as aryl trialkoxysilanes, alkyl trialkoxysilanes; and dialkoxysilanes, such as dialkyldialkoxysilanes and diaryldialkoxysilanes; and among these, trialkoxysilanes such as alkyl trialkoxysilanes are preferred. Examples of alkyl trialkoxysilanes include: alkyl trialkoxysilanes, wherein the carbon number of the alkyl group is about 1 to 10, such as methyl trimethoxysilane, methyl triethoxysilane, n-propyl trimethoxysilane, n-propyl triethoxysilane, n-hexyl trimethoxysilane, n-hexyl triethoxysilane, n-octyl triethoxysilane and n-decyl trimethoxysilane. In addition, examples of aryl trimethoxysilanes include: aryl trimethoxysilanes, wherein the carbon number of the aryl group is about 6 to 10, such as phenyl trimethoxysilane, benzyl trimethoxysilane and tolyl trimethoxysilane. Also, examples of dialkoxysilane include dimethyldimethoxysilane and dimethyldiethoxysilane.As a preferred aspect of the silane compound, a polymeric silane compound is used which is a reaction product of an alkoxysilane having a reactive group and a polyorganosiloxane having a functional group reactive with the reactive group.

[0076] Suitable polymerized silane compounds can be obtained, for example, by mixing alkoxysilanes with reactive groups with polyorganosiloxanes and reacting these substances under heating in the presence of a catalyst (e.g., a platinum-based catalyst, a palladium-based catalyst, or a rhodium-based catalyst). As alkoxysilanes with reactive groups, those listed above can be used; but among the above substances, trialkoxysilanes are preferably used. As alkoxysilanes with reactive groups, silane compounds with (meth)acryloyl or vinyl groups are preferably used, and trialkoxysilanes with (meth)acryloyl groups are more preferably used. When using a silane compound with (meth)acryloyl or vinyl groups, because the silane compound is easily reacted with an organopolysiloxane with a hydrosilyl group (-SiH) described later, a polymerized silane compound can be obtained by a simple method. The polyorganosiloxane with a functional group to be used for the polymerized silane compound can have one functional group, or can have two or more functional groups. In the case of having two or more functional groups, two or more alkoxysilane molecules with reactive groups can be bonded to a polyorganosiloxane molecule. The polyorganosiloxane with functional groups is preferably an organopolysiloxane with hydrosilyl (-SiH). The example of the organopolysiloxane with hydrosilyl (-SiH) includes methylhydrosiloxane-dimethylsiloxane copolymer and methylhydrosiloxane-phenylmethylsiloxane copolymer. These materials may be included in the hydrosilyl on the end, or may not be included. The weight average molecular weight of the polyorganosiloxane with functional groups is preferably 800 to 5000, and more preferably 1500 to 4000. Here, the weight average molecular weight is the value (in terms of polystyrene) converted with polystyrene measured by GPC.

[0077] There is no particular limitation on the method for surface treatment using a silane compound, and it may be a well-known method; and, for example, a wet treatment method, a dry treatment method, or a pretreatment method may be used. In the present invention, among these methods, a wet treatment method is preferred. In the wet treatment method, the surface treatment may be performed, for example, by adding diamond particles to a solution in which a silane compound is dispersed or dissolved, mixing the mixture, and thereafter heat-treating the mixture to bond or adhere the silane compound to the surface of the diamond particles. A dry treatment method is a method for surface treatment without using a solution; and specifically, it is a method in which diamond particles are mixed with a silane compound and stirred by a mixer or the like, and thereafter heat-treated to bond or adhere the silane compound to the surface of the diamond particles.

[0078] Suitable commercially available examples of component (C) are: SD-715, SD-715Q, SD-720 and SD-720Q from FoShan ZhanXun Material Co., Ltd; HFD-A, HFD-B and HFD-C from Henan Huifeng Diamond Co., Ltd.

[0079] In a particularly preferred embodiment, component (C) is present in an amount of 0.01 wt% to 85 wt%, more preferably 0.01 wt% to 60 wt%, based on the total weight of the composition.

[0080] (D) Other thermally conductive fillers

[0081] In some embodiments, the thermally conductive silicone composition may further comprise a conductive filler different from component (C), including but not limited to alumina particles, aluminum nitride particles, fumed silica, precipitated silica, fumed titanium oxide, and combinations thereof, preferably alumina particles, aluminum nitride particles, and combinations thereof.

