Molding method, optical film, cholesteric liquid crystal layer, optical laminate, and method for producing curved optical functional layer
By using a cholesteric liquid crystal layer and a low-retard film in a virtual reality display device, combined with Gaussian curvature mold and elliptical cutting technology, the phase difference problem caused by curved surface shape formation is solved, and the correct Ghost suppression and image clarity improvement of optical films in virtual reality display devices.
Patent Information
- Application Number
- CN202380029928.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-22
- Filing Date
- 2023-04-12
- Publication Date
- 2024-11-22
AI Technical Summary
In a virtual reality display device, when the cholesteric liquid crystal layer is formed into a curved surface shape, local phase difference occurs, resulting in unnecessary transmission of light, and increasing heavy shadow (light leakage).
By forming the cholesteric liquid crystal layer and the low-retardation film, the molding is performed by selective stretching, and the phase difference is given in the plane in advance to offset the local phase difference when forming a curved surface shape. The Gaussian curvature is not allowed to be used to be positive. The spread surface mold and elliptical cutting method control the in-plane delay within a certain range to reduce phase difference.
It effectively suppresses the ghosting of the optical film in the virtual reality display device, improves the clarity and wearability of the image, and reduces unnecessary light leakage.
Smart Images

Figure CN119013589A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a forming method, an optical film, a cholesteric liquid crystal layer, an optical laminate and a method for manufacturing a curved optical functional layer. Background Art
[0002] A virtual reality display device is a display device that allows users to wear a dedicated headset on their head and visually recognize images displayed through a composite lens, thereby providing a sense of presence as if they have entered a virtual world.
[0003] A virtual reality display device generally includes an image display panel and a Fresnel lens. However, since the distance between the image display panel and the Fresnel lens is large, there is a problem that the headset becomes thicker and the wearability is poor.
[0004] Therefore, as described in Patent Documents 1 and 2, a lens structure of a composite lens called a pancake lens (reciprocating optical system, folding optical system) is proposed, which has an image display panel, a reflective polarizer and a half-reflective mirror. The overall thickness of the headset is reduced by making the light emitted from the image display panel reciprocate between the reflective polarizer and the half-reflective mirror.
[0005] Here, the reflective polarizer is a polarizer having a function of reflecting one polarized light in the incident light and transmitting the other polarized light. The reflected light and the transmitted light generated by the reflective polarizer are in polarization states orthogonal to each other.
[0006] Here, mutually orthogonal polarization states refer to polarization states located at opposite diameters on the Poincare sphere, for example, mutually orthogonal linear polarized light, and right circularly polarized light (right-handed circularly polarized light) and left circularly polarized light (left-handed circularly polarized light) correspond thereto.
[0007] As a reflective linear polarizer in which transmitted light and reflected light become linearly polarized light, for example, a film obtained by stretching a dielectric multilayer film and a wire grid polarizer are known. Also, as a reflective circular polarizer in which transmitted light and reflected light become circularly polarized light, for example, a film having a light reflecting layer (cholesteric liquid crystal layer) in which a cholesteric liquid crystal phase is fixed is known.
[0008] Previous technical literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application No. 2020-519964
[0011] Patent Document 2: U.S. Patent No. 10394040
[0012] Patent document 1 discloses a composite lens of a pancake lens structure, which uses a reflective linear polarizer as a reflective polarizer and includes an image display panel, a reflective linear polarizer, and a half mirror in sequence. When the image display panel, the reflective polarizer, and the half mirror are included in sequence, the reflective polarizer needs to have a concave mirror effect for light incident from the half mirror side. In order to make the reflective linear polarizer have a concave mirror effect, a structure in which the reflective linear polarizer is formed into a curved shape is proposed.
[0013] In addition, Patent Document 2 discloses a composite lens of a pancake lens structure, which uses a reflective linear polarizer as a reflective polarizer and includes an image display panel, a half mirror, and a reflective linear polarizer in sequence. Patent Document 2 proposes a structure in which both the half mirror and the reflective polarizer are curved to improve the image curvature. In this case, the reflective polarizer needs to function as a convex mirror.
[0014] Furthermore, as described above, as a reflective polarizer, a cholesteric liquid crystal layer as a reflective circular polarizer can also be used.
[0015] As is known to all, the cholesteric liquid crystal layer has a spiral structure in which liquid crystal compounds are stacked in a spiral rotation, and has a structure in which the liquid crystal compounds are stacked in a spiral rotation (360° rotation) with a spiral pitch of one and multiple pitches of the liquid crystal compounds are stacked.
[0016] The cholesteric liquid crystal layer selectively reflects a predetermined circularly polarized light in a predetermined wavelength band and transmits other light. Therefore, such a cholesteric liquid crystal layer can be preferably used as a reflective circular polarizer in a pancake lens.
[0017] The cholesteric liquid crystal layer has substantially no phase difference, that is, the in-plane retardation of the cholesteric liquid crystal layer is substantially zero.
[0018] However, according to the research of the present inventors, it is known that if a reflective polarizer using a cholesteric liquid crystal layer is formed into a curved shape as described in Patent Documents 1 and 2, a part of the helical axis in the plane changes, resulting in a phase difference.
[0019] A cholesteric liquid crystal layer having a phase difference cannot properly reflect and transmit incident light. Therefore, if such a cholesteric liquid crystal layer is used in a pancake lens constituting a virtual reality display device, light is transmitted unnecessarily, and unnecessary images, i.e., so-called ghosting (light leakage), are observed.
[0020] The present invention is completed in view of the above-mentioned problems. The problem to be solved by the present invention is to provide a molding method, an optical film, a cholesteric liquid crystal layer, an optical laminate and a method for producing a curved optical functional layer. The molding method can obtain an optical film that can suppress the occurrence of ghosting when used in a virtual reality display device, for example. Summary of the invention
[0021] Means for solving technical problems
[0022] As a result of intensive research, the present inventors have found that when an optical film having a curved shape is produced by forming a cholesteric liquid crystal layer and a low retardation film (zero retardation film), the formation is performed by selectively stretching the center, thereby suppressing the occurrence of local phase difference caused by the forming.
[0023] Furthermore, as a result of intensive studies, the present inventors have found that by providing a phase difference in a predetermined pattern in advance in a surface of a cholesteric liquid crystal layer, it is possible to cancel out the occurrence of a local phase difference when the layer is formed into a curved shape.
[0024] That is, it was found that the above-mentioned problems can be solved by the following configuration.
[0025] [1] A forming method, which is a forming method of an optical film, comprising the following steps:
[0026] A heating process for heating the optical film;
[0027] A forming step of pressing the optical film onto a mold and deforming the optical film along the shape of the mold; and
[0028] Cutting process, cutting optical film,
[0029] The heating step is a step of heating the optical film by irradiating infrared rays, and the irradiation amount of the infrared rays has a distribution within the surface of the optical film.
[0030] [2] The forming method according to [1], wherein:
[0031] The mold is a concave non-developable surface with positive Gaussian curvature. When the position of the optical film in the plane is projected onto the mold from the normal direction of the main surface of the optical film,
[0032] The amount of infrared light irradiating the optical film at the apex of the concave surface is greater than the amount of infrared light irradiating the optical film at the end of the concave surface.
[0033] [3] A forming method, which is a forming method of an optical film comprising the following steps:
[0034] A heating process for heating the optical film;
[0035] A forming step of pressing the optical film onto a mold and deforming the optical film along the shape of the mold; and
[0036] Cutting process, cutting optical film,
[0037] The surface of the mold in contact with the optical film is a concave surface with a positive Gaussian curvature and a non-developable surface, and the outer peripheral shape is an ellipse.
[0038] The cut shape in the cutting step is an ellipse, and the major axis of the ellipse outer peripheral shape of the optical film cut out by the cutting is greater than 50% and less than 95% of the major axis of the ellipse outer peripheral shape of the mold.
[0039] [4] A forming method, which is a forming method of an optical film comprising the following steps:
[0040] A heating process for heating the optical film;
[0041] A forming step of pressing the optical film onto a mold and deforming the optical film along the shape of the mold; and
[0042] Cutting process, cutting optical film,
[0043] In the heating step, the region of the optical film in contact with the mold is heated to a temperature higher than the glass transition temperature Tg of the optical film.
[0044] In the molding step, immediately after the optical film comes into contact with the mold, the pressing of the optical film against the mold is controlled so that the temperature of the region of the optical film in contact with the mold becomes lower than the glass transition temperature Tg.
[0045] [5] A forming method, which is a forming method of an optical film comprising the following steps:
[0046] A heating process is used to heat the mold;
[0047] A forming step of pressing a heated mold onto the optical film and deforming the optical film along the shape of the mold; and
[0048] Cutting process, cutting optical film,
[0049] The mold is a convex non-developable surface with positive Gaussian curvature,
[0050] In the molding step, the convex apex of the mold is pressed against the center of the optical film.
[0051] [6] The forming method according to [5], wherein:
[0052] The cut shape of the optical film in the cutting process is an ellipse.
[0053] In the molding step, the optical film is pressed against the mold in a state where the position on the oval line forming the cut shape is restricted.
[0054] [7] A cholesteric liquid crystal layer, wherein:
[0055] The cholesteric liquid crystal layer has a phase difference region in which the phase difference increases from the center to the outside.
[0056] In the phase difference region, the slow axis direction at one point in the phase difference region is orthogonal to the direction from the center toward the one point.
[0057] [8] An optical layered body comprising a plurality of cholesteric liquid crystal layers according to [7].
[0058] [9] The optical laminate according to [8], which is formed by alternately laminating cholesteric liquid crystal layers formed using a rod-like liquid crystal compound and cholesteric liquid crystal layers formed using a discotic liquid crystal compound.
[0059]
[10] A method for manufacturing a curved optical functional layer, comprising:
[0060] A cholesteric liquid crystal layer manufacturing process, manufacturing the cholesteric liquid crystal layer described in [7]; and
[0061] In the forming step, curved surface forming is performed so as to eliminate the phase difference of the cholesteric liquid crystal layer.
[0062]
[11] The method for producing a curved optically functional layer according to
[10] , wherein:
[0063] In the forming step, the cholesteric liquid crystal layer is placed on a forming mold and deformed along the concave forming surface so that the bottom of the concave forming surface of the forming mold having the concave forming surface coincides with the center of the cholesteric liquid crystal layer.
[0064]
[12] An optical film having a non-developable surface with a positive Gaussian curvature, wherein:
[0065] The optical film is a cholesteric liquid crystal layer.
[0066] The evaluation wavelength of the in-plane retardation is a wavelength obtained by subtracting 20 nm from the half-value wavelength on the shorter side than the selective reflection center wavelength on the cholesteric liquid crystal layer.
[0067] The in-plane retardation A of the cholesteric liquid crystal layer at the central evaluation wavelength is less than a value of 2% of the evaluation wavelength, and
[0068] The in-plane retardation B of the cholesteric liquid crystal layer at the evaluation wavelength in the outer edge portion is less than 2% of the evaluation wavelength.
[0069]
[13] An optical film having a non-developable surface with positive Gaussian curvature, wherein:
[0070] Optical film does not have selective reflection properties.
[0071] The in-plane retardation A of the optical film at a central wavelength of 550 nm is less than 11 nm, and
[0072] The in-plane retardation B of the optical film at a wavelength of 550 nm in the outer edge portion is less than 11 nm.
[0073]
[14] The optical film according to
[12] or
[13] , wherein the outer peripheral shape is an ellipse.
[0074] Effects of the Invention
[0075] According to the present invention, a forming method, an optical film, a cholesteric liquid crystal layer, an optical laminate, and a method for producing a curved optical functional layer can be provided. The forming method can obtain an optical film that can suppress ghosting when used in a virtual reality display device, for example. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] Figure 1 This is an example of a virtual reality display device that can use the optical film according to the first embodiment of the present invention, and shows an example of light rays of a main image.
[0077] Figure 2 This is an example of a virtual reality display device that can use the optical film according to the first embodiment of the present invention, and shows an example of light rays of double images.
[0078] Figure 3 This is a schematic diagram showing an example of a laminated optical body including the optical film according to the first embodiment of the present invention.
[0079] Figure 4 This is a schematic diagram showing an example of the optical film according to the first embodiment of the present invention.
[0080] Figure 5 This is a schematic diagram of an exposure mask.
[0081] Figure 6 This is a schematic diagram for explaining the effects of the first embodiment of the present invention.
[0082] Figure 7 This is a conceptual diagram showing an example of a cholesteric liquid crystal layer.
[0083] Figure 8 This is a conceptual diagram showing an example of a view of a part of the liquid crystal compound of the cholesteric liquid crystal layer according to the second embodiment of the present invention as viewed from the helical axis direction.
[0084] Fig. 9 This is a diagram showing a part of a plurality of liquid crystal compounds twistedly aligned along the helical axis in the cholesteric liquid crystal layer according to the second embodiment of the present invention, as viewed from the helical axis direction.
[0085] Fig.10 This is a diagram conceptually showing the existence probability of the liquid crystal compound observed from the helical axis direction in the cholesteric liquid crystal layer according to the second embodiment of the present invention.
[0086] Fig.11 It is a schematic diagram of an exposure mask used when producing a cholesteric liquid crystal layer according to the second embodiment of the present invention.
[0087] Fig.12 This is a conceptual diagram showing the slow axis of each region of the cholesteric liquid crystal layer according to the second embodiment of the present invention. DETAILED DESCRIPTION
[0088] Hereinafter, the present invention will be described in detail.
[0089] The description of the constituent elements described below is made based on representative embodiments of the present invention, but the present invention is not limited to these embodiments.
[0090] In addition, in this specification, the numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0091] Furthermore, in this specification, the terms "parallel" and "orthogonal" do not mean parallel or orthogonal in a strict sense, but rather mean parallel or orthogonal within a range of ±5°.
[0092] Furthermore, in this specification, the liquid crystal composition and the liquid crystal compound are concepts that also include substances that no longer exhibit liquid crystallinity due to curing or the like.
[0093] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. The description of the constituent elements described below is sometimes completed based on representative embodiments and specific examples, but the present invention is not limited to such embodiments. In addition, in this specification, the numerical range represented by "to" refers to the range including the numerical values described before and after "to" as the lower limit and upper limit.
[0094] In this specification, "orthogonal" is set to mean 90°±10° (preferably 90°±5°), not 90° in a strict sense. Also, "parallel" is set to mean 0°±10° (preferably 0°±5°), not 0° in a strict sense. Furthermore, "45°" is set to mean 45°±10° (preferably 45°±5°), not 45° in a strict sense.
[0095] However, in the expression of polarization, "polarization states orthogonal to each other" refers to polarization states that are located at opposite diameters from each other on the Poincaré sphere, for example, linear polarized light and right-handed circularly polarized light (right circularly polarized light) and left-handed circularly polarized light (left circularly polarized light) that are orthogonal to each other as described above, corresponding to them.
[0096] In this specification, the "absorption axis" refers to the polarization direction in which the absorbance in the plane becomes the maximum when incident linear polarized light. In addition, the "reflection axis" refers to the polarization direction in which the reflectivity in the plane becomes the maximum when incident linear polarized light. In addition, the "transmission axis" refers to the direction in the plane that is orthogonal to the absorption axis or the reflection axis. Furthermore, the "slow axis" refers to the direction in which the refractive index in the plane becomes the maximum.
[0097] In this specification, unless otherwise specified, phase difference refers to in-plane retardation and is recorded as Re(λ). Here, Re(λ) represents in-plane retardation at a wavelength λ, and unless otherwise specified, the wavelength λ is 550 nm.
[0098] In addition, the retardation in the thickness direction at the wavelength λ is described as Rth(λ) in this specification.
[0099] Re(λ) and Rth(λ) can use values measured at wavelength λ by AxoScan OPMF-1 (manufactured by OPTO SCIENCE, INC.) The following is calculated by inputting the average refractive index ((nx+ny+nz) / 3) and the film thickness (d (μm)) into AxoScan.
[0100] Slow axis direction (°)
[0101] Re(λ)=R0(λ)
[0102] Rth(λ)=((nx+ny) / 2-nz)×d.
[0103] Furthermore, in this specification, the liquid crystal composition and the liquid crystal compound are concepts that also include substances that no longer exhibit liquid crystallinity due to curing or the like.
[0104] [First embodiment]
[0105] <Optical film>
[0106] The optical film according to the first embodiment of the present invention has a curved surface shape.
[0107] Specifically, the optical film of the first embodiment of the present invention has a non-developable curved surface with positive Gaussian curvature. As such a curved surface shape, various curved surface shapes having non-developable curved surfaces with positive Gaussian curvature can be used, such as a sphere, a parabola, an ellipse, an aspheric surface whose curvature changes from the center to the outside (for example, a non-center-symmetric curved surface such as a curved surface that is not optically axis-symmetric in the radial direction in the case of a circular lens).
[0108] Furthermore, in the optical film of the first embodiment of the present invention having such a curved surface shape, the peripheral shape (shape of the peripheral end), i.e., the planar shape, is not limited, and various shapes such as an ellipse, an oblong shape other than an ellipse, a polygon, and an irregular shape can be used. Among them, an ellipse is preferred. In addition, in the present invention, an ellipse also includes a circle.
[0109] The planar shape refers to the shape when viewed from the normal direction of the top (bottom) of the curved surface of the optical film. For example, when the optical film having a curved surface shape is a lens, it is generally the shape when viewed from the optical axis direction.
[0110] The optical film according to the first embodiment of the present invention is composed of a cholesteric liquid crystal layer or a film having a small phase difference, that is, a so-called zero retardation film.
[0111] Specifically, the first form of the optical film of the first embodiment of the present invention is composed of a cholesteric liquid crystal layer having a curved shape as described above, and the evaluation wavelength (measurement wavelength) is taken as a wavelength obtained by subtracting 20 nm from the half-value wavelength on the side shorter than the selective reflection center wavelength on the cholesteric liquid crystal layer, and the in-plane delay A at the evaluation wavelength at the center is less than 2% of the value of the evaluation wavelength, and the in-plane delay B at the evaluation wavelength at the outer edge is less than 2% of the value of the evaluation wavelength.
[0112] The first form of the optical film of the first embodiment of the present invention is, for example, an optical film as follows, wherein when the half-value wavelength on the side shorter than the selective reflection center wavelength on the cholesteric liquid crystal layer is 430nm, light with a wavelength of 410nm is used as the evaluation wavelength of the in-plane delay, the in-plane delay A at the center is less than 8.2nm, and the in-plane delay B at the outer edge is also less than 8.2nm.
[0113] In addition, when the first form of the first embodiment of the present invention has multiple cholesteric liquid crystal layers, the evaluation wavelength of the in-plane retardation of the optical film can be obtained by subtracting 20nm from the half-value wavelength on the side shorter than the selective reflection center wavelength of the cholesteric liquid crystal layer with the shortest selective reflection center wavelength.
[0114] Furthermore, the second form of the optical film of the first embodiment of the present invention is composed of a film having a curved surface shape as described above and not having selective reflectivity, and the in-plane retardation A at the central wavelength of 550nm is less than 11nm, and the in-plane retardation B at the evaluation wavelength at the outer edge is less than 11nm.
[0115] In the optical film of the first embodiment of the present invention, the center is usually the lowest part (deepest part) when the curved surface shape is concave, and the top part when the curved surface shape is convex. When the optical film functions as a lens, the center is usually the optical axis.
[0116] Furthermore, the outer edge portion (end portion) refers to a point 5 mm inside from the outermost edge of the lens.
[0117] That is, the optical film according to the first embodiment of the present invention is composed of a cholesteric liquid crystal layer having a curved surface shape or a film having a curved surface shape and not having selective reflectivity, and the phase difference, that is, the in-plane retardation is small as a whole.
[0118] According to the optical film of the first embodiment of the present invention, when used as a reflective polarizer constituting a pancake lens of a virtual reality display device, for example, it is possible to suppress the occurrence of ghosting.
[0119] The optical film of the first embodiment of the present invention can be used as a laminated optical body in combination with various optical elements such as a support (transparent film), a retardation film (retardation plate), a polarizer (polarizing plate), a reflective polarizer, and an antireflection film.
[0120] The laminated optical body will be described in detail later.
[0121] [Film without selective reflectivity]
[0122] In the optical film of the first embodiment of the present invention, various films having a small phase difference, that is, so-called zero retardation films (low retardation films) made of a low birefringence polymer resin can be used as the film without selective reflectivity.
[0123] As a low-birefringence polymer resin, it is also possible to use low-birefringence organic materials used in optical disc substrates, pickup lenses, lenses of cameras, microscopes or video cameras, substrates for liquid crystal displays, prisms, optical interconnection components, optical fibers, light guide plates for liquid crystal displays / laser beam printers, lenses for projectors and fax machines, Fresnel lenses, contact lenses, polarizing plate protective films, and microlens arrays, where birefringence becomes an obstacle to image formation or a source of noise.