[0082] In a preferred embodiment, component (D) has D 50 The particle size is at least 0.01 μm but not more than 100 μm, more preferably 0.01 μm to 50 μm.

[0083] In a preferred embodiment, the following combination of substances is used as component (D) in the present invention: 50 Alumina particles having a particle size of 0.01 μm to 5 μm, preferably 0.1 μm to 2 μm, and D 50 Aluminum nitride particles with a particle size of 1 μm to 50 μm, preferably 2 μm to 35 μm.

[0084] There is no particular limitation on the shape of component (D) used in the present invention. They may have a spherical, rod-like, needle-like, disc-like or amorphous shape, preferably a spherical shape.

[0085] Other fillers may be surface treated or non-surface treated. It is preferred to use surface treated particles as component (D) in the present invention to increase compatibility with component (C) in the silicone polymer matrix.

[0086] Suitable commercially available examples of component (D) include alumina particles from: AN5, AN20 and AN30, which are from Suzhou Ginet New Material Technology Co., Ltd.; AA04, which is from Sumitomo Chemical; NSM-1 and BAK-2, which are from Bestry Performance Materials Co., Ltd.; DAM-03, which is from Denka Corporation.

[0087] In a particularly preferred embodiment, component (D) is present in an amount of 0.01 wt% to 85 wt%, more preferably 20 wt% to 70 wt%, based on the total weight of the composition.

[0088] (E) Silane coupling agent

[0089] According to the present invention, the thermally conductive silicone composition includes (E) a silane coupling agent.

[0090] Suitable silane coupling agents that can be used in the present invention include, but are not limited to, 3-methacryloxypropyltrimethoxysilane, methyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, tetraethoxysilane, vinyltriethoxysilane, methyltris(methylethylketoxime)silane, vinyltriacetoxysilane, ethyl orthosilicate, and the like.

[0091] Commercially available examples of silane coupling agents include: 3-methacryloxypropyltrimethoxysilane, methyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, which are from Sinopharm; and 9116 from Evonik.

[0092] According to the present invention, component (E) is present in an amount of 0.1 wt % to 5 wt %, preferably 0.1 wt % to 3 wt %, based on the total weight of the composition. If the amount falls within this range, the adhesive strength of the cured product obtained by the composition of the present invention can be improved.

[0093] (F) catalyst

[0094] According to the present invention, the thermally conductive silicone composition comprises (F) a catalyst for accelerating the curing process, preferably a platinum-based curing catalyst.

[0095] Component (F) is a catalyst for promoting the addition reaction of the alkenyl group derived from component (A) and the -Si-H group derived from component (B), and a catalyst known as a catalyst used in a hydrosilylation reaction can be used.

[0096] Specific examples thereof include: simple platinum group metals such as platinum (including platinum black), rhodium and palladium; platinum chloride, chloroplatinic acid and chloroplatinates such as H2PtCl4·nH2O, H2PtCl6·nH2O, NaHPtCl6·nH2O, KaHPtCl6·nH2O, Na2PtCl6·H2O, K2PtCl4·nH2O, PtCl4·nH2O, PtCl2 and Na2HPtCl4·nH2O (these wherein n is an integer of 0 to 6, preferably alcohol-modified chloroplatinic acid); a complex of chloroplatinic acid and an olefin; obtained by loading a platinum group metal (e.g., platinum black and palladium) on a carrier (e.g., alumina, silica, or carbon); a rhodium-olefin complex, chlorotris(triphenylphosphine)rhodium (Wilkinson catalyst); and a complex of platinum chloride, chloroplatinic acid or a chloroplatinate and a vinyl-containing siloxane (particularly a vinyl-containing cyclic siloxane) can be used.

[0097] Suitable commercially available examples of catalysts include: CATALYST 512, which is available from Evonik; and CAT-50, which is available from Avantor.

[0098] According to the present invention, component (F) is present in an amount of 1 ppm by weight to 1000 ppm by weight, preferably 1 ppm by weight to 500 ppm by weight, based on the total weight of the composition.

[0099] (G) additive

[0100] In some embodiments, the thermally conductive silicone composition may further optionally include additives selected from inhibitors, pigments, dyes, fluorescent dyes, heat-resistant additives, flame retardants, plasticizers, adhesion-imparting agents, and combinations thereof, provided that the inclusion of these additives does not impair the purpose of the present invention; in particular, curing reaction inhibitors.