[0124] Examples of such films include acrylic resins (acrylates such as polymethyl (meth)acrylate), polycarbonates, cyclic polyolefins such as cyclopentadiene polyolefins and norbornene polyolefins, polyolefins such as polypropylene, aromatic vinyl polymers such as polystyrene, polyarylates, and cellulose acylate.
[0125] The thickness of these films is not particularly limited, and may be appropriately set according to the forming material, application, and the like.
[0126] [Cholesteric liquid crystal layer]
[0127] As described above, the cholesteric liquid crystal layer is formed by fixing the cholesteric liquid crystal phase, and has a spiral structure in which liquid crystal compounds are stacked by spirally rotating. It has a structure in which liquid crystal compounds 40 are stacked by spirally rotating one circle (360° rotation) as a spiral pitch and multiple pitches of spirally rotating liquid crystal compounds are stacked.
[0128] Furthermore, it is well known that the cholesteric liquid crystal layer has selective reflectivity. Specifically, the cholesteric liquid crystal layer selectively reflects light in a predetermined wavelength band and transmits light in other wavelength regions. Furthermore, the cholesteric liquid crystal layer selectively reflects right circularly polarized light and transmits left circularly polarized light, or selectively reflects left circularly polarized light and transmits right circularly polarized light.
[0129] That is, the cholesteric liquid crystal layer selectively reflects right circularly polarized light or left circularly polarized light in a specified wavelength band and transmits the rest of the light. In other words, the cholesteric liquid crystal layer separates incident light into right circularly polarized light and left circularly polarized light in a specific wavelength band, reflects one circularly polarized light and transmits the other circularly polarized light.
[0130] In the cholesteric liquid crystal phase, the central wavelength of selective reflection (selective reflection central wavelength λ) depends on the length of the helical pitch (helical pitch P) in the cholesteric liquid crystal phase, and satisfies the relationship between the average refractive index n of the cholesteric liquid crystal phase and λ=n×P. Therefore, by adjusting the helical pitch, the selective reflection central wavelength, i.e., the selective reflection wavelength region, can be adjusted. The longer the helical pitch P, the longer the selective reflection central wavelength of the cholesteric liquid crystal phase.
[0131] Furthermore, it is shown that the half width Δλ (nm) of the wavelength region (circularly polarized light reflection wavelength region) of the selective reflection depends on Δn and the helical pitch P of the cholesteric liquid crystal phase, and satisfies the relationship of Δλ=Δn×P. Therefore, the width of the selective reflection wavelength region can be controlled by adjusting Δn. Δn can be adjusted by the type and mixing ratio of the liquid crystal compound forming the cholesteric liquid crystal layer and the temperature when the orientation is fixed.
[0132] In the present invention, various known cholesteric liquid crystal layers can be used as the cholesteric liquid crystal layer.
[0133] As a cholesteric liquid crystal layer, for example, it is possible to use a cholesteric liquid crystal layer formed by fixing the cholesteric liquid crystal phase with reference to Japanese Patent Gazette No. 2020-060627. The cholesteric liquid crystal layer formed by fixing the cholesteric liquid crystal phase is a thin film, and the transmitted light has a high degree of polarization, so it is preferred. From the viewpoint of suppressing the reduction of polarization degree or polarization axis distortion when stretching or forming into a three-dimensional shape, it is preferred to use the cholesteric liquid crystal layer as an optical film for curved surface forming. In addition, the reduction of polarization degree caused by polarization axis distortion is not easy to occur.
[0134] The optical film according to the first embodiment of the present invention may include a plurality of stacked cholesteric liquid crystal layers.
[0135] As an example, it is preferred to have at least a blue light reflection layer with a reflectivity of 40% or more at a wavelength of 460nm, a green light reflection layer with a reflectivity of 40% or more at a wavelength of 550nm, a yellow light reflection layer with a reflectivity of 40% or more at a wavelength of 600nm, and a red light reflection layer with a reflectivity of 40% or more at a wavelength of 650nm. If it is such a structure, it can show high reflectivity in a wavelength range wide in the visible range, so it is preferred. In addition, the above reflectivity is the reflectivity when non-polarized light is incident on the cholesteric liquid crystal layer at each wavelength.
[0136] Furthermore, the cholesteric liquid crystal layer formed by fixing the cholesteric liquid crystal phase, i.e., the blue light reflecting layer, the green light reflecting layer, the yellow light reflecting layer, and the red light reflecting layer, may have a pitch gradient structure in which the helical pitch of the cholesteric liquid crystal phase is continuously changed in the thickness direction. According to the pitch gradient structure, for example, with reference to Japanese Patent Publication No. 2020-060627, a green light reflecting layer and a yellow light reflecting layer can be continuously produced.
[0137] In the optical film according to the first aspect of the present invention, it is preferred that the cholesteric liquid crystal layer is a layer composed of a blue light reflecting layer, a green light reflecting layer, a yellow light reflecting layer, and a red light reflecting layer laminated in this order.
[0138] In addition, there are many cases where the cholesteric liquid crystal layer is combined with a phase difference layer. In this case, it is preferred to arrange the blue light reflection layer on the opposite side of the phase difference layer that converts circularly polarized light into linearly polarized light, that is, on the light source side. In this configuration, light passes through the blue light reflection layer, the green light reflection layer, the yellow light reflection layer, and the red light reflection layer in sequence.
[0139] The inventors of the present invention believe that the reason why ghosting can be suppressed by configuring the blue light reflecting layer on the light source side is that the influence of Rth can be suppressed. The inferred mechanism is as follows. In the cholesteric liquid crystal layer used as a light reflecting layer, the film thickness required to obtain a sufficient reflectivity (for example, more than 40%) becomes thicker as it approaches the long wavelength side. Therefore, when there is a light reflecting layer that reflects long wavelength light on the light source side, its film thickness becomes thicker, and as a result, the Rth received by the light passing through the layer becomes larger. For this reason, it is believed that the reflection band of the light reflecting layer configured on the light source side is more preferably on the short wavelength side.
[0140] It is also preferable that the optical film according to the first aspect of the present invention has a cholesteric liquid crystal layer containing a rod-like liquid crystal compound and a cholesteric liquid crystal layer containing a discotic liquid crystal compound.
[0141] With this structure, the cholesteric liquid crystal phase containing the rod-shaped liquid crystal compound has a positive RtH, while the cholesteric liquid crystal phase containing the discotic liquid crystal compound has a negative RtH, so that their Rths are canceled out and ghosting can be suppressed even for incident light from an oblique direction, which is preferred.
[0142] According to the research of the inventors, it is preferred that a blue light reflecting layer composed of a cholesteric liquid crystal layer containing a discotic liquid crystal compound, a green light reflecting layer composed of a cholesteric liquid crystal layer containing a rod-shaped liquid crystal compound, a yellow light reflecting layer composed of a cholesteric liquid crystal layer containing a discotic liquid crystal compound, and a red light reflecting layer composed of a cholesteric liquid crystal layer containing a rod-shaped liquid crystal compound are sequentially included. In addition, the order of the reflecting layers and the type of liquid crystal are only examples and are not limited to these structures.
[0143] The cancellation of Rth can be expressed as follows.
[0144] In an optical laminate film having n light reflecting layers, when the light reflecting layers are named L1, L2, L3, ..., Ln in order from the light source side, the sum of Rth of each layer from the light reflecting layer L1 to the light reflecting layer Li is SRthi. Specifically, it is the following formula.
[0145] SRth1=Rth1
[0146] SRth2=Rth1+Rth2
[0147] …
[0148] SRthi=Rth1+Rth2……+Rthi
[0149] …
[0150] SRthn=Rth1+Rth2……+Rthi……+Rthn
[0151] The absolute value of all these SRthi (SRth1 to SRthn) is preferably 0.3 μm or less, more preferably 0.2 μm or less, and most preferably 0.1 μm or less. Rthi of each layer in the above formula is obtained by the formula for calculating Rth described in
[0023] .
[0152] The thickness of the cholesteric liquid crystal layer is not particularly limited, but is preferably 30 μm or less, and more preferably 15 μm or less, from the viewpoint of thinning.
[0153] Furthermore, when the cholesteric liquid crystal layer is stretched or formed, the reflection wavelength region of the cholesteric liquid crystal layer may shift. Therefore, it is preferable to select the reflection wavelength region in anticipation of the wavelength shift.
[0154] For example, when a cholesteric liquid crystal layer is used, the film is stretched due to stretching and forming, which sometimes causes the helical pitch of the cholesteric liquid crystal layer to become smaller, so it is preferred to pre-set the helical pitch of the cholesteric liquid crystal phase to be large. In addition, assuming the short-wave shift in the reflection wavelength region caused by stretching or forming, the cholesteric liquid crystal layer also preferably has an infrared light reflection layer with a reflectivity of 40% or more at a wavelength of 800nm.
[0155] Furthermore, when the stretching ratio during stretching or forming is not uniform in the plane, a suitable reflection wavelength region can be selected at each part in the plane according to the wavelength shift caused by stretching. That is, there may be regions with different reflection wavelength regions in the plane. In addition, it is also preferred to set the reflection wavelength region wider than the desired wavelength region in advance, assuming that the stretching ratio at each part in the plane is different.
[0156] (Method for producing a cholesteric liquid crystal layer)
[0157] The cholesteric liquid crystal layer can be formed as follows: a liquid crystal composition obtained by dissolving a liquid crystal compound, a chiral reagent, a polymerization initiator, and further a surfactant added as needed in a solvent is applied on a support or on a base layer (orientation film) formed on a support and dried to obtain a coating film, the liquid crystal compound in the coating film is oriented, and the coating film is irradiated with active light to cure the liquid crystal composition.
[0158] Thereby, a cholesteric liquid crystal layer having a cholesteric liquid crystal structure in which cholesteric regularity (cholesteric liquid crystal phase) is fixed can be formed.
[0159] 〔Coating method〕
[0160] Examples of the coating method include known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spray coating, and inkjet.
[0161] [Method of providing in-plane distribution of the helical pitch]
[0162] The helical pitch of the cholesteric liquid crystal layer constituting the optical film of the first embodiment of the present invention may have an in-plane distribution. Since the helical pitch of the cholesteric liquid crystal layer has an in-plane distribution, even if the film thickness changes due to the formation into a curved surface shape described later, the unevenness of the selective reflection wavelength region in the plane can still be suppressed.
[0163] As a method for imparting an in-plane distribution to the helical pitch of the cholesteric liquid crystal layer, for example, there is a method of using a chiral reagent that is changed by photoisomerization of HTP.
[0164] The following is a detailed description.
[0165] A liquid crystal composition containing a chiral agent whose HTP changes due to photoisomerization is applied, and the cholesteric liquid crystal layer obtained by subsequent heat treatment and orientation is irradiated with light corresponding to the photoisomerization as needed, whereby the HTP of the chiral agent changes, resulting in that the helical pitch of the cholesteric liquid crystal layer can be changed and the reflection wavelength can be changed.
[0166] By utilizing this property, the oriented cholesteric liquid crystal layer is subjected to patterned light irradiation using an exposure mask or the like to photoisomerize it, thereby obtaining a pattern in which the reflection wavelength changes only in the area irradiated with light. After obtaining the pattern, the entire cholesteric liquid crystal layer is exposed to cure the liquid crystal composition, and the liquid crystal composition is polymerized, thereby finally obtaining a cholesteric liquid crystal layer (patterned cholesteric liquid crystal layer) having an in-plane distribution of the helical pitch. Photoisomerization no longer occurs in the cured patterned cholesteric liquid crystal layer, and the layer has stable properties.
[0167] In order to efficiently perform pattern formation, it is preferable to separate the light irradiation for photoisomerization from the light irradiation for curing. In other words, in order to efficiently perform pattern formation, it is preferable to prevent the photoisomerization and curing from being performed as much as possible while the other is being performed.
[0168] Examples of a method for separating the two include separation based on oxygen concentration and separation based on exposure wavelength.
[0169] First, regarding oxygen concentration, photoisomerization is not easily affected by oxygen concentration. Although it depends on the initiator used, curing is basically less likely to occur as the oxygen concentration is higher.
[0170] Therefore, photoisomerization is performed under conditions of high oxygen concentration, such as in the atmosphere, and curing is performed under conditions of low oxygen concentration, such as in a nitrogen atmosphere at an oxygen concentration of 300 vol ppm or less. This makes it easy to separate photoisomerization from curing.
[0171] Furthermore, regarding the exposure wavelength, photoisomerization of the chiral agent easily proceeds at the absorption wavelength of the chiral agent, and curing easily proceeds at the absorption wavelength of the photopolymerization initiator.
[0172] Therefore, by selecting a chiral agent and a photopolymerization initiator so that the absorption wavelengths of the chiral agent and the photopolymerization initiator are different from each other, it is possible to separate photoisomerization and curing based on the exposure wavelength.
[0173] In addition, one or both of photoisomerization and curing may be performed under heating as needed. The temperature during heating is preferably 25 to 140°C, more preferably 30 to 100°C.
[0174] As another method using a chiral reagent converted by photoisomerization of HTP, there is also a method in which curing is first performed in a pattern and then isomerization of the uncured region is performed.
[0175] That is, for the oriented cholesteric liquid crystal phase, first, a light exposure mask or the like is used to irradiate the curing light in a pattern. Thereafter, light irradiation for overall photoisomerization can be performed. It is impossible for the pitch change caused by photoisomerization to occur in the area that was cured first. Therefore, the pitch change caused by photoisomerization and the change in the reflection wavelength occur only in the area that was not cured first.
[0176] In this case, after the pattern is obtained, the entire cholesteric liquid crystal layer is exposed to light for curing the liquid crystal composition to polymerize the liquid crystal composition, thereby obtaining a final patterned cholesteric liquid crystal layer.
[0177] [Direct coating of each layer]
[0178] As described above, the optical film according to the first embodiment of the present invention may have a plurality of cholesteric liquid crystal layers laminated thereon.
[0179] At this time, it is preferred to directly form an adjacent layer between each cholesteric liquid crystal layer without an adhesive layer. When forming the layer, the adhesive layer can be omitted by directly coating on the already formed adjacent layer. In the following description, the cholesteric liquid crystal layer is also referred to as a "light reflecting layer".
[0180] Furthermore, in order to reduce the refractive index difference in all directions within the plane, it is preferable to arrange the liquid crystal compound so that the orientation direction (slow axis direction) changes continuously at the interface. For example, when a light reflecting layer containing rod-shaped liquid crystals is formed on a light reflecting layer containing discotic liquid crystals, a coating liquid containing rod-shaped liquid crystals is directly applied, and the orientation can be made so that the slow axis direction continues at the interface due to the orientation restriction force generated by the discotic liquid crystals of the light reflecting layer containing discotic liquid crystals.
[0181] [How to paste each layer]
[0182] As described above, the optical film of the first embodiment of the present invention may be laminated with a plurality of cholesteric liquid crystal layers (light reflecting layers). In this case, each light reflecting layer may be attached by any attachment method. The attachment may be performed using a bonding agent or adhesive.
[0183] As the adhesive, any commercially available adhesive can be used. Here, from the viewpoint of thinning the optical film and reducing the surface roughness Ra, the thickness of the adhesive is preferably 25 μm or less, more preferably 15 μm or less, and further preferably 6 μm or less. In addition, an adhesive that does not easily release gas is preferably used. In particular, vacuum treatment or heat treatment is sometimes required during stretching or forming, and it is also preferable that no release gas is generated under these conditions.
[0184] As the adhesive, any commercially available adhesive can be used. Specifically, as the adhesive, epoxy resin adhesives and acrylic resin adhesives can be exemplified.
[0185] Here, from the viewpoint of thinning the optical film and reducing the surface roughness Ra, the thickness of the adhesive is preferably 25 μm or less, more preferably 5 μm or less, and further preferably 1 μm or less. In addition, from the viewpoint of thinning the adhesive layer and applying the adhesive to the adherend with a uniform thickness, the viscosity of the adhesive is preferably 300 cP or less, and more preferably 100 cP or less.
[0186] Furthermore, when the adherend has a surface concavo-convex, from the viewpoint of reducing the surface roughness Ra of the cholesteric liquid crystal layer, the adhesive and the bonding agent can also select a suitable viscoelasticity or thickness so as to be able to embed the surface concavo-convex of the bonding layer. From the viewpoint of embedding the surface concavo-convex, the viscosity of the adhesive and the bonding agent is preferably 50 cP or more. Furthermore, the thickness is preferably thicker than the height of the surface concavo-convex.
[0187] As a method for adjusting the viscosity of the adhesive, for example, a method of using an adhesive containing a solvent can be cited. At this time, the viscosity of the adhesive can be adjusted according to the ratio of the solvent. In addition, by applying the adhesive to the adherend and then drying the solvent, the thickness of the adhesive can be further reduced.
[0188] In the cholesteric liquid crystal layer, from the viewpoint of reducing unnecessary reflection and suppressing the decrease in the polarization degree of transmitted light, it is preferred that the adhesive used to bond each layer and the adhesive have a small refractive index difference with the adjacent layer. Since the liquid crystal layer has birefringence and the refractive index in the fast axis direction is different from that in the slow axis direction, when the value obtained by adding the refractive index in the fast axis direction and the slow axis direction and dividing by 2 is set as the average refractive index nave of the liquid crystal layer, the difference between the refractive index of the adjacent adhesive layer or adhesive layer and nave is preferably 0.075 or less, more preferably 0.05 or less, and further preferably 0.025 or less. The refractive index of the adhesive and the adhesive can be adjusted by, for example, mixing titanium oxide particles or zirconium oxide particles.
[0189] Furthermore, the cholesteric liquid crystal layer has anisotropy of refractive index in the plane, but preferably the difference of refractive index with adjacent layers in all directions in the plane is 0.10 or less. Therefore, the adhesive or bonding agent may have anisotropy of refractive index in the plane. In this regard, the same also applies to the case where the laminated optical body using the optical film (cholesteric liquid crystal layer) of the first embodiment of the present invention includes a phase difference layer and a linear polarizer having anisotropy of refractive index in the plane.
[0190] Furthermore, when the optical film of the first embodiment of the present invention is composed of a multilayer cholesteric layer, a refractive index adjustment layer having a refractive index difference between a fast axis direction and a slow axis direction smaller than that of the cholesteric liquid crystal layer may be provided between the cholesteric liquid crystal layer and the adhesive or between the cholesteric liquid crystal layer and the adhesive. In this case, the refractive index adjustment layer preferably has a cholesteric liquid crystal layer. By having a refractive index adjustment layer, it is possible to further suppress interface reflection and further suppress the generation of ghosting. Furthermore, it is preferred that the average refractive index of the refractive index adjustment layer is smaller than the average refractive index of the cholesteric liquid crystal layer. Furthermore, the central wavelength of the reflected light of the refractive index adjustment layer may be less than 430 nm or greater than 670 nm, more preferably less than 430 nm.
[0191] Furthermore, it is preferred that the thickness of the adhesive layer between the cholesteric liquid crystal layers be 100 nm or less.
[0192] When the thickness of the adhesive layer is 100 nm or less, the refractive index difference is less likely to be felt by light in the visible range, and unnecessary reflection can be suppressed. The thickness of the adhesive layer is more preferably 50 nm or less, and further preferably 30 nm or less.
[0193] As a method of forming an adhesive layer having a thickness of 100 nm or less, for example, there is a method of vapor-depositing a ceramic adhesive such as silicon oxide (SiOx layer) on the bonding surface.
[0194] The bonding surface of the bonding component may be subjected to surface modification treatment such as plasma treatment, corona treatment, and saponification treatment before bonding. In addition, a primer layer may be provided on the bonding surface of the bonding component.
[0195] Furthermore, when there are a plurality of laminating surfaces, the type and thickness of the adhesive layer can be adjusted for each laminating surface. Specifically, for example, an adhesive layer having a thickness of 100 nm or less can be provided in the order shown in the following (1) to (3).
[0196] (1) The laminated layers are bonded to a dummy support made of a glass substrate.
[0197] (2) A SiOx layer having a thickness of 100 nm or less is formed on both the surface of the stacked layer and the surface of the stacked layer by vapor deposition or the like. The vapor deposition can be performed using SiOx powder as a vapor deposition source, for example, using a vapor deposition device (model ULEYES) manufactured by ULVAC, Inc. In addition, it is preferred that a plasma treatment be performed in advance on the surface of the formed SiOx layer.
[0198] (3) After the formed SiOx layers are bonded together, the dummy support is peeled off. The bonding is preferably performed at a temperature of 120°C, for example.
[0199] The coating, bonding or lamination of each layer can be performed in a roll-to-roll manner or in a single wafer manner.
[0200] The roll-to-roll method is preferable in terms of improving productivity and reducing axial deviation of each layer.