[0101] Suitable examples of inhibitors used in the present invention include, but are not limited to, acetylene-based compounds such as 2-methyl-3-butyn-2-ol, 2-phenyl-3-butyn-2-ol, or 1-ethynyl-1-cyclohexanol; ene-in compounds such as 3-methyl-3-penten-1-in, 3,5-dimethyl-3-hexen-1-in; hydrazine-based compounds; phosphine-based compounds; or thiol-based compounds to adjust the curing rate of the composition, thereby improving fluidity and processability.

[0102] Suitable commercially available examples of inhibitors include: Inhibitor MVC from Evonik, and 3,5-dimethyl-1-hexyn-3-ol from Sigma-Aldrich Company.

[0103] In those instances where the compositions of the present invention include an inhibitor, there is no particular limitation on the amount of the inhibitor, although amounts in the range of 0.0001 to 1.0 wt % based on the total weight of the composition are preferred.

[0104] In a particularly preferred embodiment, the thermally conductive silicone composition comprises, based on the total weight of the composition:

[0105] (A) 0.01 to 5 wt%, preferably 0.05 to 3 wt% of an organopolysiloxane containing an alkenyl group;

[0106] (B) 0.01 to 5 wt%, preferably 0.05 to 3 wt% of an organohydrogenpolysiloxane having an average of at least two hydrogen atoms directly bonded to silicon in its molecules;

[0107] (C) 0.01 to 85 wt%, more preferably 0.01 to 60 wt% of D 50 Surface treated diamond particles with a particle size greater than 70 μm;

[0108] (D) 0.01 to 85 wt %, preferably 20 to 70 wt % of a thermally conductive filler other than component (C);

[0109] (E) 0.1 wt % to 5 wt %, preferably 0.1 wt % to 3 wt % of a silane coupling agent; and

[0110] (F) 1 wt ppm to 1000 wt ppm, preferably 1 wt ppm to 500 wt ppm of a catalyst; and

[0111] (G) 0 to 1.0 wt % of additives.

[0112] Another aspect of the present invention relates to a method of preparing a thermally conductive silicone composition by mixing the components simultaneously at room temperature, for example for at least one hour, preferably for at least two hours.

[0113] The thermally conductive silicone composition of the present invention has good fluidity at a thermally conductive filler loading of greater than 80%, for example, a flow rate of greater than 15 g / min, preferably greater than 18 g / min, and more preferably greater than 20 g / min, wherein the flow rate is defined as the weight of the adhesive composition dispensed per minute at a pressure of 90 psi using a dispenser Nordson Ultimus-I equipped with a 30 cc plastic tube, wherein the 30 cc plastic tube has a nozzle with a diameter of 2.54 ± 5% mm. Such a flow rate (especially a flow rate of greater than 15 g / min) ensures that the nozzle of a conventional adhesive dispenser will not be clogged by the adhesive composition after mixing.

[0114] In a preferred embodiment, the thermally conductive silicone composition can be cured at room temperature in no more than 7 days. Curing can be accelerated by heating, for example by heating at a temperature of from 60°C to 200°C for 30 minutes to 2 hours.

[0115] In the present invention, the thermally conductive silicone composition can be applied to the desired substrate by any convenient technique. It can be applied cold or warm, if desired. It can be applied by extruding it onto a substrate or applying it onto a substrate or other mechanical application methods such as a caulking gun. Typically, the thermally conductive silicone composition of the present invention is applied to one surface of a pair of substrates, which are then brought into contact with each other to bond together. After application, the adhesive composition of the present invention cures at room temperature, optionally subsequently cured at an elevated temperature.

[0116] In another aspect of the present invention, there is provided an article comprising a first substrate, a cured adhesive and a second substrate, wherein the second substrate is bonded to the first substrate via the cured adhesive, the cured adhesive comprising a cured product obtained from the curable adhesive composition according to any one of the preceding claims.

[0117] The first substrate and / or the second substrate may be of a single material and a single layer, or may comprise multiple layers of the same or different materials. These layers may be connected or discontinuous.

[0118] The substrates of the articles described herein can have a variety of properties, including rigidity (e.g., a rigid substrate (i.e., the substrate cannot be bent by an individual using two hands, or the substrate breaks if an attempt is made to bend the substrate using two hands)), flexibility (e.g., a flexible substrate (i.e., the substrate can be bent with no more than two hands)), porosity, conductivity, lack of conductivity, and combinations thereof.

[0119] The substrate of the article can be in a variety of forms, including, for example, fibers, threads, yarns, woven fabrics, nonwovens, films (e.g., polymer films, metallized polymer films, continuous films, discontinuous films, and combinations thereof), foils (e.g., metal foils), sheets (e.g., metal sheets, polymer sheets, continuous sheets, discontinuous sheets, and combinations thereof), and combinations thereof.

[0120] The substrate materials used in the present invention include, for example, polymers (e.g., polycarbonate, ABS resin (acrylonitrile-butadiene-styrene resin), liquid crystal polymers, polyolefins (e.g., polypropylene, polyethylene, low-density polyethylene, linear low-density polyethylene, high-density polyethylene, polypropylene, and oriented polypropylene, copolymers of polyolefins and other comonomers), polyether terephthalate, ethylene-vinyl acetate, ethylene-methacrylic acid ionomer, ethylene-vinyl-alcohol, polyesters (e.g., polyethylene terephthalate, polycarbonate), polyamides (e.g., nylon-6 and nylon-6,6), polyvinyl chloride, polyvinylidene chloride, cellulose, The present invention relates to a polymer composite material (e.g., cellulosics, polystyrene, and epoxy resin), a polymer composite material (e.g., a composite material of a polymer and a metal, cellulose, glass, a polymer, and a combination thereof), a metal (aluminum, copper, zinc, lead, gold, silver, platinum, and magnesium, and a metal alloy, such as steel (e.g., stainless steel), tin, brass, and magnesium and aluminum alloys), a carbon-fiber composite material, other fiber-based composite materials, graphene, fillers, glass (e.g., alkali metal-aluminosilicate tempered glass and borosilicate glass), quartz, boron nitride, gallium nitride, sapphire, silicon, carbide, ceramic, and a combination thereof); preferably, it is a liquid crystal polymer, glass, and a combination thereof.

[0121] The cured product of the thermally conductive silicone composition of the present invention has a thermal conductivity measured according to ASTM-D5470 of greater than 10 W / (m·K), preferably greater than 14 W / (m·K).

[0122] Another related aspect of the present invention relates to the use of the thermally conductive silicone composition according to the present invention and the cured product of the thermally conductive silicone composition in the manufacture of electronic devices (especially telecommunication and data communication equipment, such as 5G stations, etc.).

[0123] Exemplary electronic devices include: computers and computer equipment, such as telecommunications and data communications equipment, such as 5G stations, etc.; printers, fax machines, scanners, keyboards, etc.; medical sensors; automotive sensors, etc.; wearable electronic devices (e.g., watches and glasses), handheld electronic devices (e.g., phones (e.g., cellular phones and cellular smartphones)), cameras, tablets, e-readers, monitors (e.g., monitors used in hospitals and by health care workers, athletes and individuals), watches, calculators, mice, touchpads and joysticks), computers (e.g., desktop and laptop computers), computer monitors, televisions, media players, household appliances (e.g., refrigerators, washing machines, dryers, ovens and microwave ovens), light bulbs (e.g., incandescent lamps, light emitting diodes and fluorescent lamps), and articles including visible transparent or transparent components, glass housing structures, protective transparent covers for displays or other optical components.

[0124] According to the invention, it is preferred that the embodiments identified above as preferred or more preferred are used for the use of the thermally conductive silicone composition of the invention, wherein preferably two or more of the aspects or corresponding features described for the thermally conductive silicone composition are combined with one another.

[0125] Example

[0126] The following examples are intended to help those skilled in the art better understand and practice the present invention. The scope of the present invention is not limited by the examples, but by the appended claims. All parts and percentages are based on weight unless otherwise indicated.

[0127] Raw materials:

[0128] Component (A)

[0129] Component a: RH-Vi100E is a vinyl terminated polydimethylsiloxane having a viscosity of 85 to 115 mPa·s, prepared by Zhejiang Runhe Chemical New Materials Co., Ltd.

[0130] Component (B)

[0131] Component b: RH-H86 is a methyl-terminated hydrogen-branched silicone oil, which is prepared by Zhejiang Runhe Chemical New Materials Co., Ltd.