[0201] On the other hand, the single wafer method is preferred from the viewpoints of suitability for small-volume and high-variety production and the ability to select a special bonding method such as the aforementioned adhesive layer having a thickness of 100 nm or less.
[0202] In addition, examples of methods for applying the adhesive to an adherend include well-known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spray coating, and inkjet.
[0203] As described above, the cholesteric liquid crystal layer as the optical film of the first embodiment of the present invention can also be laminated with other layers to be used as a laminated optical body. These layers may include a support body, an alignment layer, and the like.
[0204] Here, the support and the alignment layer may be a pseudo support that is peeled off and removed when making the laminated optical body. When using a pseudo support, after the cholesteric liquid crystal layer is transferred to another laminate, the pseudo support is peeled off and removed, thereby making it possible to make the laminated optical body thinner, and further to remove the adverse effect of the phase difference of the pseudo support on the polarization degree of the transmitted light, so it is preferred.
[0205] The type of support is not particularly limited, but is preferably transparent. For example, films such as cellulose acylate, polycarbonate, polysulfone, polyethersulfone, polyacrylate, polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester can be used. Among them, films such as cellulose acylate, cyclic polyolefin, polyacrylate, and polymethacrylate are preferred. In addition, these films can be commercially available. As commercially available products, for example, if it is a cellulose acetate film, "TD80U" and "Z-TAC" manufactured by FUJIFILM Corporation can be exemplified.
[0206] When the support is a pseudo support, a support having high tear strength is preferred from the viewpoint of preventing breakage during peeling. From this viewpoint, polycarbonate and polyester films are preferred.
[0207] Furthermore, from the viewpoint of suppressing the adverse effects on the polarization degree of the transmitted light, it is preferred that the phase difference of the support is small. Specifically, the Re (in-plane retardation) of the support is preferably less than 10 nm, and the absolute value of Rth (delay in the thickness direction) is preferably less than 50 nm. In addition, even if the support is used as the above-mentioned pseudo support, in the manufacturing process of the laminated optical body, when the quality inspection of the cholesteric liquid crystal layer or other laminated bodies is performed, it is also preferred that the phase difference of the pseudo support is small.
[0208] In addition, various sensors that use near-infrared light as a light source for eye tracking, expression recognition, iris authentication, etc. are sometimes incorporated into optical systems such as virtual reality display devices and electronic viewfinders. In this case, in order to minimize the impact on the sensors, the cholesteric liquid crystal layer is preferably transmissive to near-infrared light.
[0209] [Laminated optical body]
[0210] As described above, the optical film (cholesteric liquid crystal layer) according to the first embodiment of the present invention can be used as a laminated optical body laminated with other film-like optical elements.
[0211] Here, as a laminated optical body, a structure preferably exemplified is one having, in addition to a cholesteric liquid crystal layer, a phase difference layer for converting circularly polarized light into linearly polarized light and a linear polarizer in this order.
[0212] The optical lens of the first embodiment of the present invention and the laminated optical body including the optical film (cholesteric liquid crystal layer) of the first embodiment of the present invention can be combined with a lens to be used as a composite lens. As a preferred example of the use of the composite lens, a virtual reality display device is preferably exemplified.
[0213] Hereinafter, the function of the laminated optical body including the optical film (cholesteric liquid crystal layer) according to the first embodiment of the present invention will be described in detail by describing the function of the virtual reality display device.
[0214] Figure 1 This is a diagram conceptually showing a virtual reality display device using a stacked optical body.
[0215] Figure 1 The virtual reality display device shown has an image display panel 500, a circular polarizing plate 400, a half mirror 300, a lens 200, and a laminated optical body 100. As described above, the laminated optical body 100 has a cholesteric liquid crystal layer, a phase difference layer, and a linear polarizer in this order.
[0216] exist Figure 1 In the virtual reality display device shown, the light 1000 (display image) emitted by the image display panel 500 will pass through the circular polarizer 400 to become circularly polarized light, half of which will pass through the half mirror 300.
[0217] The light 1000 that has passed through the half mirror 300 then passes through the lens 200 and enters the laminated optical body 100 from the cholesteric liquid crystal layer side, and is reflected as right circularly polarized light or left circularly polarized light.
[0218] After the circularly polarized light reflected in the cholesteric liquid crystal layer transmits through the lens 200 again, it is reflected again in the half mirror 300, transmits through the lens 200 again, and enters the stacked optical body 100. Here, the circularly polarized light state of the light 1000 does not change when it is reflected in the stacked optical body (cholesteric liquid crystal layer), and when it is reflected in the half mirror 300, it becomes a circularly polarized light orthogonal to the circularly polarized light when it first enters the stacked optical body 100. That is, the right circularly polarized light becomes the left circularly polarized light, and the left circularly polarized light becomes the right circularly polarized light. Therefore, the light 1000 reflected in the half mirror 300 transmits the stacked optical body 100 and is visually recognized by the user.
[0219] Furthermore, when the light 1000 is reflected by the half mirror 300, the image is magnified because the half mirror is in the shape of a concave mirror, and the user can visually recognize the magnified virtual image. This optical system is called a pancake lens (reciprocating optical system, folding optical system).
[0220] on the other hand, Figure 2 It is a schematic diagram showing a situation where the light 1000 is not reflected when it first enters the stacked optical body 100 but is transmitted unnecessarily to become leakage light 2000. Specifically, the leakage light 2000 is, for example, light that is not reflected but is transmitted unnecessarily when the stacked optical body 100 (cholesteric liquid crystal layer) selectively reflects right circularly polarized light.
[0221] like Figure 2 As shown, at this time, the user visually recognizes an image that is not magnified, that is, a light leakage 2000. This image is called a ghost image, etc., and is required to be reduced.
[0222] The cholesteric liquid crystal layer originally has no phase difference (in-plane retardation). Figure 1 and Figure 2 In the virtual reality display device shown, the stacked optical body 100, i.e., the cholesteric liquid crystal layer, is formed into a concave mirror shape. Therefore, the helical axis of a part of the surface of the cholesteric liquid crystal layer changes, resulting in a phase difference. The cholesteric liquid crystal layer having a phase difference cannot properly reflect and transmit the incident light. Therefore, if such a cholesteric liquid crystal layer is used in a pancake lens constituting a virtual reality display device, light leakage 2000, i.e., ghosting, will increase.
[0223] In contrast, as described above, the optical film (cholesteric liquid crystal layer) of the first embodiment of the present invention has a curved surface shape, and further, the evaluation wavelength (measurement wavelength) of the in-plane retardation is a wavelength obtained by subtracting 20 nm from the half-value wavelength on the side shorter than the selective reflection center wavelength on the cholesteric liquid crystal layer, and the in-plane retardation A of the cholesteric liquid crystal layer at the evaluation wavelength at the center is less than 2% of the evaluation wavelength, and the in-plane retardation B of the cholesteric liquid crystal layer at the evaluation wavelength at the outer edge is less than 2% of the evaluation wavelength. That is, the phase difference of the optical film of the first embodiment of the present invention is small as a whole.
[0224] Therefore, the virtual reality display device using the laminated optical body 100 having the optical film according to the first embodiment of the present invention can suppress the occurrence of ghost images even when using a cholesteric liquid crystal layer which is an optical film having a curved shape.
[0225] Then, such an optical film having a small phase difference as a whole can be produced by a molding method according to a first embodiment of the present invention described later.
[0226] The layer structure of one embodiment of the laminated optical body 100 is shown in FIG. Figure 3 .
[0227] Figure 3 The laminated optical body 100 shown includes an antireflection layer 101, a positive C plate 102, an optical film 103, a positive C plate 104, a retardation layer 105, and a linear polarizer 106 in this order. The optical film 103 is an optical film according to the first embodiment of the present invention, and is a cholesteric liquid crystal layer.
[0228] The laminated optical body 100 includes an optical film 103, a phase difference layer 105 that converts circularly polarized light into linearly polarized light, and a linear polarizer 106 in this order. Here, the phase difference layer 105 and the linear polarizer 106 are configured to convert circularly polarized light originally reflected by the optical film 103 into a linear polarizer in a direction absorbed by the linear polarizer. According to the laminated optical body 100, light leakage from the optical film 103 (cholesteric liquid crystal layer) can be absorbed by the linear polarizer. Therefore, the polarization degree of the transmitted light can be increased.
[0229] In addition, when forming a stacked optical body, the cholesteric liquid crystal layer may produce a phase difference, but as described above, even if the cholesteric liquid crystal layer of the first embodiment of the present invention is stretched or formed, the phase difference remains small, and the amount of light leakage from the cholesteric liquid crystal layer is small, so the increase in light leakage can be suppressed to a small amount.
[0230] As described above, the optical film according to the first embodiment of the present invention may be composed of a plurality of cholesteric liquid crystal layers. Figure 4 An example of this structure is shown.
[0231] The optical film 103 sequentially comprises a first light reflecting layer (cholesteric liquid crystal layer) 31, a second light reflecting layer 32, a third light reflecting layer 33, and a fourth light reflecting layer 34. As such an optical film 103, the above-mentioned optical film having a blue light reflecting layer with a reflectivity of 40% or more at a wavelength of 460nm, a green light reflecting layer with a reflectivity of 40% or more at a wavelength of 550nm, a yellow light reflecting layer with a reflectivity of 40% or more at a wavelength of 600nm, and a red light reflecting layer with a reflectivity of 40% or more at a wavelength of 650nm can be exemplified.
[0232] Furthermore, it is preferred that the surface roughness Ra of the laminated optical body be 100 nm or less.
[0233] If Ra is small, it is preferred that the clarity of the image can be improved when the laminated optical body is applied to a virtual reality display device, etc. The inventors speculate that when light is reflected in the laminated optical body, if there are concave and convex surfaces, the angle distortion of the reflected light, the distortion or blurring of the image will be caused. The Ra of the laminated optical body is preferably 50 nm or less, more preferably 30 nm or less, and further preferably 10 nm or less.
[0234] Furthermore, the laminated optical body is made by laminating a plurality of layers. According to the research of the inventors, it is found that when another layer is laminated on a layer having concavoconvexity, the concavoconvexity is sometimes magnified. Therefore, in the laminated optical body, it is preferred that the Ra of all layers is small. The Ra of each layer of the laminated optical body is preferably 50 nm or less, more preferably 30 nm or less, and further preferably 10 nm or less.
[0235] Furthermore, from the viewpoint of improving the image clarity of a reflected image, it is particularly preferred that the Ra of the cholesteric liquid crystal layer is small.
[0236] The surface roughness Ra can be measured, for example, using the non-contact surface / layer cross-section shape measuring system VertScan (manufactured by Mitsubishi Chemical Systems, Inc.). Since Vertscan is a surface shape measuring method that uses the phase of the reflected light from the sample, when measuring the cholesteric liquid crystal layer, it sometimes causes the reflected light from the inside of the film to overlap and the surface shape cannot be accurately measured. At this time, in order to increase the reflectivity of the surface to further suppress the reflection from the inside, a metal layer can be formed on the surface of the sample. As the main method for forming a metal layer on the surface of the sample, a sputtering method is used. As a sputtering material, Au, Al, Pt, etc. are used.
[0237] The laminated optical body preferably has a small number of point defects per unit area. Point defects can lead to a decrease in the polarization degree of transmitted light or a decrease in image clarity, so a small number is preferred.
[0238] Since the laminated optical body is produced by laminating a plurality of layers, in order to reduce the number of point defects in the laminated optical body as a whole, it is also preferred that the number of point defects in each layer is small. Specifically, the number of point defects in each layer is preferably 20 or less per square meter, more preferably 10 or less, and further preferably 1 or less. Furthermore, as for the laminated optical body as a whole, the number of point defects is preferably 100 or less per square meter, more preferably 50 or less, and further preferably 5 or less.
[0239] The number of point defects is preferably counted if the size of the point defects is 100 μm or more (more preferably 30 μm or more, and even more preferably 10 μm or more).
[0240] In addition, point defects include foreign matter, scratches, dirt, film thickness variation, and poor orientation of liquid crystal compounds.
[0241] In addition, various sensors that use near-infrared light as a light source, such as eye tracking, expression recognition, and iris authentication, are sometimes incorporated into optical systems such as virtual reality display devices and electronic viewfinders. In this case, in order to minimize the impact on the sensors, it is preferred that the laminated optical body has transmissivity to near-infrared light.
[0242] 〔Phase difference layer〕
[0243] The phase difference layer used for the laminated optical body has a function of converting the outgoing light into approximately linear polarized light when circularly polarized light is incident.
[0244] As the phase difference layer, for example, a phase difference layer whose in-plane retardation Re is about 1 / 4 wavelength at any wavelength in the visible range can be used. As an example, the in-plane retardation Re (550) of the phase difference layer at a wavelength of 550 nm is preferably 120 to 150 nm, more preferably 125 to 145 nm, and further preferably 135 to 140 nm.
[0245] Furthermore, a retardation layer having Re of approximately 3 / 4 wavelength or approximately 5 / 4 wavelength is also preferred because it can convert linearly polarized light into circularly polarized light.
[0246] Furthermore, the phase difference layer used in the laminated optical body preferably has anomalous dispersion with respect to wavelength.
[0247] If the retardation layer has anomalous dispersion, it is preferable because it can convert circularly polarized light into linearly polarized light in a wide wavelength range of the visible range. Here, having anomalous dispersion with respect to wavelength means that as the wavelength increases, the retardation value at the wavelength increases.
[0248] The phase difference layer having anomalous dispersion can be produced by uniaxially stretching a polymer film such as a modified polycarbonate resin film having anomalous dispersion, for example, with reference to Japanese Patent Application Laid-Open No. 2017-049574.
[0249] Furthermore, as long as the phase difference layer having anomalous dispersion substantially has anomalous dispersion, for example, as disclosed in Japanese Patent Gazette No. 06259925, it can also be produced by stacking a phase difference layer having Re of approximately 1 / 4 wavelength and a phase difference layer having Re of approximately 1 / 2 wavelength in such a manner that their slow axes form an angle of approximately 60° with each other. It is known that at this time, even if the 1 / 4 wavelength phase difference layer and the 1 / 2 wavelength phase difference layer are respectively normal dispersion (as the wavelength becomes larger, the phase difference value at the wavelength becomes smaller), circularly polarized light can be converted into linearly polarized light within a wide wavelength range of the visible range, and can be regarded as substantially having anomalous dispersion. At this time, the stacked optical body preferably has a cholesteric liquid crystal layer, a 1 / 4 wavelength phase difference layer, a 1 / 2 wavelength phase difference layer, and a linear polarizer in this order.
[0250] Furthermore, the phase difference layer used for the laminated optical body also preferably has a layer in which a uniformly aligned liquid crystal compound is fixed.
[0251] As such a phase difference layer, for example, a layer in which a rod-shaped liquid crystal compound is uniformly oriented horizontally to the in-plane direction and a layer in which a disc-shaped liquid crystal compound is uniformly oriented vertically to the in-plane direction can be used. Furthermore, for example, a phase difference layer with anomalous dispersion prepared by uniformly oriented and fixed rod-shaped liquid crystal compounds with anomalous dispersion can also be used with reference to Japanese Patent Publication No. 2020-084070.
[0252] Furthermore, the phase difference layer used for the laminated optical body also preferably has a layer in which a liquid crystal compound twistedly oriented with the thickness direction as the helical axis is fixed.
[0253] For example, as disclosed in Japanese Patent No. 05753922 and Japanese Patent No. 05960743, a phase difference layer having a layer formed by fixing a rod-shaped liquid crystal compound or a disc-shaped liquid crystal compound twisted and oriented with the thickness direction as the helical axis can also be used. In this case, the phase difference layer can be regarded as having anomalous dispersion in essence, and is therefore preferred.
[0254] The thickness of the retardation layer is not particularly limited, but is preferably 0.1 to 8 μm, more preferably 0.3 to 5 μm, from the viewpoint of thinning.
[0255] The phase difference layer may include a support, an alignment layer, and the like.
[0256] In addition, the support and the alignment layer can be a pseudo support that is peeled off and removed when making the laminated optical body. When using a pseudo support, after the phase difference layer is transferred to another laminate, the pseudo support is peeled off and removed, thereby making the laminated optical body thinner and further removing the adverse effect of the phase difference of the pseudo support on the polarization degree of the transmitted light, so it is preferred.
[0257] The type of the support is not particularly limited, but is preferably transparent. For example, films such as cellulose acylate, polycarbonate, polysulfone, polyethersulfone, polyacrylate, polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester can be used. Among them, cellulose acylate films, cyclic polyolefin, polyacrylate, and polymethacrylate are preferred. Commercially available products can also be used as the support. As an example of a commercially available product, if it is a cellulose acetate film, "TD80U" and "Z-TAC" manufactured by FUJIFILM Corporation can be exemplified.
[0258] When the support is a pseudo support, a support having high tear strength is preferred from the viewpoint of preventing breakage during peeling. From this viewpoint, polycarbonate and polyester films are preferred.
[0259] Furthermore, from the viewpoint of suppressing the adverse effects on the polarization degree of the transmitted light, it is preferred that the phase difference of the support is small. Specifically, the in-plane delay of the support is preferably 10 nm or less, and the absolute value of the delay Rth in the thickness direction is preferably 50 nm or less. Furthermore, even if the support is used as the above-mentioned pseudo support, when the quality inspection of the phase difference layer or other laminated bodies is performed in the manufacturing process of the laminated optical body, it is also preferred that the phase difference of the pseudo support is small.
[0260] In addition, various sensors that use near-infrared light as a light source, such as eye tracking, expression recognition, and iris authentication, are sometimes incorporated into optical systems such as virtual reality display devices and electronic viewfinders. In this case, in order to minimize the impact on the sensor, the phase difference layer used for the laminated optical body is preferably transmissive to near-infrared light.
[0261] 〔Linear polarizer〕
[0262] The linear polarizer used for the laminated optical body is an absorption-type polarizer that absorbs linear polarized light in the absorption axis direction of incident light and transmits linear polarized light in the transmission axis direction.
[0263] As a linear polarizer, a general polarizer can be used. As an example, a polarizer oriented by dyeing polyvinyl alcohol or other polymer resins with a dichroic substance and stretching, and a polarizer oriented by orienting a dichroic substance using a liquid crystal compound are exemplified. From the viewpoint of availability and the viewpoint of improving the polarization degree, a polarizer dyed with polyvinyl alcohol with iodine and stretched is preferred.
[0264] The thickness of the linear polarizer is preferably 10 μm or less, more preferably 7 μm or less, and further preferably 5 μm or less. When the linear polarizer is thin, cracks or breaks in the film can be prevented when the laminated optical body is stretched or formed.
[0265] Furthermore, the single plate transmittance of the linear polarizer is preferably 40% or more, more preferably 42% or more. Furthermore, the polarization degree is preferably 90% or more, more preferably 95% or more, and further preferably 99% or more. In addition, in this specification, the single plate transmittance and polarization degree of the linear polarizer are measured using an automatic polarization film measuring device: VAP-7070 (manufactured by JASCO Corporation).
[0266] Furthermore, the transmission axis of the linear polarizer is preferably aligned with the polarization axis of the light converted into linear polarized light by the phase difference layer. For example, when the phase difference layer is a layer having a phase difference of 1 / 4 wavelength, the angle between the transmission axis of the linear polarizer and the slow axis of the phase difference layer is preferably about 45°.
[0267] The linear polarizer used for the laminated optical body is also preferably a light absorption anisotropic layer containing a liquid crystal compound and a dichroic substance. The linear polarizer containing a liquid crystal compound and a dichroic substance can be made thinner and is not prone to cracking or breaking even after stretching or forming, so it is preferred. The thickness of the light absorption anisotropic layer is not particularly limited, but is preferably 0.1 to 8 μm, more preferably 0.3 to 5 μm, from the viewpoint of thinning.
[0268] A linear polarizer including a liquid crystal compound and a dichroic substance can be produced with reference to, for example, Japanese Patent Application Laid-Open No. 2020-023153.
[0269] From the viewpoint of improving the polarization degree of the linear polarizer, the orientation degree of the dichroic substance in the light absorption anisotropic layer is preferably 0.95 or more, more preferably 0.97 or more.
[0270] When the linear polarizer is composed of a light absorption anisotropic layer containing a liquid crystal compound and a dichroic substance, the linear polarizer may include a support, an alignment layer, and the like.
[0271] The support and the alignment layer may be a pseudo support that is peeled off and removed when making the laminated optical body. When using a pseudo support, after the light absorption anisotropic layer is transferred to another laminate, the pseudo support is peeled off and removed, thereby making it possible to make the laminated optical body thinner and further remove the adverse effect of the phase difference of the pseudo support on the polarization degree of the transmitted light, so it is preferred.
[0272] The type of support is not particularly limited, but is preferably transparent. For example, films such as cellulose acylate, polycarbonate, polysulfone, polyethersulfone, polyacrylate, polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester can be used. Among them, cellulose acylate films, cyclic polyolefin, polyacrylate, and polymethacrylate are preferred. Commercial products can also be used as the support. As an example of a commercial product, if it is a cellulose acetate film, "TD80U" and "Z-TAC" manufactured by FUJIFILM Corporation can be exemplified.
[0273] When the support is a pseudo support, a support having high tear strength is preferred from the viewpoint of preventing breakage during peeling. From this viewpoint, polycarbonate and polyester films are preferred.
[0274] Furthermore, from the viewpoint of suppressing the adverse effect on the polarization degree of the transmitted light, it is preferred that the phase difference of the support is small. Specifically, the in-plane retardation Re of the support is preferably 10 nm or less, and the absolute value of the retardation Rth in the thickness direction is preferably 50 nm or less. Furthermore, even if the support is used as the above-mentioned pseudo support, when the quality inspection of the light absorption anisotropic layer or other laminated bodies is performed in the manufacturing process of the laminated optical body, it is also preferred that the phase difference of the pseudo support is small.
[0275] In addition, various sensors that use near-infrared light as a light source, such as eye tracking, expression recognition, and iris authentication, are sometimes incorporated into optical systems such as virtual reality display devices and electronic viewfinders. In this case, in order to minimize the impact on the sensor, the linear polarizer used in the laminated optical body is preferably transmissive to near-infrared light.
[0276] 〔Other functional layers〕
[0277] The laminated optical body may have other functional layers in addition to the cholesteric liquid crystal layer, the phase difference layer and the linear polarizer.
[0278] In addition, various sensors that use near-infrared light as a light source, such as eye tracking, expression recognition, and iris authentication, are sometimes incorporated into optical systems such as virtual reality display devices and electronic viewfinders. In this case, in order to minimize the impact on the sensor, the other functional layers used for the laminated optical body are preferably transmissive to near-infrared light.
[0279] <Positive C plate>
[0280] like Figure 3 As shown, the laminated optical body also preferably further has a positive C plate. Here, the positive C plate refers to a phase difference layer having substantially zero in-plane retardation Re and a negative retardation Rth in the thickness direction.
[0281] The positive C plate can be obtained, for example, by vertically aligning a rod-shaped liquid crystal compound. The details of the method for producing the positive C plate can be found in, for example, Japanese Patent Application Publication Nos. 2017-187732, 2016-53709, and 2015-200861.
[0282] The positive C plate functions as an optical compensation layer for increasing the polarization degree of the transmitted light for the light incident from an oblique direction. The positive C plate can be provided at any position of the laminated optical body, and a plurality of positive C plates can be provided.
[0283] The positive C-plate may be disposed adjacent to the cholesteric liquid crystal layer, or disposed inside the cholesteric liquid crystal layer.
[0284] As a cholesteric liquid crystal layer, for example, when a light reflecting layer formed by fixing a cholesteric liquid crystal phase containing a rod-shaped liquid crystal compound is used, the light reflecting layer has a positive Rth. At this time, when light is incident from an oblique direction relative to the cholesteric liquid crystal layer, the polarization state of the reflected light and the transmitted light changes due to the effect of Rth, and sometimes the polarization degree of the transmitted light decreases. If there is a positive C plate inside or near the cholesteric liquid crystal layer, the change in the polarization state of the obliquely incident light can be suppressed, and the decrease in the polarization degree of the transmitted light can be suppressed, so it is preferred. According to the research of the inventors, the positive C plate is preferably arranged on the opposite side of the green reflecting layer relative to the blue light reflecting layer, and can also be arranged at other locations.
[0285] In this case, the in-plane retardation Re of the positive C plate is preferably 10 nm or less, and the retardation Rth in the thickness direction is preferably -600 to -100 nm, more preferably -400 to -200 nm.
[0286] Furthermore, in the stacked optical body, the positive C plate may be disposed adjacent to the phase difference layer or disposed inside the phase difference layer.
[0287] As a phase difference layer, for example, when a layer formed by fixing a rod-like liquid crystal compound is used, the phase difference layer has a positive Rth. At this time, when light is incident from an oblique direction relative to the phase difference layer, the polarization state of the transmitted light changes due to the action of Rth, and sometimes the polarization degree of the transmitted light decreases. If there is a positive C plate inside or near the phase difference layer, the change in the polarization state of the oblique incident light can be suppressed, and the decrease in the polarization degree of the transmitted light can be suppressed, so it is preferred. According to the research of the inventors, the positive C plate is preferably set on the opposite side of the linear polarizer relative to the phase difference layer, and can also be set at other locations.
[0288] In this case, the in-plane retardation Re of the positive C plate is preferably about 10 nm or less, and the retardation Rth in the thickness direction is preferably -90 to -40 nm.
[0289] <Anti-reflection layer>
[0290] The laminated optical body also preferably has an antireflection layer on the surface.
[0291] The laminated optical body has the function of reflecting specific circularly polarized light and transmitting circularly polarized light orthogonal thereto, and the reflection on the surface of the laminated optical body generally includes the reflection of undesired polarized light, thereby reducing the polarization degree of the transmitted light. Therefore, the laminated optical body preferably has an antireflection layer on the surface.
[0292] The antireflection layer may be provided on one surface of the laminated optical body or on both surfaces.
[0293] The type of anti-reflection layer is not particularly limited, and from the viewpoint of further reducing the reflectivity, moth-eye film and AR film are preferably exemplified. Furthermore, when the laminated optical body is stretched or formed, even if the film thickness changes due to stretching, high anti-reflection performance can be maintained, so moth-eye film is more preferred.
[0294] Furthermore, the anti-reflection layer may include a support. When the anti-reflection layer includes a support, when the laminated optical body is stretched or formed, the peak temperature of Tg of the support of the anti-reflection layer is preferably 170° C. or less, and more preferably 130° C. or less, from the viewpoint of facilitating the stretching or forming. Specifically, as the support, for example, a PMMA film or the like is preferred.
[0295] <Second phase difference layer>
[0296] The laminated optical body also preferably further has a second retardation layer. For example, the laminated optical body may include a cholesteric liquid crystal layer, a retardation layer, a linear polarizer, and a second retardation layer in this order.
[0297] The second retardation layer preferably converts linearly polarized light into circularly polarized light, and for example, preferably has Re of 1 / 4 wavelength. The reason for this is described below.
[0298] Light incident on the stacked optical body from the cholesteric liquid crystal layer side and passing through the cholesteric liquid crystal layer, the phase difference layer and the linear polarizer becomes linearly polarized light, a portion of which is reflected on the outermost surface on the linear polarizer side and emitted again from the surface on the cholesteric liquid crystal layer side. This light is unnecessary reflected light and may become a factor in reducing the polarization degree of the reflected light, so it is preferred to reduce it. Therefore, in order to suppress the reflection on the outermost surface on the linear polarizer side, there is a method of stacking an anti-reflection layer, but when the stacked optical body is bonded to a medium such as glass or plastic for use, even if there is an anti-reflection layer on the bonding surface of the stacked optical body, the reflection on the surface of the medium cannot be suppressed, so the anti-reflection effect cannot be obtained.
[0299] In contrast, when a second phase difference layer is provided that converts linear polarized light into circular polarized light, light that reaches the outermost surface of the linear polarizer becomes circular polarized light, and is converted into orthogonal circular polarized light when reflected from the outermost surface of the medium. After that, the light passes through the second phase difference layer again, and when it reaches the linear polarizer, the light becomes linear polarized light in the absorption axis orientation of the linear polarizer, and is absorbed by the linear polarizer. Therefore, unnecessary reflection can be prevented.
[0300] From the viewpoint of more effectively suppressing unnecessary reflection, the second retardation layer preferably has substantially anomalous dispersion properties.
[0301] <Support body>
[0302] The laminated optical body may further include a support. The support can be provided at any position, and for example, when the cholesteric liquid crystal layer, the phase difference layer, or the linear polarizer is a film transferred from a dummy support, the support can be used as the transfer destination.
[0303] The type of the support is not particularly limited, but is preferably transparent. For example, films such as cellulose acylate, polycarbonate, polysulfone, polyethersulfone, polyacrylate, polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester can be used. Among them, cellulose acylate films, cyclic polyolefin, polyacrylate, and polymethacrylate are preferred. In addition, commercial products can also be used as the support. As an example of a commercial product, if it is a cellulose acetate film, "TD80U" and "Z-TAC" manufactured by FUJIFILM Corporation can be exemplified.
[0304] Furthermore, from the viewpoint of suppressing the adverse effects on the polarization degree of transmitted light and facilitating optical inspection of the laminated optical body, the phase difference of the support is preferably small. Specifically, the in-plane delay Re is preferably less than 10 nm, and the absolute value of the delay Rth in the thickness direction is preferably less than 50 nm.
[0305] When the laminated optical body is stretched or molded, the peak temperature of tan δ of the support is preferably 170° C. or lower. From the viewpoint of enabling molding at low temperatures, the peak temperature of tan δ is preferably 150° C. or lower, more preferably 130° C. or lower.
[0306] Here, the method for measuring tan δ is described.
[0307] Using a dynamic viscoelasticity measuring apparatus (e.g., DVA-200 manufactured by ITKDVA), a film sample that has been pre-humidified in an Rh atmosphere at a temperature of 25°C and a humidity of 60% for more than 2 hours is measured under the following conditions: E" (loss modulus) and E' (storage modulus), which are used as the value for calculating tanδ (=E" / E').
[0308] Device: DVA-200 manufactured by ITKDVA
[0309] Sample: 5mm, length 50mm (gap 20mm)
[0310] Measurement conditions: tensile mode
[0311] Measuring temperature: -150℃~220℃
[0312] Heating conditions: 5℃ / min
[0313] Frequency: 1Hz
[0314] In general optical applications, stretched resin substrates are often used, and the peak temperature of tan δ is often high due to the stretching process. For example, the peak temperature of tan δ of a TAC (triacetylcellulose) substrate (TG40 manufactured by FUJIFILM Corporation) is 180° C. or higher.
[0315] The support having a tan δ peak temperature of 170° C. or less is not particularly limited, and various resin substrates can be used.
[0316] As an example, polyolefins such as polyethylene, polypropylene, and norbornene polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; acrylic resins such as polymethacrylate and polyacrylate; polyethylene naphthalate; polycarbonate; polysulfone; polyethersulfone; polyetherketone; polyphenylene sulfide and polyphenylene ether can be cited. Among them, cyclic olefin resins, polyethylene terephthalate, and acrylic resins are preferably cited, and cyclic olefin resins or polymethacrylates are particularly preferably cited, from the perspectives of easy market availability and excellent transparency.
[0317] Examples of commercially available resin substrates include TECHNOLLOY S001G, TECHNOLLOY S014G, TECHNOLLOY S000, TECHNOLLOY C001, and TECHNOLLOY C000 (SUMIKA ACRYL CO., LTD.), Lumirror U type, Lumirror FX10, and Lumirror SF20 (TORAY INDUSTR IES, INC.), HK-53A (Higashiyama Film Co., Ltd.), Teflex FT3 (Teijin DuPont Films), ESUSHINA and SCA40 (SEKISUI CHEMICAL CO., LTD.), Zeonor Film (OPTES Corporation), and Arton Film (JSRCorporation).
[0318] The thickness of the support is not particularly limited, but is preferably 5 to 300 μm, more preferably 5 to 100 μm, and even more preferably 5 to 30 μm.
[0319] [Method of bonding each layer]
[0320] The laminated optical body is a laminated body composed of a plurality of layers. The layers can also be attached by any attachment method. The attachment can be performed using an adhesive, a bonding agent, or the like.
[0321] As the adhesive, any commercially available adhesive can be used. Here, from the viewpoint of thinning and reducing the surface roughness Ra of the laminated optical body, the thickness of the adhesive is preferably 25 μm or less, more preferably 15 μm or less, and further preferably 6 μm or less. In addition, an adhesive that does not easily produce outgassing is preferred. In particular, when the laminated optical body is stretched and formed, vacuum treatment or heat treatment is sometimes required, and it is also preferred that outgassing does not occur under these conditions.
[0322] As the adhesive, any commercially available adhesive can be used. Examples of the adhesive include epoxy resin adhesives and acrylic resin adhesives.
[0323] From the viewpoint of thinning and reducing the surface roughness Ra of the laminated optical body, the thickness of the adhesive is preferably 25 μm or less, more preferably 5 μm or less, and further preferably 1 μm or less. In addition, from the viewpoint of thinning the adhesive layer and applying the adhesive to the adherend with a uniform thickness, the viscosity of the adhesive is preferably 300 cP or less, more preferably 100 cP or less, and further preferably 10 cP or less.
[0324] Furthermore, when the adherend has a surface concavo-convex, from the viewpoint of reducing the surface roughness Ra of the laminated optical body, the adhesive or bonding agent can also select suitable viscoelasticity or thickness so as to be able to embed the surface concavo-convex of the adherend layer. From the viewpoint of embedding the surface concavo-convex, the viscosity of the adhesive or bonding agent is preferably more than 50cP. Furthermore, the preferred thickness is thicker than the height of the surface concavo-convex.
[0325] As a method for adjusting the viscosity of the adhesive, for example, a method of using an adhesive containing a solvent can be cited. At this time, the viscosity of the adhesive can be adjusted according to the ratio of the solvent. In addition, by applying the adhesive to the adherend and then drying the solvent, the thickness of the adhesive can be further reduced.
[0326] In the laminated optical body, from the viewpoint of reducing unnecessary reflection and suppressing the decrease in the polarization degree of transmitted light and reflected light, the adhesive or bonding agent used to bond each layer preferably has a small refractive index difference with the adjacent layer. Specifically, the refractive index difference between adjacent layers is preferably 0.1 or less, more preferably 0.05 or less, and further preferably 0.01 or less. The refractive index of the adhesive or bonding agent can be adjusted by, for example, mixing titanium oxide particles or zirconium oxide particles.
[0327] Furthermore, although the cholesteric liquid crystal layer, phase difference layer and linear polarizer have in-plane refractive index anisotropy, the refractive index difference with adjacent layers in all directions in the plane is preferably 0.05 or less. Therefore, the adhesive or pressure-sensitive adhesive may have in-plane refractive index anisotropy.
[0328] Furthermore, the thickness of the adhesive layer between the layers is preferably 100 nm or less. If the thickness of the adhesive layer is 100 nm or less, the refractive index difference is not easily felt by light in the visible range, and unnecessary reflection can be suppressed. The thickness of the adhesive layer is more preferably 50 nm or less.
[0329] As a method for forming an adhesive layer with a thickness of 100 nm or less, for example, a method of vapor-depositing a ceramic adhesive such as silicon oxide (SiOx layer) on the bonding surface can be cited. The bonding surface of the bonding component can be subjected to surface modification treatment such as plasma treatment, corona treatment and saponification treatment before bonding. In addition, a primer layer can be provided on the bonding surface of the bonding component.
[0330] Furthermore, when there are a plurality of laminating surfaces, the type and thickness of the adhesive layer can be adjusted for each laminating surface. Specifically, for example, an adhesive layer having a thickness of 100 nm or less can be provided in the order shown in the following (1) to (3).
[0331] (1) The laminated layers are bonded to a dummy support made of a glass substrate.
[0332] (2) A SiOx layer having a thickness of 100 nm or less is formed on both the surface of the stacked layer and the surface of the stacked layer by vapor deposition or the like. The vapor deposition can be performed using SiOx powder as a vapor deposition source, for example, using a vapor deposition device (model ULEYES) manufactured by ULVAC, Inc. In addition, it is preferred that a plasma treatment be performed in advance on the surface of the formed SiOx layer.
[0333] (3) After the formed SiOx layers are bonded together, the dummy support is peeled off. The bonding is preferably performed at a temperature of 120°C, for example.
[0334] The coating, bonding or lamination of each layer can be performed by a roll-to-roll method or a single wafer method. The roll-to-roll method is preferred from the viewpoint of improving productivity and reducing axial deviation of each layer.
[0335] On the other hand, the single wafer method is preferred from the viewpoints of suitability for small-volume and high-variety production and the ability to select a special bonding method such as the aforementioned adhesive layer having a thickness of 100 nm or less.
[0336] In addition, examples of methods for applying the adhesive to an adherend include well-known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spray coating, and inkjet.
[0337] [Direct coating of each layer]
[0338] It is also preferable that there is no adhesive layer between the layers of the laminated optical body. When forming the layers, the adhesive layer can be omitted by directly coating on the adjacent layers that have already been formed.
[0339] Furthermore, when one or both of the adjacent layers are layers containing a liquid crystal compound, in order to reduce the refractive index difference in all directions in the plane, it is preferably set so that the orientation direction of the liquid crystal compound changes continuously at the interface. For example, by directly coating a phase difference layer containing a liquid crystal compound on a linear polarizer containing a liquid crystal compound and a dichroic substance, the liquid crystal compound of the phase difference layer can be oriented continuously at the interface due to the orientation restriction force of the linear polarizer based on the liquid crystal compound.
[0340] [Layer stacking order]
[0341] The laminated optical body is composed of a plurality of layers, but the order of the steps of laminating these layers is not particularly limited and can be arbitrarily selected.
[0342] For example, when transferring the functional layer from a film composed of a dummy support and a functional layer, the stacking order is adjusted so that the thickness of the film to be transferred becomes 10 μm or more, thereby suppressing the occurrence of wrinkles and cracks during transfer.
[0343] Furthermore, when another layer is stacked on a layer with large surface roughness, the surface roughness may be further magnified. Therefore, from the viewpoint of reducing the surface roughness Ra of the stacked optical body, it is preferred to stack the layers in order from the layer with the smallest surface roughness Ra.
[0344] Furthermore, the order of stacking can also be selected from the viewpoint of quality evaluation in the manufacturing process of the stacked optical body. For example, after stacking layers other than the cholesteric liquid crystal layer and performing quality evaluation by the transmission optical system, the cholesteric liquid crystal layer can be stacked and the quality evaluation by the reflection optical system can be performed.
[0345] Furthermore, the order of stacking can be selected from the viewpoint of improving the manufacturing yield of the stacked optical body or reducing the cost.
[0346] In addition, the second form of the optical film according to the first embodiment of the present invention is not a cholesteric liquid crystal layer but a film having no selective reflectivity.
[0347] The laminated optical body using the optical film can utilize various known optical elements, and the above description is followed for each optical element.
[0348] <Compound lens>
[0349] One form of the composite lens comprises a lens and the optical film of the first embodiment of the present invention. Alternatively, one form of the composite lens comprises a lens and a laminated optical body including the optical film of the first embodiment of the present invention. Figure 1 As shown, a half mirror can be formed on one side of the lens.
[0350] As the lens, a convex lens or a concave lens can be used. As the convex lens, a biconvex lens, a plano-convex lens, or a convex meniscus lens can be used. As the concave lens, a biconcave lens, a plano-concave lens, or a concave meniscus lens can be used.
[0351] As a lens used for a virtual reality display device, in order to expand the viewing angle, a convex meniscus lens and a concave meniscus lens are preferably exemplified, and from the viewpoint of further suppressing chromatic aberration, a concave meniscus lens is more preferable.
[0352] As the lens forming material, materials transparent to visible light such as glass, crystal, and plastic can be used. Since the birefringence of the lens may cause rainbow spots or light leakage, it is preferred to have a small birefringence, and a material with zero birefringence is more preferred.
[0353] <Virtual reality display device>
[0354] like Figure 1As shown, one form of a virtual reality display device includes at least an image display panel that emits polarized light and a composite lens including the optical film of the first embodiment of the present invention. In addition, it may also have additional optical components such as a half mirror or a diopter adjustment lens.
[0355] <Image display panel>
[0356] In the virtual reality display device using the optical film according to the first embodiment of the present invention, a known image display device can be used as the image display panel (image display device).
[0357] Specifically, as the image display panel, for example, there can be exemplified a display device in which self-luminous fine light-emitting bodies are arranged on a transparent substrate, such as an organic electroluminescent display device, an LED (Light Emitting Diode) display device, and a micro LED display device.
[0358] These self-luminous display devices usually have a (circular) polarizing plate attached to the display surface to prevent reflection from the display surface. Therefore, the emitted light is polarized.
[0359] In addition, a liquid crystal display device is exemplified as another image display device. The liquid crystal display device also has a polarizing plate on the surface, so the emitted light is polarized. In the following description, the organic electroluminescent display device is also referred to as OLED. OLED is the abbreviation of "Organic Light Emitting Diode".
[0360] <Molding method>
[0361] As described above, the optical film according to the first embodiment of the present invention may have a curved surface shape having a non-developable curved surface with a positive Gaussian curvature, such as a spherical surface, a parabolic surface, an ellipsoidal surface, or an aspherical surface.
[0362] An optical film (laminated optical body) having such a curved shape is formed by the following method: a planar optical film is prepared, the optical film is pressed onto a mold to be formed into a curved shape, and finally, the formed optical film is cut into the shape of a target optical element, such as a target shape such as a circle in the case of a lens having a circular planar shape.