[0132] Component (C)

[0133] Component c-1: SD-715Q-70 is a synthetic diamond particle treated with silane (D 50 =70 μm), which was produced by FoShanZhanXun Material Co., Ltd.

[0134] Component c-2: SD-715Q-110 is a synthetic diamond particle treated with silane (D 50 =110 μm), which was produced by FoShan ZhanXun Material Co., Ltd.

[0135] Component c-3: SD-715Q-120 is a synthetic diamond particle treated with silane (D 50 =120 μm), which was produced by FoShan ZhanXun Material Co., Ltd.

[0136] Component c-4: SD-715Q-130 is a synthetic diamond particle treated with silane (D 50 =130 μm), which was produced by FoShan ZhanXun Material Co., Ltd.

[0137] Component c-5: SD-715-130 is a synthetic diamond particle without surface treatment (D 50 =130 μm), which was produced by FoShan ZhanXun Material Co., Ltd.

[0138] Component (D)

[0139] Component d-1: AN20 is aluminum nitride powder (D 50 =15 to 25 μm), which was produced by Suzhou Jinyi New Materials Technology Co., Ltd.

[0140] Component d-2: AA04 is aluminum oxide powder (D 50 =0.4 μm), which was produced by Sumitomo Chemical.

[0141] Component (E)

[0142] Component e: 9116 is methyltrimethoxysilane, which is produced by Evonik.

[0143] Component (F)

[0144] Component f: CATALYST 512 is a divinyltetramethyldisiloxane complex with 2% by weight of platinum, produced by Evonik.

[0145] Component (G)

[0146] Component g: Inhibitor MVC is a silicone-based inhibitor produced by Evonik.

[0147] Test method:

[0148] Flow rate:

[0149] The flow rate of the thermally conductive silicone composition of the present invention and the comparative sample was measured by a dispenser (Nordson Ultimus TM -I) test. The dispenser includes a 30cc plastic tube, wherein the 30cc plastic tube has a nozzle with a diameter of 2.54±5% mm; and the tube is connected to a pressurizing unit. During the test, the sample is dispensed into a balance tray under a pressure of 90psi within 1 minute. The weight of the sample dispensed within 1 minute is measured and recorded as the flow rate value in Table 1. A larger flow rate value indicates that the thermally conductive silicone composition has greater fluidity and better handling characteristics. A flow rate greater than 15g / min may be acceptable.

[0150] Thermal Conductivity:

[0151] The thermally conductive silicone compositions of the present invention and the comparative example were cured at 125° C. for 1 hour. The thermal conductivity of the cured sample of the present invention was tested by LW 9389 manufactured by Longwin at a temperature of 80° C. and a pressure of 40 psi according to ASTM-D5470. A thermal conductivity greater than 10 W / (m·K) may be acceptable.

[0152] Examples 1 to 3 (Ex. 1 to Ex. 3) and Comparative Examples 1 to 3 (CEx. 1 to CEx. 3)

[0153] The thermally conductive silicone adhesive compositions of the present invention and the comparison were formed by mixing the components in weight percentages listed in Table 1 in a 2-liter planetary mixer (manufactured by Rose (Wuxi) Equipment Co., LTD.) at room temperature for 2 hours, and then cooled to room temperature. Each property was tested using the above method, and the evaluation results are shown in Table 1 as follows.

[0154] Table 1.

[0155]

[0156] As can be seen from Table 1, the thermally conductive silicone adhesive of the present invention (Ex. 1 to Ex. 3) exhibits good fluidity and high thermal conductivity when cured. However, in the case where the components of the present invention are not used as in Comparative Examples 1 to 3 (CEx. 1 to CEx. 3), they exhibit unsatisfactory flow rates compared to the thermally conductive silicone composition of the present invention, indicating that such adhesive compositions can easily cause clogging of the nozzles of conventional adhesive dispensers.

[0157] Although some preferred embodiments have been described, many modifications and variations are possible in light of the above teachings. It is therefore to be understood that the invention may be practiced otherwise than as specifically described without departing from the scope of the appended claims.

Claims

1. A thermally conductive silicone composition comprising: (A) an organopolysiloxane containing an alkenyl group; (B) an organohydrogenpolysiloxane having an average of at least two hydrogen atoms directly bonded to silicon atoms in the molecule; (C)D 50 Surface treated diamond particles with a particle size greater than 70 μm; (D) a thermally conductive filler other than component (C); (E) a silane coupling agent; and (F) Catalyst.