[0363] The forming method (forming method) of the first embodiment of the present invention for forming a flat optical film into such a curved optical film includes a step of heating the optical film or the mold (heating step), a step of pressing the heated optical film onto the mold and deforming it along the shape of the mold (forming step), and a step of cutting the formed optical film (cutting step). In addition, the forming method shown below also includes the forming of a laminated optical body including the optical film of the first embodiment of the present invention.
[0364] In the following description, for convenience, a planar optical film formed into a curved shape is also referred to as a "formed film".
[0365] [Heating step (step of heating the optical film)]
[0366] In the heating step, the method of heating the film to be formed is not particularly limited, and various known methods can be used.
[0367] As an example, there can be illustrated heating based on contact with a heated solid, heating based on contact with a heated liquid, heating based on contact with a heated gas, heating based on irradiation with infrared rays, heating based on irradiation with microwaves, etc. Among them, heating based on irradiation with infrared rays is preferred because it can be remotely heated just before molding.
[0368] In addition, in the heating step, the mold may be heated instead of the formed film. The heating of the mold in this case may also be performed by a known method.
[0369] The wavelength of the infrared light used for heating is not limited, but is preferably 1.0 to 30.0 μm, more preferably 1.5 to 5 μm.
[0370] Examples of the infrared light source (IR light source) include a near-infrared lamp heater in which a tungsten filament is sealed in a quartz tube, and a wavelength control heater in which a quartz tube is multiplexed and a portion between the quartz tubes is cooled with air.
[0371] Furthermore, by imparting an irradiation distribution of infrared light to the formed film, the physical property values during forming can be controlled according to the purpose. As a method for imparting an irradiation distribution (intensity distribution) of infrared light, a known method can be used. As an example, a method of setting a density of the configuration of the IR light source and a method of arranging a filter that patterns the transmittance of infrared light between the IR light source and the formed film can be illustrated.
[0372] Examples of filters that pattern the transmittance include filters with metal vapor deposited on glass, filters with a cholesteric liquid crystal layer that selectively reflects infrared rays in a wavelength band, filters with a dielectric multilayer film that selectively reflects infrared rays in a wavelength band, and filters coated with ink that absorbs infrared rays.
[0373] In the heating process, the temperature of the formed film can be controlled by the amount of infrared rays irradiated. As an example, a method of controlling by the irradiation time of infrared rays and a method of controlling by the illuminance of infrared rays irradiated can be exemplified. In addition, the temperature of the formed film can be monitored using, for example, a non-contact radiation thermometer and a thermocouple and set as a target temperature.
[0374] In addition, in the heating step, the mold may be heated instead of the formed film. The heating of the mold in this case may also be performed by a known method.
[0375] [Forming step (a step of pressing the film to be formed against a mold and deforming it along the shape of the mold)]
[0376] In the forming step, as a method of pressing the formed film against the mold and deforming it along the shape of the mold, for example, when the mold is concave, decompression and pressurization of the forming space can be exemplified. In addition, when the mold is convex, a method of pressing the mold can also be used.
[0377] [Optical film cutting process]
[0378] As a method of cutting the formed optical film into an arbitrary shape, a cutter, scissors, a plotter, a laser cutter, or the like can be used.
[0379] The optical film having a curved surface according to the first embodiment of the present invention is an optical thin film obtained by forming a cholesteric liquid crystal layer or an optical film having no selective reflectivity into a curved surface.
[0380] The cholesteric liquid crystal layer basically has no phase difference (in-plane delay). In addition, in the present invention, the optical film without selective reflectivity is preferably an optical film with a small phase difference composed of a low-birefringence polymer resin, specifically an optical film with an in-plane delay of less than 11 nm at a wavelength of 550 nm. In addition, in the present invention, unless otherwise specified, the phase difference refers to the in-plane phase difference (phase difference in the in-plane direction).
[0381] Here, according to the study by the inventors of the present invention, when such an optical film (film to be formed) is heated and formed into a curved shape, the amount and direction of local stretching differ, resulting in generation of a phase difference within the plane.
[0382] As an example, Figure 6 Conceptually, the case where the film F to be formed is pressed against the mold M having a spherical concave surface for forming is taken as an example.
[0383] When such molding is performed, the stretched state of the formed optical film F is different between the central portion and the outer edge portion (end portion). Specifically, at this time, the film is stretched in both the circumferential and radial directions in the central portion of the optical film F. In contrast, the optical film F, i.e., the outer edge portion of the spherical mold M, is almost not stretched in the circumferential direction, but is stretched only in the radial direction.
[0384] That is, at this time, the optical film F is uniformly stretched in the center, while it is stretched only in one radial direction in the outer edge. The unevenness of the stretching amount increases from the center toward the outer edge. In other words, when the optical film is pressed on the mold M to form a curved surface, the optical film is isotropically stretched in the center, but the stretching at the outer edge, i.e., the end, is anisotropic. Moreover, the anisotropy of the stretching gradually increases from the center toward the end.
[0385] As a result, in the cholesteric liquid crystal layer, the change of the helical axis in the central part is small, but the helical axis changes in the outer edge and the vicinity of the outer edge, resulting in a phase difference. The cholesteric liquid crystal layer with a phase difference cannot properly reflect and transmit the incident light. Therefore, as described above, if such a cholesteric liquid crystal layer is used in a pancake lens constituting a virtual reality display device, it will lead to an increase in the observation of unnecessary images, that is, so-called ghosting (light leakage).
[0386] Furthermore, even if it is a so-called low-retardation film (zero-retardation film), if it is stretched uniformly in the plane direction at the center and greatly stretched only in the radial direction at the outer edge, the optical properties of the film will be unbalanced at the outer edge and near the outer edge. As a result, phase difference is generated, and the optical film with a curved surface shape has uneven phase difference in the plane, and the function as a low-retardation film is reduced.
[0387] On the other hand, according to the molding method of the first embodiment of the present invention, it is possible to suppress the generation of phase difference when a planar optical film (film to be molded) is heated and pressed against a mold to be molded into a curved shape.
[0388] As a result, according to the molding method of the first embodiment of the present invention, as described above, the optical film of the first embodiment of the present invention can be produced, which is composed of a cholesteric liquid crystal layer with a curved surface shape or a film with a curved surface shape and no selective reflectivity, and the phase difference, i.e., the in-plane delay, is small as a whole.
[0389] Hereinafter, a molding method according to a first embodiment of the present invention will be described.
[0390] As described above, the forming method of the first embodiment of the present invention includes a heating step of heating the planar optical film (formed film) as described above, a forming step of forming the heated formed film into a curved shape by pressing the heated formed film onto a mold and deforming it along the mold, and a cutting step of cutting the formed optical film.
[0391] In the first form of the molding method according to the first embodiment of the present invention, in the heating step of the molding method, the film to be molded is heated by irradiating infrared rays, and the irradiation amount of the infrared rays is provided with an in-plane distribution. In other words, in the first form of the molding method according to the first embodiment of the present invention, in the heating of the film to be molded by irradiating infrared rays, the heating amount of the film to be molded, that is, the temperature of the film to be molded after heating, is provided with an in-plane distribution.
[0392] More specifically, as a preferred form, in the first form of the molding method of the first embodiment of the present invention, a mold having a concave surface that is a non-developable surface with a positive Gaussian curvature is used, and when the position of the optical film in the plane is projected onto the mold from the normal direction of the main surface of the molded film, the infrared irradiation amount to the molded film at the concave surface vertex (bottom) is set to be greater than the infrared irradiation amount to the molded film at the concave surface end, i.e., the outer edge. In other words, in the first form of the molding method of the first embodiment of the present invention, when the molded film is heated by infrared irradiation, the temperature of the mold's concave surface vertex, i.e., the center of the molded film after molding, is set to be higher than the outer edge (end).
[0393] The main surface refers to the largest surface of a sheet-like object (film, plate-like object, layer), usually both surfaces in the thickness direction. In other words, the normal direction refers to the direction perpendicular to the main surface of the sheet-like object.
[0394] In molding by pressing against a mold, deformation, that is, stretching of the film to be molded is generally easily performed at a high temperature.
[0395] That is, in the first form of the forming method of the first embodiment of the present invention, by setting the temperature of the central portion of the formed film higher than that of the outer edge portion, most of the forming, i.e., stretching, is performed in the central portion that is stretched uniformly in the surface direction. Therefore, most of the optical film formed into a curved shape can be a region that is stretched uniformly in the surface direction without generating a phase difference.
[0396] As a result, according to the first aspect of the molding method of the first embodiment of the present invention, it is possible to produce the optical film of the first embodiment of the present invention having a small phase difference, that is, in-plane retardation as a whole.
[0397] In the first form of the forming method of the first embodiment of the present invention, the temperature difference between the center and the end of the formed film (mold) is not particularly limited and can be appropriately set according to the forming material of the formed film (laminated optical body before forming). As an example, a method can be exemplified in which the temperature of the center is set to be above Tg and the temperature of the end is set to be less than Tg according to the Tg (glass transition temperature) of the layer that mainly controls the stretching of the formed film.
[0398] This allows the central portion, which is uniformly stretched in the planar direction, to be further deformed.
[0399] Furthermore, in the first aspect of the molding method according to the first embodiment of the present invention, the change in the irradiation amount of infrared rays between the center portion and the end portions, that is, the temperature change may be stepwise or continuous.
[0400] In addition, in the first form of the forming method of the first embodiment of the present invention, the method of making the irradiation amount of infrared light different between the central part and the end part can use a known method. As an example, the above-mentioned method of setting the density of the light source and the method of arranging a filter with patterned transmittance of infrared light between the light source and the formed film can be exemplified.
[0401] As described above, in the second form of the molding method of the first embodiment of the present invention, in the molding of the optical film including the heating step, the molding step and the cutting step, the surface of the mold in contact with the optical film (film to be molded) is set to a concave surface of a non-developable curved surface with a positive Gaussian curvature and the outer peripheral shape is set to an ellipse. In addition, in the cutting step, the optical film is cut into an ellipse and the major diameter of the elliptical outer peripheral shape of the optical film cut by cutting is set to be greater than 50% and less than 95% of the major diameter of the ellipse of the outer peripheral shape of the mold.
[0402] In addition, in the present invention, as described above, the elliptical shape includes a circular shape.
[0403] That is, in the second aspect of the molding method of the first embodiment of the present invention, a flat film to be molded that is larger than the optical film having a curved surface shape to be manufactured and a large mold are used to perform the heating step and the molding step. Then, in the cutting step, only the portion that is molded or stretched by pressing on the center of the optical film, i.e., the center of the mold, is cut out.
[0404] Therefore, in the second form of the forming method of the first embodiment of the present invention, most of the optical film formed into a curved shape and cut also becomes a region that is uniformly stretched in the plane direction without generating a phase difference. As a result, in the second form of the forming method of the first embodiment of the present invention, it is also possible to produce an optical film of the present invention having a small phase difference, that is, in-plane retardation as a whole.
[0405] In a second aspect of the molding method of the first embodiment of the present invention, the major axis of the elliptical outer peripheral shape of the optical film cut out in the cutting step is set to be greater than 50% and less than 95% of the major axis of the elliptical outer peripheral shape of the mold.
[0406] When the major axis of the cut optical film is 50% or less of the major axis of the outer peripheral shape of the mold, there occurs a problem that the optical film is wasted.
[0407] When the major axis of the cut optical film is 95% or more of the major axis of the outer peripheral shape of the mold, there are many regions where the stretching amounts in the circumferential direction and radial direction differ greatly, and an optical film having a curved shape and a sufficiently small overall retardation cannot be obtained.
[0408] In the second aspect of the molding method of the first embodiment of the present invention, the major axis of the elliptical outer peripheral shape of the optical film cut out in the cutting step is preferably 60 to 90%, more preferably 70 to 90% of the major axis of the elliptical outer peripheral shape of the mold.
[0409] As described above, the third form of the molding method of the first embodiment of the present invention is in the molding of an optical film including a heating process, a molding process and a cutting process. In the heating process, the area of the optical film (film to be molded) in contact with the mold is heated to a temperature higher than the glass transition temperature Tg of the film to be molded. In the molding process, the pressing of the film to be molded to the mold is controlled just after the film to be molded contacts the mold so that the temperature of the area of the film to be molded in contact with the mold is lower than the glass transition temperature Tg.
[0410] In this molding method, when molding a laminated optical body including an optical film, that is, when the laminated optical body including an optical film is a formed film, the temperature is controlled with the glass transition temperature Tg of the most rigid member such as a support body as the target.
[0411] For example, when the mold is concave, when a flat optical film (film to be formed) is pressed against the mold, the film to be formed contacts the ends of the mold from the ends, and finally the center contacts the top (bottom) of the concave surface. In addition, unless heating is performed, the temperature of the mold is lower than the temperature of the film to be formed which is heated for forming.
[0412] That is, in the third form of the forming method of the first embodiment of the present invention, in the forming process, the central part is maintained in an easily stretchable state at a temperature above Tg, and the area contacting the mold is set to a state that is not easy to stretch, and the formed film is formed based on pressing against the mold.
[0413] Therefore, in the third form of the forming method of the first embodiment of the present invention, by performing most of the forming, i.e., stretching, in the central portion which is stretched evenly in the surface direction, most of the optical film after being formed into a curved shape can also become an area which is stretched evenly in the surface direction without generating phase difference.
[0414] As a result, according to the third aspect of the molding method of the first embodiment of the present invention, it is possible to produce the optical film of the first embodiment of the present invention having a small phase difference, that is, in-plane retardation as a whole.
[0415] In the third form of the molding method of the first embodiment of the present invention, various methods can be used as a control method for pressing the formed film to make the temperature of the area in contact with the mold lower than the glass transition temperature Tg just after the formed film contacts the mold in the molding step.
[0416] As an example, a control method can be exemplified in which, after heating the film to be formed in the heating step, the speed at which the film to be formed is pressed against the mold is adjusted to make the temperature of the region in contact with the mold lower than the glass transition temperature Tg.
[0417] The fourth form of the molding method of the first embodiment of the present invention includes a heating step of heating the mold, a molding step of pressing the heated mold against an optical film (film to be molded) to deform the optical film along the shape of the mold, and a cutting step of cutting the optical film.
[0418] In the fourth form of the forming method of the first embodiment of the present invention, the mold is a convex surface of a non-developable surface with positive Gaussian curvature, and in the forming step, the convex vertex of the mold is pressed at the center of the formed film, thereby forming the formed film.
[0419] Furthermore, it is preferred that the cut shape of the optical film in the cutting step is set to an ellipse, and further, in the molding step, the molded film is pressed against the mold in a state where the position on the ellipse line of the cut shape is restricted.
[0420] That is, in the fourth form of the molding method of the first embodiment of the present invention, a heated mold is pressed against the center of an optical film (film to be formed) to form it into a curved shape, and the temperature of the central portion of the film to be formed is raised to an initial temperature to set it in a state that is easy to stretch. As the mold is pressed, the high temperature area diffuses toward the end.
[0421] Therefore, in the fourth form of the forming method of the first embodiment of the present invention, by performing most of the forming, i.e., stretching, in the central portion which is stretched evenly in the surface direction, most of the optical film after being formed into a curved shape can also become an area which is stretched evenly in the surface direction without generating phase difference.
[0422] Preferably, the molding is performed by pressing the mold while the ends of the formed film are restricted, so that stretching near the ends where stretching is anisotropic and phase difference is likely to occur can be suppressed, and it is more preferable to perform most of the molding or stretching in the center.
[0423] As a result, according to the fourth aspect of the molding method of the first embodiment of the present invention, it is possible to produce the optical film of the first embodiment of the present invention having a small phase difference, that is, in-plane retardation as a whole.
[0424] In the fourth aspect of the forming method according to the first embodiment of the present invention, the method of limiting the end portion of the film to be formed is not limited, and various methods can be used.
[0425] As an example, there can be illustrated a method of sticking the vicinity of the end of a formed film on a support table supporting the formed film formed by pressing a convex mold using a removable adhesive sheet, a method of fixing the vicinity of the end of a formed film on a support table supporting the formed film formed by pressing a convex mold using a clamp, etc.
[0426] <Forming device>
[0427] The optical film molding apparatus that performs the molding method according to the first embodiment of the present invention is not particularly limited, and molding apparatuses having various structures can be used.
[0428] As one form of the forming device, it is composed of a mold box 1 having an opening on the top and a mold box 2 having an opening on the bottom. In order to form a forming space, the opening of the mold box 1 and the opening of the mold box 2 are spliced together directly or through other clamps, thereby forming a closed forming space.
[0429] The planar optical film (film to be formed) to be formed and the mold for forming the optical film are arranged in the forming space. In addition, when the optical film (laminated optical body) of the first embodiment of the present invention is pasted on a lens to make the above-mentioned composite lens, a lens such as a concave lens can be used as a mold, and the optical film formed into a curved surface shape can be directly pasted on the mold.
[0430] The forming device is provided with a heating mechanism such as an IR light source for heating the formed film. A plurality of heating mechanisms may be dispersedly arranged. The heating mechanism may be arranged in the forming space, or may be arranged outside the forming space and irradiate the formed film with infrared or other heat rays through a transparent window.
[0431] The film to be formed is arranged as a partition so as to divide the forming space constituted by the mold box 1 and the mold box 2 into two spaces. Furthermore, the mold is arranged in the mold box 1 below the film to be formed.
[0432] In this state, the interiors of mold boxes 1 and 2 are decompressed to a predetermined pressure, and then the film to be formed is heated. Thereafter, the pressure in mold box 2 is increased (the degree of decompression is reduced), thereby pressing the film to be formed against the mold.
[0433] [Second embodiment]
[0434] <Cholesteric liquid crystal layer (optically functional layer)>
[0435] The cholesteric liquid crystal layer (optically functional layer) of the second embodiment of the present invention is an optically functional layer containing a liquid crystal compound. The cholesteric liquid crystal layer has a phase difference region in which the phase difference increases from the center to the outside. Within the phase difference region, the slow axis direction at a point within the phase difference region is orthogonal to the direction from the center toward the point.
[0436] Furthermore, the optical layered body according to the second embodiment of the present invention is an optical layered body having a plurality of the above-mentioned cholesteric liquid crystal layers.
[0437] The cholesteric liquid crystal layer and the optical layered body according to the second embodiment of the present invention may be used alone, or may be laminated with other functional layers such as a support and an alignment film to be used as an optical film.
[0438] 〔Cholesteric liquid crystal phase〕
[0439] It is known that a cholesteric liquid crystal phase exhibits selective reflectivity at a specific wavelength.
[0440] In a general cholesteric liquid crystal phase, the central wavelength of selective reflection (selective reflection central wavelength) λ depends on the pitch P of the helix in the cholesteric liquid crystal phase, and satisfies the relationship between the average refractive index n of the cholesteric liquid crystal phase and λ=n×P. Therefore, by adjusting the helical pitch, the central wavelength of selective reflection can be adjusted.
[0441] The longer the pitch P is, the longer the selective reflection center wavelength of the cholesteric liquid crystal phase is.
[0442] In addition, as mentioned above, the pitch P of the spiral refers to the amount of one pitch of the spiral structure of the cholesteric liquid crystal phase (the period of the spiral), in other words, the amount of one turn of the spiral, that is, the length in the direction of the spiral axis when the director (the long axis direction in the case of rod-shaped liquid crystal) of the liquid crystal compound constituting the cholesteric liquid crystal phase is rotated 360°.
[0443] When the cross section of the cholesteric liquid crystal layer is observed by a scanning electron microscope (SEM (Scanning Electron Microscope)), a stripe pattern in which bright lines (bright part) and dark lines (dark part) alternately exist in the thickness direction, which originates from the cholesteric liquid crystal phase, is observed. The pitch P of the spiral period is equal to the length of two bright lines and two dark lines in the thickness direction, that is, the length of two dark lines and two bright lines in the thickness direction.
[0444] The helical pitch of the cholesteric liquid crystal phase depends on the type of chiral agent used together with the liquid crystal compound when forming the cholesteric liquid crystal layer and the concentration of the chiral agent added. Therefore, by adjusting these, a desired helical pitch can be obtained.
[0445] In addition, the pitch adjustment is described in detail in Fujifilm Research Report No. 50 (2005) pages 60-63. The method for measuring the handedness and pitch of the helix can be used in "Introduction to Liquid Crystal Chemistry Experiments" edited by the Liquid Crystal Society of Japan, published by Sigma Publishing in 2007, page 46, and "Liquid Crystal Handbook" Liquid Crystal Handbook Editorial Committee Maruzen page 196.
[0446] The cholesteric liquid crystal phase shows selective reflectivity to any left or right circularly polarized light at a specific wavelength. Whether the reflected light is right circularly polarized light or left circularly polarized light depends on the sense of the spiral of the cholesteric liquid crystal phase. The selective reflection of circularly polarized light based on the cholesteric liquid crystal phase reflects right circularly polarized light when the sense of the spiral of the cholesteric liquid crystal layer is right, and reflects left circularly polarized light when the sense of the spiral is left. Therefore, the sense of the spiral in the cholesteric liquid crystal phase can be confirmed by causing right circularly polarized light and / or left circularly polarized light to be incident on the cholesteric liquid crystal layer.
[0447] In addition, the handedness of the cholesteric liquid crystal phase can be adjusted by the type of liquid crystal compound forming the cholesteric liquid crystal layer and / or the type of chiral agent added.
[0448] Furthermore, the half width Δλ (nm) of the selective reflection wavelength region (circularly polarized light reflection wavelength region) showing selective reflection depends on Δn of the cholesteric liquid crystal phase and the pitch P of the spiral, and satisfies the relationship of Δλ=Δn×P. Therefore, the width of the selective reflection wavelength region (selective reflection wavelength region) can be controlled by adjusting Δn. Δn can be adjusted by the type of liquid crystal compound forming the cholesteric liquid crystal layer and its mixing ratio and the temperature when the orientation is fixed.
[0449] [Cholesteric liquid crystal layer]
[0450] As is known to all, the cholesteric liquid crystal layer is a layer formed by fixing a cholesteric liquid crystal phase in which a liquid crystal compound is cholesterically oriented in a spiral shape. The cholesteric liquid crystal layer has a selective reflection center wavelength determined by the spiral pitch of the cholesteric liquid crystal phase, reflects light in a wavelength region including the selective reflection center wavelength, and transmits light in other wavelength regions.
[0451] Here, a general cholesteric liquid crystal layer has no in-plane refractive index difference, and the in-plane retardation is substantially zero.
[0452] In contrast, in the present invention, the cholesteric liquid crystal layer has a structure in which the refractive index nx in the slow axis direction in the plane and the refractive index ny in the fast axis direction satisfy nx>ny in the region (phase difference region), so the cholesteric liquid crystal layer exhibits front retardation (in-plane retardation). Furthermore, in the present invention, the cholesteric liquid crystal layer has a structure in which the phase difference increases from the center to the outside in the phase difference region, and the slow axis direction at a point in the phase difference region is orthogonal to the direction from the center toward the point.
[0453] Hereinafter, a cholesteric liquid crystal layer having a region satisfying nx>ny will be described.
[0454] Figure 7 An example of such a cholesteric liquid crystal layer is conceptually shown in . The cholesteric liquid crystal layer 126 can be formed on the alignment film 124 formed on the support 120 .
[0455] In the following description, the support 120 side is also referred to as the lower side, and the cholesteric liquid crystal layer 126 side is also referred to as the upper side. Therefore, in the support 120, the cholesteric liquid crystal layer 126 side is also referred to as the upper side, and the opposite side is also referred to as the lower side. In addition, in the alignment film 124 and the cholesteric liquid crystal layer 126, the surface on the support 120 side is also referred to as the lower side, and the opposite side is also referred to as the upper side.
[0456] The support 120 supports the cholesteric liquid crystal layer when the cholesteric liquid crystal layer 126 is formed. When the support 120 is a pseudo support, various pseudo supports used when making a cholesteric liquid crystal layer can be exemplified. For example, as a pseudo support, a film-like member composed of glass, triacetyl cellulose (TAC), polyethylene terephthalate (PET), polycarbonate, polyvinyl chloride, acrylic acid, and polyolefin can be exemplified. In addition, it can be a multilayer support having a plurality of layers composed of these materials.
[0457] The alignment film 124 may be formed on the surface (upper surface) of the support 120 .
[0458] The alignment film 124 is an alignment film for aligning the liquid crystal compound 132 in a predetermined alignment state when forming the cholesteric liquid crystal layer 126 .
[0459] As the alignment film 124 , various known alignment films can be used.
[0460] For example, there can be cited friction-treated films composed of organic compounds such as polymers, oblique vapor-deposited films of inorganic compounds, films having microgrooves, films formed by LB (Langmuir-Blodgett) films based on the Langmuir-Blodgett method and layered with organic compounds such as ω-tricosanoic acid, dioctadecylmethylammonium chloride and methyl stearate, and photo-oriented films formed by emitting polarized light or non-polarized light to a photo-oriented material to form an oriented film.
[0461] The alignment film 124 may be formed by a known method according to the material used to form the alignment film.
[0462] For example, an alignment film based on a rubbing treatment can be formed by rubbing the surface of a polymer layer with paper or cloth in a certain direction.
[0463] Preferred materials for the alignment film include polyimide, polyvinyl alcohol, polymers having polymerizable groups described in JP-A-9-152509, and materials for forming alignment films described in JP-A-2005-97377, JP-A-2005-99228, and JP-A-2005-128503.
[0464] Furthermore, instead of forming the alignment film 124 , the support 120 may be subjected to a rubbing treatment, laser processing, or the like to use the support 120 as an alignment film.
[0465] The alignment film 124 is preferably a so-called photo-alignment film formed by irradiating a photo-alignment material with polarized light or non-polarized light. That is, the alignment film 124 is preferably a photo-alignment film formed by coating a photo-alignment material on the support 120 .
[0466] Polarized light can be irradiated to the photo-alignment film from a vertical direction or an oblique direction, and non-polarized light can be irradiated to the photo-alignment film from an oblique direction.
[0467] Examples of the photo-alignment material that can be used in the alignment film of the present invention include Japanese Patent Application Publication No. 2006-285197, Japanese Patent Application Publication No. 2007-76839, Japanese Patent Application Publication No. 2007-138138, Japanese Patent Application Publication No. 2007-94071, Japanese Patent Application Publication No. 2007-121721, Japanese Patent Application Publication No. 2007-140465, Japanese Patent Application Publication No. 2007-156439 The azo compounds described in Japanese Patent Publication No. 2007-133184, Japanese Patent Publication No. 2009-109831, Japanese Patent No. 3883848 and Japanese Patent No. 4151746, the aromatic ester compounds described in Japanese Patent Publication No. 2002-229039, the photosensitive adhesives described in Japanese Patent Publication No. 2002-265541 and Japanese Patent Publication No. 2002-317013 Maleimide and / or alkenyl-substituted nadimide compounds containing a tropic unit, photo-crosslinkable silane derivatives described in Japanese Patent Nos. 4205195 and 4205198, photo-crosslinkable polyimides, photo-crosslinkable polyamides, and photo-crosslinkable polyesters described in Japanese Patent Publication Nos. 2003-520878, 2004-529220, and 4162850 Preferred examples include compounds capable of photodimerization described in JP-A-9-118717, JP-A-10-506420, JP-A-2003-505561, International Publication No. 2010 / 150748, JP-A-2013-177561, and JP-A-2014-12823, particularly cinnamate compounds, chalcone compounds, and coumarin compounds.
[0468] Among them, it is preferable to use an azo compound, a photo-crosslinkable polyimide, a photo-crosslinkable polyamide, a photo-crosslinkable polyester, a cinnamate compound, and a chalcone compound.
[0469] The thickness of the alignment film 124 is not limited, and may be appropriately set to a thickness that can obtain a desired alignment function according to the material forming the alignment film.
[0470] The thickness of the alignment film is preferably 0.01 to 5 μm, more preferably 0.05 to 2 μm.
[0471] The support and the alignment film may be a dummy support that is peeled off and removed. When a dummy support is used, after the cholesteric liquid crystal layer is transferred to another laminate, the dummy support is peeled off and removed, thereby eliminating the adverse effect of the phase difference of the dummy support on the polarization degree of the transmitted light and the reflected light, and is therefore preferred.
[0472] The cholesteric liquid crystal layer 126 is formed on the surface (upper surface) of the alignment film 124 .
[0473] In addition, Figure 7 In order to simplify the drawings, the structure of the cholesteric liquid crystal layer 126 is clearly shown, and the cholesteric liquid crystal layer 126 only conceptually shows the helical orientation of the liquid crystal compound 132 in the cholesteric liquid crystal phase by 2 rotations (720° rotation). Figure 7 In FIG. 1 , only two pitches of the helical structure of the cholesteric liquid crystal phase are shown.
[0474] However, the cholesteric liquid crystal layer 126 has a spiral structure in which the liquid crystal compound 132 is stacked by spirally rotating the spiral axis along the thickness direction, similarly to the cholesteric liquid crystal layer formed by fixing the usual cholesteric liquid crystal phase, and has a structure in which the liquid crystal compound 132 is stacked by spirally rotating one circle (360° rotation) as the spiral period 1 pitch and the spirally rotated liquid crystal compound 132 is stacked with more than 1 pitch.
[0475] That is, in the present invention, the cholesteric liquid crystal phase (cholesteric liquid crystal layer) means stacking a helical structure of one pitch or more. The cholesteric liquid crystal layer exhibits the above-mentioned wavelength-selective reflectivity by stacking a helical structure of one pitch or more based on the liquid crystal compound 132 .
[0476] Therefore, in the present invention, even if a layer has a helical structure in which the liquid crystal compound 132 is stacked by spirally rotating along the helical axis in the thickness direction, a layer having a helical period of less than 1 pitch is not a cholesteric liquid crystal layer.
[0477] The cholesteric liquid crystal layer 126 is formed by fixing the cholesteric liquid crystal phase. That is, the cholesteric liquid crystal layer 126 is a layer in which the liquid crystal compound 132 (liquid crystal material) is cholesterically oriented. It is well known that the cholesteric liquid layer formed by fixing the cholesteric liquid crystal phase has wavelength selective reflectivity. As described above, the selective reflection wavelength region of the cholesteric liquid crystal layer depends on the length of the pitch of the helix 1 in the thickness direction ( Figure 7 Pitch P shown).
[0478] Here, in the present invention, the cholesteric liquid crystal layer 126 has a region (phase difference region) where the refractive index nx in the slow axis direction and the refractive index ny in the fast axis direction in the plane satisfy nx>ny. Furthermore, in the present invention, the cholesteric liquid crystal layer has a structure in which the phase difference increases from the center to the outside in the phase difference region, and the slow axis direction at a point in the phase difference region is orthogonal to the direction from the center toward the point.
[0479] In the present invention, if Figure 8As shown, the cholesteric liquid crystal layer 126 has a structure in which the angle between the molecular axes of the adjacent liquid crystal compounds 132 when the arrangement of the liquid crystal compounds 132 is observed from the helical axis direction changes stepwise. In other words, the probability of the existence of the liquid crystal compounds 132 when the arrangement of the liquid crystal compounds 132 is observed from the helical axis direction is different. As a result, the refractive index nx in the slow axis direction and the refractive index ny in the fast axis direction within the structural plane of the cholesteric liquid crystal layer 126 satisfy nx>ny.
[0480] In addition, in the following description, Figure 8 As shown, the cholesteric liquid crystal layer 126 having a structure in which the angle between the molecular axes of adjacent liquid crystal compounds 132 changes gradually when the arrangement of the liquid crystal compounds 132 is observed from the helical axis direction is also referred to as having a refractive index ellipsoid.
[0481] In the cholesteric liquid crystal layer, the reflection center wavelength is not particularly limited and may be appropriately set according to the application.
[0482] In the present invention, as the cholesteric liquid crystal layer, it is preferred to have at least a blue light reflecting layer with a reflectivity of 40% or more at a wavelength of 450nm, a green light reflecting layer with a reflectivity of 40% or more at a wavelength of 530nm, and a red light reflecting layer with a reflectivity of 40% or more at a wavelength of 630nm. That is, in an optical laminate having a multilayer cholesteric liquid crystal layer, the selective reflection center wavelengths of each cholesteric liquid crystal layer can be different from each other. If it is such a structure, it is possible to show high reflection characteristics within a wide wavelength range of the visible range, so it is preferred. In addition, the above-mentioned reflectivity is the reflectivity when the non-polarized light is incident on the reflective circular polarizer at each wavelength.
[0483] In the image display device, there is a luminescence peak in each wavelength range of blue light, green light and red light. For example, a liquid crystal display device having a backlight source including quantum dots, a liquid crystal display device having a backlight source provided with LEDs emitting blue, green and red light, an organic EL display device, a micro-LED display device, etc. have a luminescence peak with a narrower half-width in each wavelength range of blue light, green light and red light. When the half-width of the luminescence peak of each color is narrow, the color reproducibility can be improved, so it is preferred. When used in combination with these image display devices, the reflective circular polarizer (cholesteric liquid crystal layer) preferably selectively has a reflection band in the wavelength region corresponding to the luminescence peak of the image display device.
[0484] Furthermore, the blue light reflecting layer, the green light reflecting layer, and the red light reflecting layer formed by fixing the cholesteric liquid crystal phase may have a pitch gradient layer that continuously changes the helical pitch of the cholesteric liquid crystal phase in the thickness direction. For example, the green light reflecting layer and the red light reflecting layer can be continuously produced with reference to Japanese Patent Publication No. 2020-060627.
[0485] Furthermore, when the cholesteric liquid crystal layer (optical film including the cholesteric liquid crystal layer) of the present invention is stretched or formed, the reflection wavelength region as a reflective circular polarizer may sometimes shift to the short wavelength side, so it is preferable to select the reflection wavelength region by assuming the wavelength shift in advance. For example, when an optical film including a cholesteric liquid crystal layer in which a cholesteric liquid crystal phase is fixed is used as a reflective circular polarizer, the film is elongated due to stretching and forming, which sometimes causes the helical pitch of the cholesteric liquid crystal phase to become smaller, so it is preferable to pre-set the helical pitch of the cholesteric liquid crystal phase to be larger. Furthermore, it is also preferable that the reflective circular polarizer has an infrared light reflection layer having a reflectivity of 40% or more at a wavelength of 800nm, assuming the short-wave shift of the reflection wavelength region caused by stretching and forming.
[0486] Furthermore, when the stretching ratio during stretching and forming is not uniform in the plane, a suitable reflection wavelength region can be selected at each part in the plane according to the wavelength shift caused by stretching. That is, there can be regions with different reflection wavelength regions in the plane. And, preferably, the reflection wavelength region is set in advance to be wider than the desired wavelength region, assuming that the stretching ratio at each part in the plane is different.
[0487] In the present invention, in the case of an optical laminate having a plurality of cholesteric liquid crystal layers, it is preferred that a blue light reflecting layer, a green light reflecting layer, and a red light reflecting layer as cholesteric liquid crystal layers are stacked in sequence. Furthermore, when a phase difference layer is provided in addition to the plurality of cholesteric liquid crystal layers, it is preferred that the blue light reflecting layer is provided on the opposite side of the phase difference layer that converts circularly polarized light into linearly polarized light. If this configuration is adopted, light passes through the blue light reflecting layer, the green light reflecting layer, and the red light reflecting layer in sequence. The inventors of the present invention speculate that at this time, especially at oblique incidence, the polarization degree of the reflected light and the polarization degree of the transmitted light can be increased so as to be less susceptible to the influence of the Rth of each layer.
[0488] The optical layered body according to the second embodiment of the present invention is also preferably formed by alternately laminating first cholesteric liquid crystal layers formed using a rod-like liquid crystal compound and second cholesteric liquid crystal layers formed using a discotic liquid crystal compound.
[0489] Preferably, the first cholesteric liquid crystal layer is a light reflecting layer formed by fixing a cholesteric liquid crystal phase containing a rod-shaped liquid crystal compound, and the second cholesteric liquid crystal layer is a light reflecting layer formed by fixing a cholesteric liquid crystal phase containing a disc-shaped liquid crystal compound, and the first cholesteric liquid crystal layer and the second cholesteric liquid crystal layer are arranged alternately. This is because, if it is such a structure, the cholesteric liquid crystal phase containing the rod-shaped liquid crystal compound has a positive RtH, and the cholesteric liquid crystal phase containing the disc-shaped liquid crystal compound has a negative RtH, so the Rth of each other is offset, and the polarization degree of the reflected light and the transmitted light can be increased for the incident light from the oblique direction, so it is preferred. In this case, the selective reflection center wavelengths of the first cholesteric liquid crystal layer and the second cholesteric liquid crystal layer may be substantially the same or different. According to the research of the inventors, it is preferred that a blue light reflecting layer composed of a cholesteric liquid crystal phase containing a discotic liquid crystal compound, a red light reflecting layer composed of a cholesteric liquid crystal phase containing a rod-shaped liquid crystal compound, and a green light reflecting layer composed of a cholesteric liquid crystal phase containing a rod-shaped liquid crystal compound are sequentially included, and the blue light reflecting layer is provided on the opposite side of the phase difference layer that converts circularly polarized light into linearly polarized light. In addition, from the viewpoint of luminous efficiency, the order of the reflecting layers is preferably green, red, and blue from the display side.
[0490] Furthermore, from the viewpoint of compensation, the type of liquid crystal is preferably disc-shaped, rod-shaped, disc-shaped, or disc-shaped, rod-shaped, rod-shaped from the display side.
[0491] The order of the reflective layer (cholesteric liquid crystal layer) and the type of liquid crystal are merely examples, and the structures are not limited to these.
[0492] The thickness of the optical functional layer (cholesteric liquid crystal layer) may be appropriately set to obtain a desired light reflectance depending on the material forming the cholesteric liquid crystal layer, and is preferably 30 μm or less, more preferably 20 μm or less, from the viewpoint of thinning.
[0493] [Method for forming a cholesteric liquid crystal layer]
[0494] The cholesteric liquid crystal layer can be formed by fixing a cholesteric liquid crystal phase in a lamellar manner.
[0495] The structure for fixing the cholesteric liquid crystal phase only needs to be a structure in which the orientation of the liquid crystal compound that becomes the cholesteric liquid crystal phase is maintained. Generally, it is preferred that, in addition to setting the polymerizable liquid crystal compound to the orientation state of the cholesteric liquid crystal phase, a structure is formed by polymerizing and curing through ultraviolet irradiation, heating, etc. to form a layer without fluidity, and at the same time, the orientation state is not changed by an external field or external force.
[0496] In addition, in a structure where the cholesteric liquid crystal phase is fixed, it is sufficient to maintain the optical properties of the cholesteric liquid crystal phase, and the liquid crystal compound may not exhibit liquid crystallinity in the cholesteric liquid crystal layer. For example, a polymerizable liquid crystal compound may become high molecular weight by a curing reaction and may lose liquid crystallinity.
[0497] As a material used for forming a cholesteric liquid crystal layer in which a cholesteric liquid crystal phase is fixed, a liquid crystal composition containing a liquid crystal compound is mentioned as an example. The liquid crystal compound is preferably a polymerizable liquid crystal compound.
[0498] Furthermore, the liquid crystal composition used for forming the cholesteric liquid crystal layer may further contain a surfactant and a chiral agent.
[0499] The polymerizable liquid crystal compound may be a rod-like liquid crystal compound or a disc-like liquid crystal compound.
[0500] As examples of rod-shaped polymerizable liquid crystal compounds that form a cholesteric liquid crystal phase, rod-shaped nematic liquid crystal compounds can be cited. As rod-shaped nematic liquid crystal compounds, preferably used are azomethines, azoxyls, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolans, and alkenylcyclohexylbenzonitriles. Not only low molecular weight liquid crystal compounds but also high molecular weight liquid crystal compounds can be used.
[0501] The polymerizable liquid crystal compound can be obtained by introducing a polymerizable group into the liquid crystal compound. Examples of the polymerizable group include unsaturated polymerizable groups, epoxy groups and aziridine groups, preferably unsaturated polymerizable groups, more preferably ethylenically unsaturated polymerizable groups. The polymerizable group can be introduced into the molecules of the liquid crystal compound by various methods. The number of polymerizable groups possessed by the polymerizable liquid crystal compound is preferably 1 to 6, more preferably 1 to 3.
[0502] Examples of polymerizable liquid crystal compounds include compounds described in Makromol.Chem., Vol. 190, p. 2255 (1989), Advanced Materials, Vol. 5, p. 107 (1993), U.S. Pat. No. 4,683,327, U.S. Pat. No. 5,622,648, U.S. Pat. No. 5,770,107, International Publication No. 95 / 22586, International Publication No. 95 / 24455, International Publication No. 97 / 00600, International Publication No. 98 / 23580, International Publication No. 98 / 52905, Japanese Patent Application Publication No. 1-272551, Japanese Patent Application Publication No. 6-16616, Japanese Patent Application Publication No. 7-110469, Japanese Patent Application Publication No. 11-80081 and Japanese Patent Application Publication No. 2001-328973. Two or more polymerizable liquid crystal compounds may be used simultaneously. When two or more polymerizable liquid crystal compounds are used simultaneously, the alignment temperature can be lowered.