2. The thermally conductive silicone composition according to claim 1, wherein the component (A) is represented by any one of the general formulas (i) to (v) shown below: wherein in each formula, R represents a substituted or unsubstituted monovalent hydrocarbon group other than an alkenyl group; in formulas (i) and (v), n is an integer from 0 to 5000; and in formulas (ii) and (iv), n is an integer from 0 to 5000, m is an integer from 5 to 5000, and n+m ranges from 5 to 10000. 3 . The thermally conductive silicone composition according to claim 1 , wherein the component (A) has a viscosity at 25° C. of 10 to 1000 mPa·s, and preferably 10 to 500 mPa·s.

4. The thermally conductive silicone composition according to any one of the preceding claims, wherein the component (B) is represented by the general formula (vi): wherein R' independently represents a hydrogen atom or an unsubstituted or substituted monovalent hydrocarbon group other than an aliphatic unsaturated bond, at least two R' groups are hydrogen atoms, and e represents an integer of 1 or greater.

5. A thermally conductive silicone composition according to any one of the preceding claims, wherein the component (C) has a D 50 The particle size is greater than 90 μm, preferably greater than 100 μm, more preferably greater than 100 μm to 200 μm, even more preferably 110 μm to 150 μm.

6. The thermally conductive silicone composition according to any one of the preceding claims, wherein the component (D) is selected from the group consisting of aluminum oxide particles, aluminum nitride particles, fumed silica, precipitated silica, fumed titanium oxide, and combinations thereof.

7. The thermally conductive silicone composition according to claim 6, wherein the component (D) has a D 50 The particle size is at least 0.01 μm but not more than 100 μm, more preferably 0.01 μm to 50 μm.

8. The thermally conductive silicone composition according to claim 6, wherein the component (D) is a combination of the following substances: 50 Alumina particles having a particle size of 0.01 μm to 5 μm, preferably 0.1 μm to 2 μm, and D 50 Aluminum nitride particles with a particle size of 1 μm to 50 μm, preferably 2 μm to 35 μm.

9. The thermally conductive silicone composition according to any one of the preceding claims, wherein the component (A) is present in an amount of 0.01 to 5 wt%, preferably 0.05 to 3 wt%, based on the total weight of the composition.

10. The thermally conductive silicone composition according to any one of the preceding claims, wherein the component (B) is present in an amount of 0.01 to 5 wt%, preferably 0.05 to 3 wt%, based on the total weight of the composition.

11. The thermally conductive silicone composition according to any one of the preceding claims, wherein the component (C) is present in an amount of 0.01 to 85 wt%, more preferably 0.01 to 60 wt%, based on the total weight of the composition.

12. The thermally conductive silicone composition according to any one of the preceding claims, wherein the component (D) is present in an amount of 0.01 to 85 wt%, preferably 20 to 70 wt%, based on the total weight of the composition.

13. The thermally conductive silicone composition according to any one of the preceding claims, wherein the component (E) is present in an amount of 0.1 to 5 wt%, preferably 0.1 to 3 wt%, based on the total weight of the composition.

14. The thermally conductive silicone composition according to any one of the preceding claims, wherein the component (F) is present in an amount of 1 to 1000 ppm by weight, preferably 1 to 500 ppm by weight, based on the total weight of the composition.

15. The thermally conductive silicone composition according to any one of the preceding claims, wherein the composition further comprises component (G) at least one additive selected from inhibitors, pigments, dyes, fluorescent dyes, heat resistant additives, flame retardants, plasticizers, adhesion imparting agents, and combinations thereof.

16. A method for preparing a thermally conductive silicone composition according to any one of the preceding claims, comprising the step of mixing the components simultaneously at room temperature.

17. A cured product of the thermally conductive silicone composition according to any one of claims 1 to 15.

18. Use of the thermally conductive silicone composition according to any one of claims 1 to 15 or the cured product according to claim 17 in manufacturing electronic devices.

Citation Information

Patent Citations

  • Heat-dissipating silicone grease composition

    JP2003301189A

  • Thermally conductive silicone grease

    JP2010013563A

  • Thermally conductive composition

    US20180134938A1

Cited By

  • One-component curable high thermal conductivity silicone polymers, their preparation methods and products

    CN123107377A