[0503] In addition, as polymerizable liquid crystal compounds other than the above, cyclic organopolysiloxane compounds having a cholesteric phase as disclosed in Japanese Patent Application Laid-Open No. 57-165480 can be used. Furthermore, as the polymer liquid crystal compound, a polymer having a mesogen group exhibiting liquid crystal introduced into the main chain, the side chain, or both the main chain and the side chain, a polymer cholesteric liquid crystal having a cholesteric group introduced into the side chain, a liquid crystal polymer as disclosed in Japanese Patent Application Laid-Open No. 9-133810, and a liquid crystal polymer as disclosed in Japanese Patent Application Laid-Open No. 11-293252 can be used.
[0504] As the discotic liquid crystal compound, for example, liquid crystal compounds described in JP-A-2007-108732 and JP-A-2010-244038 can be preferably used.
[0505] The amount of the polymerizable liquid crystal compound added to the liquid crystal composition is preferably 75 to 99.9% by mass, more preferably 80 to 99% by mass, and even more preferably 85 to 90% by mass, relative to the solid content mass of the liquid crystal composition (mass excluding the solvent).
[0506] <<Surfactant>>
[0507] The liquid crystal composition used in forming the cholesteric liquid crystal layer may contain a surfactant.
[0508] The surfactant is preferably a compound that can function as an alignment control agent that helps to orient the cholesteric liquid crystal phase stably and quickly. Examples of the surfactant include silicone surfactants and fluorine surfactants, and preferably fluorine surfactants are used.
[0509] Specific examples of the surfactant include compounds described in paragraphs
[0082] to
[0090] of JP-A-2014-119605, and paragraphs
[0031] to
[0034] of JP-A-2012-203237.
[0510] The compounds described in, the compounds exemplified in paragraphs
[0092] and
[0093] of JP-A-2005-99248, paragraphs
[0076] to
[0078] and paragraphs
[0082] to
[0085] of JP-A-2002-129162
[0511] The compounds exemplified in , and the fluoro(meth)acrylate polymers described in paragraphs
[0018] to
[0043] of JP-A-2007-272185, and the like.
[0512] The surfactant may be used alone or in combination of two or more.
[0513] As the fluorine-based surfactant, compounds described in paragraphs
[0082] to
[0090] of JP-A-2014-119605 are preferred.
[0514] The amount of the surfactant added in the liquid crystal composition is preferably 0.01 to 10% by mass, more preferably 0.01 to 5% by mass, and even more preferably 0.02 to 1% by mass, relative to the total mass of the liquid crystal compound.
[0515] <<Chiral reagents (optically active compounds)>>
[0516] The chiral agent has the function of twisting the helical structure of the cholesteric liquid crystal phase. The handedness or helical period pitch of the twisted helix varies depending on the compound, so the chiral agent can be selected according to the purpose.
[0517] The chiral agent is not limited, and known compounds (for example, Liquid Crystal Device Handbook, Chapter 3, Item 4-3, TN (twisted nematic), STN (Super Twisted Nematic) Chiral Agents, page 199, edited by the 142nd Committee of the Japan Society for the Promotion of Science, 1989), isosorbide and dehydrated mannitol derivatives, etc. can be used.
[0518] Chiral agents generally contain asymmetric carbon atoms, but axial asymmetric compounds or planar asymmetric compounds that do not contain asymmetric carbon atoms can also be used as chiral agents. Examples of axial asymmetric compounds or planar asymmetric compounds include binaphthyl, helical hydrocarbons, cycloaromatic hydrocarbons and their derivatives. The chiral agent may have a polymerizable group. When both the chiral agent and the liquid crystal compound have a polymerizable group, a polymer having a repeating unit derived from the polymerizable liquid crystal compound and a repeating unit derived from the chiral agent can be formed by the polymerization reaction of the polymerizable chiral agent and the polymerizable liquid crystal compound. In this form, the polymerizable group possessed by the polymerizable chiral agent is preferably a group of the same type as the polymerizable group possessed by the polymerizable liquid crystal compound. Therefore, the polymerizable group of the chiral agent is also preferably an unsaturated polymerizable group, an epoxy group or an aziridine group, more preferably an unsaturated polymerizable group, and further preferably an olefinic unsaturated polymerizable group.
[0519] Also, the chiral agent may be a liquid crystal compound.
[0520] When the chiral agent has a photoisomerizable group, it is preferred because a pattern of a desired reflection wavelength corresponding to the emission wavelength can be formed by emitting active light through a photomask such as coating and orientation. As the photoisomerizable group, an isomerization site of a compound showing photochromic properties, an azo group, an oxyazolyl group or a cinnamoyl group is preferred. As specific compounds, compounds described in JP-A-2002-80478, JP-A-2002-80851, JP-A-2002-179668, JP-A-2002-179669, JP-A-2002-179670, JP-A-2002-179681, JP-A-2002-179682, JP-A-2002-338575, JP-A-2002-338668, JP-A-2003-313189, JP-A-2003-313292, etc. can be used.
[0521] The content of the chiral agent in the liquid crystal composition is preferably 0.01 to 200 mol %, more preferably 1 to 30 mol %, based on the molar amount of the liquid crystal compound.
[0522] <<Polymerization initiator>>
[0523] When the liquid crystal composition contains a polymerizable compound, it preferably contains a polymerization initiator. In the embodiment in which the polymerization reaction is carried out by ultraviolet irradiation, the polymerization initiator used is preferably a photopolymerization initiator that can start the polymerization reaction by ultraviolet irradiation.
[0524] Examples of photopolymerization initiators include α-carbonyl compounds (described in the specifications of U.S. Patent No. 2367661 and U.S. Patent No. 2367670), acyloin ethers (described in the specification of U.S. Patent No. 2448828), α-hydrocarbon-substituted aromatic acyloin compounds (described in the specification of U.S. Patent No. 2722512), polynuclear quinone compounds (described in the specifications of U.S. Patent No. 3046127 and U.S. Patent No. 2951758), a combination of a triaryl imidazole dimer and p-aminophenone (described in the specification of U.S. Patent No. 3549367), acridine and phenazine compounds (described in Japanese Patent Application Laid-Open No. 60-105667 and the specification of U.S. Patent No. 4239850), and oxadiazole compounds (described in the specification of U.S. Patent No. 4212970).
[0525] Among them, the polymerization initiator is preferably a dichroic radical polymerization initiator.
[0526] A dichroic free radical polymerization initiator refers to a photopolymerization initiator that has absorption selectivity for light of a specific polarization direction and is excited by the polarized light to generate free radicals. That is, a dichroic free radical polymerization initiator refers to a polymerization initiator that has different absorption selectivity for light of a specific polarization direction and light of a polarization direction orthogonal to the light of the specific polarization direction.
[0527] The details and specific examples are described in WO2003 / 054111 pamphlet.
[0528] Specific examples of the dichroic radical polymerization initiator include polymerization initiators of the following chemical formula: In addition, as the dichroic radical polymerization initiator, polymerization initiators described in paragraphs
[0046] to
[0097] of JP-T 2016-535863A can be used.
[0529] [Chemical formula 1]
[0530]
[0531] The content of the photopolymerization initiator in the liquid crystal composition is preferably 0.1 to 20% by mass, more preferably 0.5 to 12% by mass, based on the content of the liquid crystal compound.
[0532] <<Crosslinking agent>>
[0533] The liquid crystal composition may contain a crosslinking agent to increase the film strength after curing and improve durability. As the crosslinking agent, a crosslinking agent that is cured by ultraviolet rays, heat, moisture, etc. can be preferably used.
[0534] As a crosslinking agent, there is no particular limitation, and it can be appropriately selected according to the purpose, for example, multifunctional acrylate compounds such as trimethylolpropane tri(meth)acrylate and pentaerythritol tri(meth)acrylate can be cited; epoxy compounds such as (meth) acrylic acid glycidyl ester and ethylene glycol diglycidyl ether; aziridine compounds such as 2,2-bishydroxymethylbutanol-tris[3-(1-aziridine) propionate] and 4,4-bis(ethyleneiminocarbonylamino) diphenylmethane; isocyanate compounds such as hexamethylene diisocyanate and biuret type isocyanate; polyoxazoline compounds having oxazoline groups in the side chain; and alkoxysilane compounds such as vinyltrimethoxysilane, N-(2-aminoethyl) 3-aminopropyltrimethoxysilane, etc. In addition, according to the reactivity of the crosslinking agent, a known catalyst can be used, which can improve the productivity in addition to improving the film strength and durability. These can be used alone or in combination of two or more.
[0535] The content of the crosslinking agent is preferably 3 to 20% by mass, more preferably 5 to 15% by mass, relative to the solid content of the liquid crystal composition. If the content of the crosslinking agent is within the above range, the effect of increasing the crosslinking density is easily obtained, and the stability of the cholesteric liquid crystal phase is further improved.
[0536] <<Other additives>>
[0537] To the liquid crystal composition, a polymerization inhibitor, an antioxidant, an ultraviolet absorber, a light stabilizer, a colorant, metal oxide fine particles, and the like may be further added as necessary within a range that does not deteriorate optical properties.
[0538] The liquid crystal composition is preferably used as a liquid when forming a cholesteric liquid crystal layer. The liquid crystal composition may contain a solvent. The solvent is not particularly limited and can be appropriately selected according to the purpose, and is preferably an organic solvent.
[0539] The organic solvent is not particularly limited and can be appropriately selected according to the purpose. For example, ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters and ethers can be mentioned. These can be used alone or in combination of two or more. Among them, ketones are preferred when considering environmental load.
[0540] When forming the cholesteric liquid crystal layer, it is preferred that the liquid crystal composition is applied to the surface where the cholesteric liquid crystal layer is to be formed, the liquid crystal compound is aligned in a cholesteric liquid crystal phase, and then the liquid crystal compound is cured to form the cholesteric liquid crystal layer.
[0541] For example, when forming a cholesteric liquid crystal layer 126 on the orientation film 124, it is preferred to apply a liquid crystal composition on the orientation film 124, orient the liquid crystal compound to a cholesteric liquid crystal phase, and then solidify the liquid crystal compound to form a cholesteric liquid crystal layer 126 with a fixed cholesteric liquid crystal phase.
[0542] The liquid crystal composition can be applied by any known method that can uniformly apply a liquid to a sheet, such as a printing method such as inkjet printing and roll printing, and a method such as spin coating, bar coating, and spray coating.
[0543] The applied liquid crystal composition is dried and / or heated as required, and then cured to form a cholesteric liquid crystal layer. In the drying and / or heating process, the liquid crystal compound in the liquid crystal composition is oriented in a cholesteric liquid crystal phase. When heating, the heating temperature is preferably below 200° C., more preferably below 130° C.
[0544] The oriented liquid crystal compound is further polymerized as needed. The polymerization may be any of thermal polymerization and photopolymerization based on light emission, preferably photopolymerization. Ultraviolet light is preferably used for light emission. The emission energy is preferably 20 mJ / cm 2 ~50J / cm 2 , more preferably 50 to 1500 mJ / cm 2 In order to promote the photopolymerization reaction, light emission may be carried out under heating conditions or in a nitrogen atmosphere. The wavelength of the emitted ultraviolet rays is preferably 250 to 430 nm.
[0545] (Liquid Crystal Elastomer)
[0546] In the present invention, a liquid crystal elastomer can be used in a cholesteric liquid crystal layer. A liquid crystal elastomer is a mixed material of a liquid crystal and an elastomer. For example, it has a structure in which a mesogen group with liquid crystal rigidity is introduced into a soft polymer network with rubber elasticity. Therefore, it is characterized by having soft mechanical properties and elasticity. In addition, the orientation state of the liquid crystal is strongly related to the macroscopic shape of the system, so it is characterized by that when the orientation state of the liquid crystal changes due to temperature and electric field, a macroscopic deformation corresponding to the change in orientation degree is performed. For example, when the liquid crystal elastomer is heated to a temperature at which the nematic phase changes to an isotropic phase with random orientation, the sample shrinks along the orientation direction, and the amount of shrinkage increases as the temperature rises, that is, as the orientation degree of the liquid crystal decreases. The deformation is thermally reversible, and the original shape will be restored when the temperature is lowered to the nematic phase again. On the other hand, when the liquid crystal elastomer of the cholesteric liquid crystal phase is heated and the orientation degree of the liquid crystal is reduced, a macroscopic elongation deformation occurs in the direction of the spiral axis, so the spiral pitch length increases, and the reflection center wavelength of the selective reflection peak is shifted to the long wavelength side. This change is also thermally reversible, and as the temperature decreases, the reflection center wavelength returns to the short wavelength side.
[0547] <<Refractive index ellipsoid of cholesteric liquid crystal layer>>
[0548] As described above, the cholesteric liquid crystal layer 126 has a structure, namely, a refractive index ellipsoid, in which the angle between the molecular axes of the adjacent liquid crystal compounds 132 changes stepwise when the arrangement of the liquid crystal compounds 132 is observed from the helical axis direction.
[0549] For more information about the refractive index ellipsoid, see Fig. 9 and Fig.10 to explain.
[0550] Fig. 9 This is a diagram showing a portion (amount of 1 / 4 pitch) of a plurality of liquid crystal compounds twistedly aligned along the helical axis as viewed from the helical axis direction (z direction). Fig.10 This is a diagram conceptually showing the existence probability of a liquid crystal compound observed from the helical axis direction. Fig. 9 This is an example of a case where the liquid crystal compound is a rod-shaped liquid crystal compound, and the long axis of the rod-shaped liquid crystal compound is the molecular axis. When the liquid crystal compound is a discotic liquid crystal compound, the disc plane direction of the discotic liquid crystal compound when observed from the helical axis direction is the molecular axis.
[0551] exist Fig. 9 In the embodiment, the liquid crystal compound whose molecular axis is parallel to the y direction is set as C1, the liquid crystal compound whose molecular axis is parallel to the x direction is set as C7, and the liquid crystal compounds between C1 and C7 are set as C2 to C6 from the liquid crystal compound C1 side to the liquid crystal compound C7 side. The liquid crystal compounds C1 to C7 are twisted along the helical axis and rotated 90° between the liquid crystal compound C1 and the liquid crystal compound C7. The length between the liquid crystal compounds whose angle of the twisted liquid crystal compounds is changed by 360° is set as 1 pitch ( Figure 7 When the helical axis direction from the liquid crystal compound C1 to the liquid crystal compound C7 is ( Fig. 9 The length of the strip (in the direction perpendicular to the paper plane) is 1 / 4 of the pitch.
[0552] like Fig. 9 As shown, the angles formed by the molecular axes of the adjacent liquid crystal compounds observed from the z direction (helical axis direction) are different in the 1 / 4 pitch from the liquid crystal compound C1 to the liquid crystal compound C7. Fig. 9 In the example shown, the angle θ between the liquid crystal compound C1 and the liquid crystal compound C2 is 1 is greater than the angle θ formed by the liquid crystal compound C2 and the liquid crystal compound C3 2 , the angle θ formed by the liquid crystal compound C2 and the liquid crystal compound C3 2 is greater than the angle θ formed by the liquid crystal compound C3 and the liquid crystal compound C4 3 , the angle θ formed by the liquid crystal compound C3 and the liquid crystal compound C4 3is greater than the angle θ formed by the liquid crystal compound C4 and the liquid crystal compound C5 4 , the angle θ formed by the liquid crystal compound C4 and the liquid crystal compound C5 4 is greater than the angle θ formed by the liquid crystal compound C5 and the liquid crystal compound C6 5 , the angle θ formed by the liquid crystal compound C5 and the liquid crystal compound C6 5 is greater than the angle θ formed by the liquid crystal compound C6 and the liquid crystal compound C7 6 , the angle θ formed by the liquid crystal compound C6 and the liquid crystal compound C7 6 Minimum.
[0553] That is, the twisted orientation of the liquid crystal compounds C1 to C7 is such that the angle formed by the molecular axes of the adjacent liquid crystal compounds decreases from the liquid crystal compound C1 side toward the liquid crystal compound C7 side. For example, when the interval (interval in the thickness direction) between the liquid crystal compounds is set to be substantially constant, the rotation angle per unit length in the 1 / 4 pitch from the liquid crystal compound C1 to the liquid crystal compound C7 decreases from the liquid crystal compound C1 side toward the liquid crystal compound C7 side.
[0554] In the cholesteric liquid crystal layer 126 , a structure in which the rotation angle per unit length changes is repeated at a ¼ pitch, and the liquid crystal compound is twisted and aligned.
[0555] Here, when the rotation angle per unit length is constant, the angle between the molecular axes of adjacent liquid crystal compounds is constant, so the probability of the existence of the liquid crystal compound observed from the helical axis direction is the same in all directions. Therefore, at this time, the cholesteric liquid crystal layer does not have anisotropy (isotropy) of the refractive index in the in-plane direction.
[0556] On the other hand, as described above, by setting the structure in which the rotation angle per unit length in the 1 / 4 pitch from the liquid crystal compound C1 to the liquid crystal compound C7 decreases from the liquid crystal compound C1 side toward the liquid crystal compound C7 side, as conceptually shown in FIG. Fig.10 , the probability of existence of the liquid crystal compound observed from the helical axis direction is higher in the x direction than in the y direction. The probability of existence of the liquid crystal compound is different in the x direction and the y direction, so the refractive index is different in the x direction and the y direction, thus generating refractive index anisotropy. In other words, refractive index anisotropy is generated in the plane perpendicular to the helical axis.
[0557] The refractive index nx in the x direction where the probability of the existence of the liquid crystal compound is high is greater than the refractive index ny in the y direction where the probability of the existence of the liquid crystal compound is low. Therefore, the refractive index nx and the refractive index ny satisfy nx>ny.
[0558] The x direction where the existence probability of the liquid crystal compound is high becomes the slow axis direction in the plane of the cholesteric liquid crystal layer 126 , and the y direction where the existence probability of the liquid crystal compound is low becomes the fast axis direction in the plane of the cholesteric liquid crystal layer 126 .
[0559] In this way, in the twisted orientation of the liquid crystal compound, a structure in which the rotation angle per unit length changes in a 1 / 4 pitch (a structure having a refractive index ellipsoid) can be formed as follows: after applying a composition to become a cholesteric liquid crystal layer, polarized light in a direction orthogonal to the helical axis is irradiated on the cholesteric liquid crystal phase (composition layer).
[0560] By irradiation with polarized light, the cholesteric liquid crystal phase is distorted to generate in-plane retardation, that is, the refractive index nx can be set to be greater than the refractive index ny.
[0561] Specifically, the liquid crystal compound having a molecular axis in the direction consistent with the polarization direction of the irradiated polarized light polymerizes. At this time, since only a part of the liquid crystal compound polymerizes, the chiral agent at this position is excluded and moves to another position.
[0562] Therefore, at a position where the molecular axis of the liquid crystal compound is close to the polarization direction, the amount of chiral agent decreases, and the rotation angle of the twisted orientation decreases. On the other hand, at a position where the molecular axis of the liquid crystal compound is orthogonal to the polarization direction, the amount of chiral agent increases, and the rotation angle of the twisted orientation increases.
[0563] Therefore, if Fig. 9 As shown, the structure can be set as follows: in the liquid crystal compound twisted along the helical axis, in the 1 / 4 pitch from the liquid crystal compound whose molecular axis is parallel to the polarization direction to the liquid crystal compound orthogonal to the polarization direction, the angle formed by the molecular axes of adjacent liquid crystal compounds decreases as it moves from the liquid crystal compound side parallel to the polarization direction toward the liquid crystal compound side orthogonal to the polarization direction. That is, by irradiating the cholesteric liquid crystal phase with polarized light, the probability of existence of the liquid crystal compound is different in the x direction and the y direction, and the refractive index is different in the x direction and the y direction, thereby generating refractive index anisotropy. As a result, the refractive index nx and the refractive index ny of the optical element 10 satisfy nx>ny. That is, the cholesteric liquid crystal layer can be set to have a structure with a refractive index ellipsoid.
[0564] The polarized light irradiation can be performed simultaneously with the fixation of the cholesteric liquid crystal phase, or the polarized light irradiation can be performed first and then the fixation can be further performed by non-polarized light irradiation, or the fixation can be performed first by non-polarized light irradiation and then the photo-alignment can be performed by polarized light irradiation. In order to obtain a large delay, it is preferred to perform only polarized light irradiation or to perform polarized light irradiation first. Polarized light irradiation is preferably performed in an inert gas atmosphere with an oxygen concentration of less than 0.5%. The irradiation energy is preferably 20 mJ / cm 2 ~10J / cm2 , more preferably 100 to 800 mJ / cm 2 The illumination is preferably 20 to 1000 mW / cm 2 , more preferably 50 to 500 mW / cm 2 , more preferably 100 to 350 mW / cm 2 The type of the liquid crystal compound that is cured by polarized light irradiation is not particularly limited, but liquid crystal compounds having an ethylenically unsaturated group as a reactive group are preferred.
[0565] In addition, as a method for distorting the cholesteric liquid crystal phase by polarized light irradiation to produce in-plane retardation, there can be cited a method using a dichroic liquid crystal polymerization initiator (WO03 / 054111A1) or a method using a rod-shaped liquid crystal compound having a photo-alignment functional group such as a cinnamoyl group in the molecule (Japanese Patent Application Laid-Open No. 2002-6138).
[0566] The irradiation light may be ultraviolet light, visible light or infrared light. That is, depending on the liquid crystal compound and polymerization initiator contained in the coating film, light that can polymerize the liquid crystal compound may be appropriately selected.
[0567] By using a dichroic radical polymerization initiator as the polymerization initiator, when the composition layer is irradiated with polarized light, polymerization of a liquid crystal compound having a molecular axis in a direction that coincides with the polarization direction can be more preferably carried out.
[0568] The slow axis direction, fast axis direction, refractive index nx and refractive index ny in the plane can be measured using an ellipsometer M-2000UI manufactured by JA Woollam. The refractive index nx and refractive index ny can be measured using the average birefringence n according to the measured value of the phase difference Δn×d. ave Here, Δn = nx-ny, average refractive index n ave =(nx+ny) / 2. Usually, the average refractive index of liquid crystal is about 1.5, so nx and ny can also be obtained using this value. In addition, when measuring the slow axis direction, fast axis direction, refractive index nx and refractive index ny in the plane of the cholesteric liquid crystal layer used in the present invention, the wavelength of 20nm is subtracted from the half-value wavelength on the side shorter than the selective reflection center wavelength on the cholesteric liquid crystal layer as the measurement wavelength. In this way, the influence of the delayed optical rotation component originating from the cholesteric selective reflection can be minimized, so that high-precision measurement can be performed.
[0569] Furthermore, a cholesteric liquid crystal layer having a refractive index ellipsoid can also be formed by applying a composition to form a cholesteric liquid crystal layer, or by fixing a cholesteric liquid crystal phase, or by stretching the cholesteric liquid crystal layer in a state where the cholesteric liquid crystal phase is semi-fixed.
[0570] Here, in the second embodiment of the present invention, the slow axis of the cholesteric liquid crystal layer having a refractive index ellipsoid preferably has a plurality of orientations in the plane, and the orientation is preferably changed according to the application. For example, when forming a curved surface such as a part of a sphere, if it is substantially arranged in a concentric circle shape, the phase difference caused by the stretching during the forming can be offset, so it is preferred. In addition, the delay after forming is preferably less than 10nm.
[0571] Specifically, the cholesteric liquid crystal layer has a phase difference region in which the phase difference increases from the center to the outside, and in the phase difference region, the slow axis direction at a point in the phase difference region is orthogonal to the direction from the center toward the point. Fig.12 , a cholesteric liquid crystal layer of such a structure is described.
[0572] Fig.12 This is a diagram conceptually showing the slow axis of the cholesteric liquid crystal layer of the present invention.
[0573] exist Fig.12 In FIG. 1 , the slow axis direction in a micro region within the plane of the cholesteric liquid crystal layer is indicated by an arrow, and the magnitude of the phase difference in the region is indicated by the length of the arrow.
[0574] exist Fig.12 In the example, at the center O, the phase difference is substantially 0. Also, for example, at the dashed line r extending from the center O toward the outside, 1 On the line represented by 1 , click P 2 , click P 3 The slow axis direction in each position (micro area) is consistent with the single-point dash line r 1 are roughly orthogonal. And, point P 2 The phase difference at the position is greater than point P 1 The phase difference at the position, and point P 3 The phase difference at the position is greater than point P 2 That is, the further away from the center O the position is, the greater the phase difference is.
[0575] like Fig.12 As shown, in all directions from the center O toward the outside, the phase difference of the cholesteric liquid crystal layer increases from the center O toward the outside, and the slow axis direction at a certain point is approximately orthogonal to the line segment connecting the point and the center O. In other words, the slow axis direction is approximately orthogonal to the radial direction. In this way, in the cholesteric liquid crystal layer, the slow axis direction and the phase difference of each micro region in the plane are different depending on the position in the plane.
[0576] And, preferably, Fig.12 As shown, at positions with the same distance from the center O, the phase difference is approximately the same.
[0577] exist Fig.12 In the cholesteric liquid crystal layer shown in FIG. 1 , when a tangent line is drawn that touches all arrows indicating the slow axis in a region with the same phase difference, the following is drawn: Fig.12 The circle with the center O shown by the dotted line in the middle. Draw circles with different diameters according to the phase difference, and the multiple circles become concentric circles with the common center O. In the following description, Fig.12 The pattern of slow axes shown is also called a concentric circle pattern.
[0578] The slow axis of the cholesteric liquid crystal layer according to the second embodiment of the present invention has a concentric pattern. Therefore, when the cholesteric liquid crystal layer is formed into a curved surface such as a part of a sphere, for example, the phase difference caused by stretching during the forming can be cancelled.
[0579] Specifically, in the case of conventional cholesteric liquid crystal layers, the angle formed by the molecular axes of adjacent liquid crystal compounds observed from the helical axis direction is approximately constant, that is, the rotation angle per unit length is constant. Therefore, conventional cholesteric liquid crystal layers do not have isotropy of refractive index anisotropy (phase difference) at all positions (micro regions) within the plane.
[0580] When this conventional cholesteric liquid crystal layer is formed into a curved surface such as a part of a sphere, when viewed from above, the area near the center is stretched at a constant stretch ratio regardless of the direction, so no anisotropy is generated. However, the area near the end of the formed area is stretched at different stretch ratios in the circumferential and radial directions. As a result, the probability of the existence of the liquid crystal compound deviates in the circumferential and radial directions, thereby causing anisotropy (phase difference) of the refractive index. Specifically, the closer the area is to the end, the smaller the circumferential stretch ratio is and the higher the radial stretch ratio is. Therefore, the radial liquid crystal compound has a high probability of existence and has a slow axis in the radial direction (reference Figure 6 ). In this way, when the conventional cholesteric liquid crystal layer is formed into a curved surface such as a part of a sphere, the magnitude of the phase difference generated will be different depending on the position in the surface. Therefore, when the formed cholesteric liquid crystal layer is used as a reflective circular polarizer of a pancake lens constituting a virtual reality display device, it will not be possible to properly reflect and transmit the incident light, resulting in increased light leakage. In the virtual reality display device, the light leakage is visually recognized as a double image.
[0581] In contrast, the cholesteric liquid crystal layer of the second embodiment of the present invention has a concentric pattern in which the phase difference increases toward the outside and the slow axis direction is approximately orthogonal to the radial direction. Therefore, for example, when formed into a curved surface such as a part of a sphere, when viewed from above, the area near the center is stretched at a constant stretching ratio regardless of the direction, so no anisotropy is generated and the phase difference remains approximately 0. On the other hand, in the area near the end of the formed area, it is stretched at a small stretching ratio in the circumferential direction and a high stretching ratio in the radial direction, but in the area near the end, the slow axis direction is approximately orthogonal to the radial direction, that is, the probability of the existence of liquid crystal compounds in the direction approximately orthogonal to the radial direction (circumferential direction) is high, so by being stretched in the radial direction, the difference in the probability of the existence of liquid crystal compounds in the radial and circumferential directions becomes smaller. As a result, the anisotropy (phase difference) of the refractive index in the area close to the end becomes smaller. In this way, according to the circumferential stretching ratio and radial stretching ratio at each position during molding, the cholesteric liquid crystal layer is given a concentric pattern in which the phase difference increases toward the outside and the slow axis direction is approximately orthogonal to the radial direction, thereby reducing the phase difference (approximately 0) in each area within the surface after molding. Therefore, when the cholesteric liquid crystal layer of the present invention is molded to be used as a reflective circular polarizer constituting a pancake lens of a virtual reality display device, the incident light can be appropriately reflected and transmitted to reduce light leakage. As a result, it is possible to suppress the visual recognition of ghosting in the virtual reality display device.
[0582] A method for forming a cholesteric liquid crystal layer having a concentric pattern in which the phase difference increases toward the outside and the slow axis direction is substantially orthogonal to the radial direction will be described.
[0583] As described above, a cholesteric liquid crystal layer having a phase difference can be formed by irradiating polarized light to a cholesteric liquid crystal phase (composition layer) after applying a composition that becomes a cholesteric liquid crystal layer. At this time, the probability of the existence of the liquid crystal compound in the polarization direction becomes higher, forming a refractive index ellipsoid such as a slow axis direction, so the polarized light can be irradiated in a manner that the direction of the irradiated polarized light becomes a concentric circular pattern in which the phase difference increases toward the outside and the slow axis direction is approximately orthogonal to the radial direction.
[0584] Since the slow axis of the cholesteric liquid crystal layer having a refractive index ellipsoid has a plurality of directions in the plane, a known polarized light exposure method can be used. As a specific example, it can be produced by the method described in Japanese Patent Application Laid-Open No. 2008-233903.
[0585] As an example, the use of Fig.11 A method of irradiating polarized light while rotating the cholesteric liquid crystal phase (composition layer) using the mask shown.
[0586] Fig.11The mask shown is formed such that the top of the triangular-shaped transmission part is roughly consistent with the center and becomes elongated toward the end. In addition, the transmittance of the transmission part (the transmittance of the light of the wavelength used in exposure) is low on the center side and becomes high toward the end. Through the mask, the cholesteric liquid crystal phase (composition layer) is irradiated with polarized light in a direction orthogonal to the radial direction, and the cholesteric liquid crystal phase (composition layer) is rotated at the center of the top of the triangular-shaped transmission part, thereby forming a concentric circular pattern in which the phase difference increases toward the outside and the slow axis direction is roughly orthogonal to the radial direction.
[0587] <Optical laminate>
[0588] The optical laminate of the second embodiment of the present invention includes, for example, the optical functional layer (cholesteric liquid crystal layer) and a substrate film. The optical functional layer may be a laminate of a plurality of layers. Examples of the substrate film include polyacrylate and polymethacrylate.
[0589] <Optical components>
[0590] The optical component of the second embodiment of the present invention is a molded body (curved optical functional layer) forming the above-mentioned cholesteric liquid crystal layer. When the optical component is used in a pancake lens type virtual reality display device, the optical component can be designed to have a suitable shape with a curved surface to obtain a wide field of view, low chromatic aberration, low distortion and excellent MTF.
[0591] The shape of the molded body may be various shapes such as a part of a sphere, a parabolic body of revolution, an aspherical lens shape, etc. Furthermore, the shape of the molded body may be a shape that matches the shape of the stacked lenses.
[0592] Specifically, the molded body obtained by molding the cholesteric liquid crystal layer of the second embodiment of the present invention (optical laminate including the cholesteric liquid crystal layer of the second embodiment of the present invention) can be set to the same structure as the first form of the optical film of the first embodiment of the present invention described above. That is, the molded body has a curved surface shape of a non-developable surface with a positive Gaussian curvature. As such a curved surface shape, various curved surface shapes having a non-developable surface with a positive Gaussian curvature such as a sphere, a parabola, an ellipse, an aspheric surface whose curvature changes from the center to the outside (for example, a non-center-symmetric curved surface such as a curved surface that is not optically axisymmetric in the radial direction in the case of a circular lens) can be used.
[0593] Furthermore, in the molded body having such a curved surface shape, the peripheral shape (shape of the peripheral end), i.e., the plane shape, is not limited, and various shapes such as an ellipse, an oblong shape other than an ellipse, a polygon, and an irregular shape can be used. Among them, an ellipse is preferred. In addition, in the present invention, an ellipse also includes a circle.
[0594] The planar shape refers to the shape when viewed from the normal direction of the top (bottom) of the curved surface of the molded body. For example, when the molded body having a curved surface shape is a lens, it is generally the shape when viewed from the optical axis direction.
[0595] The molded body obtained by molding the cholesteric liquid crystal layer of the second embodiment of the present invention (the optical laminate including the cholesteric liquid crystal layer of the second embodiment of the present invention) can be set to an evaluation wavelength (measurement wavelength) as a wavelength obtained by subtracting 20 nm from the half-value wavelength on the side shorter than the selective reflection center wavelength on the cholesteric liquid crystal layer, and to a wavelength at which the in-plane retardation A at the evaluation wavelength in the center is less than 2% of the evaluation wavelength and the in-plane retardation B at the evaluation wavelength in the outer edge is less than 2% of the evaluation wavelength.
[0596] The method for producing such a molded body (curved optically functional layer) includes: a cholesteric liquid crystal layer production step of producing the cholesteric liquid crystal layer; and a molding step of performing curved molding in a manner that eliminates the phase difference of the cholesteric liquid crystal layer.
[0597] Furthermore, preferably, in the molding process, the cholesteric liquid crystal layer is disposed on a molding mold and deformed along a concave molding surface so that the bottom of the concave molding surface of the molding mold having the concave molding surface is consistent with the center of the cholesteric liquid crystal layer (the center of the phase difference region).
[0598] The molding method using the molding die having such a concave molding surface can utilize a conventionally known method such as vacuum molding.
[0599] <Virtual reality display device>
[0600] The virtual reality display device of the second embodiment of the present invention includes at least an image display device that emits polarized light and the optical component (molded body) of the second embodiment of the present invention described above, and may also have additional optical components such as a half mirror and a diopter adjustment lens.
[0601] As an image display device that emits polarized light, a known image display device can be used. For example, an organic electroluminescent display device, an LED (Light Emitting Diode) display device, a micro-LED display device, and other display devices in which self-luminous fine light-emitting bodies are arranged on a transparent substrate can be exemplified. These self-luminous display devices usually have a (circular) polarizer attached to the display surface to prevent reflection of the display surface. Therefore, the emitted light is polarized. In addition, a liquid crystal display device is exemplified as another image display device. The liquid crystal display device also has a polarizer on the surface, so the emitted light is polarized. In the following description, the organic electroluminescent display device is also referred to as an OLED. OLED is the abbreviation of "Organic Light Emitting Diode".
[0602] Specifically, the virtual reality display device according to the second embodiment of the present invention can be configured as follows: Figure 1 The virtual reality display device shown is the same as the virtual reality display device of the first embodiment except that a molded body formed by molding the cholesteric liquid crystal layer of the second embodiment of the present invention (an optical laminate including the cholesteric liquid crystal layer of the second embodiment of the present invention) is used as the optical laminate 100.
[0603] Example
[0604] Below, give embodiment, feature of the present invention is described in more detail.In addition, material, usage, ratio, processing content, processing sequence etc. shown below, as long as do not depart from the gist of the present invention, then can be appropriately changed.And, as long as do not depart from the gist of the present invention, also can adopt the structure other than the structure shown below.
[0605] [Example of the first embodiment]
[0606] [Preparation of coating solutions R-1 to R-6 for reflective layer]
[0607] The following compositions were stirred and dissolved in a container maintained at 70° C. to prepare reflective layer coating solutions R-1 to R-6, respectively. Here, R represents a coating solution using rod-like liquid crystals.
[0608]
[0609] Amount of chiral agent in coating solution (R-1 to R-6) containing rod-shaped liquid crystal compound
[0610] [Table 1]
[0611]
[0612] Mixture of rod-like liquid crystal compounds
[0613] [Chemical formula 2]
[0614]
[0615] In the above mixture, the numerical values are mass %, and R is a group bonded to an oxygen atom. Furthermore, the average molar absorption coefficient of the above rod-shaped liquid crystal at a wavelength of 300 to 400 nm is 140 / mol·cm.
[0616] Chiral Reagent A
[0617] [Chemical formula 3]
[0618]
[0619] Surfactant F1
[0620] [Chemical formula 4]
[0621]
[0622] Surfactant F2
[0623] [Chemical formula 5]
[0624]
[0625] Photopolymerization initiator B
[0626] [Chemical formula 6]
[0627]
[0628] Chiral reagent A is a chiral reagent whose helical twisting power (HTP: Helical Twisting Power) decreases due to light.
[0629] (Reflective layer coating liquid D-1 to D-7)
[0630] The compositions shown below were stirred and dissolved in a container maintained at a temperature of 50° C. to prepare reflective layer coating solutions D-1 to D-7. Here, D represents a coating solution using a discotic liquid crystal.
[0631]
[0632] Amount of chiral agent in coating solution containing discotic liquid crystal compound [Table 2]
[0633]
[0634] Discotic liquid crystal compound (A)
[0635] [Chemical formula 7]
[0636]
[0637] Discotic liquid crystal compound (B)
[0638] [Chemical formula 8]
[0639]
[0640] Polymerizable monomer E1
[0641] [Chemical formula 9]
[0642]
[0643] Surfactant F4
[0644] [Chemical formula 10]
[0645]
[0646] [Production of optical film 1]
[0647] As a pseudo support, a PET (polyethylene terephthalate) film (A4100 manufactured by TOYOBO CO., LTD.) having a thickness of 50 μm was prepared. The PET film had an easy-adhesion layer on one side.
[0648] The surface without the easy-adhesive layer of the PET film was rubbed, and the reflective layer coating liquid R-1 prepared above was applied using a wire bar coater, and then dried at 110°C for 120 seconds to vaporize the solvent, and then heated and aged at 100°C for 1 minute to obtain a uniform orientation state. Thereafter, the film was irradiated at 40°C in the atmosphere through an exposure mask with an irradiation dose of 5 mJ / cm 2 The light from a high pressure mercury lamp was used for photoisomerization. The image of the exposure mask used at this time is shown in Figure 5 A rotationally symmetric exposure mask was used, which had a high transmittance at the center and a transmittance that decreased toward the ends. Then, the film was irradiated at 100°C with an illuminance of 80 mW / cm2 in a low oxygen atmosphere (less than 100 ppm). 2 、Irradiation 500mJ / cm 2 The red light reflecting layer composed of a cholesteric liquid crystal layer was cured by light from a metal halide lamp. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the red light reflecting layer after curing became 4.5 μm. By photoisomerization using an exposure mask, a patterned cholesteric liquid crystal layer with an in-plane distribution of the helical pitch of the cholesteric liquid crystal having a central wavelength of 701 nm in the center and a central wavelength of 683 nm in the end was produced.
[0649] Next, the discharge rate was 150W·min / m 2 After the red light reflecting layer was subjected to corona treatment, the reflective layer coating liquid D-2 was applied to the corona treated surface using a wire bar coater. Next, the coating film was dried at 70°C for 2 minutes to vaporize the solvent, and then heated and aged at 115°C for 3 minutes to obtain a uniform orientation state. Thereafter, the film was irradiated at 40°C through an exposure mask in the atmosphere at an irradiation dose of 5 mJ / cm 2 The light from a high-pressure mercury lamp was used to perform photoisomerization. The exposure mask used at this time was the same as the exposure mask used for the red light reflecting layer of the first layer. After that, the film was heated and aged at 115°C for 3 minutes to obtain a uniform orientation state. Then, the film was irradiated at 100°C with an illumination of 80mW / cm in a low oxygen atmosphere (less than 100ppm). 2 、Irradiation 500mJ / cm 2 The yellow light reflecting layer was cured by light from a metal halide lamp, thereby forming a yellow light reflecting layer on the red light reflecting layer. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the yellow light reflecting layer after curing became 3.3 μm.
[0650] Next, the reflective layer coating liquid R-3 was applied to the yellow light reflective layer using a wire bar coater, and then dried at 110°C for 120 seconds to vaporize the solvent, and then heated and aged at 100°C for 1 minute to obtain a uniform orientation state. Then, the film was irradiated at 40°C in the atmosphere through an exposure mask with an irradiation dose of 5 mJ / cm 2 The light from a high-pressure mercury lamp was used to perform photoisomerization. The exposure mask used at this time was the same as the exposure mask used for the first red light reflecting layer. Afterwards, the film was irradiated at 100°C with an illumination of 80 mW / cm in a low oxygen atmosphere (less than 100 ppm). 2 、Irradiation 500mJ / cm 2 The green light reflecting layer was formed on the yellow light reflecting layer by curing with the light of a metal halide lamp. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the green light reflecting layer after curing became 2.7 μm.
[0651] Next, the discharge rate was 150W·min / m 2 After the red light reflecting layer was subjected to corona treatment, the reflective layer coating liquid D-4 was applied to the corona treated surface using a wire bar coater. Next, the coating film was dried at 70°C for 2 minutes to vaporize the solvent, and then heated and aged at 115°C for 3 minutes to obtain a uniform orientation state. Thereafter, the film was irradiated at 40°C through an exposure mask in the atmosphere at an irradiation dose of 5 mJ / cm 2The light from a high-pressure mercury lamp was used to perform photoisomerization. The exposure mask used at this time was the same as the exposure mask used for the red light reflecting layer of the first layer. After that, the film was heated and aged at 115°C for 3 minutes to obtain a uniform orientation state. Then, the film was irradiated at 100°C with an illumination of 80mW / cm in a low oxygen atmosphere (less than 100ppm). 2 、Irradiation 500mJ / cm 2 The blue light reflecting layer was formed on the green light reflecting layer by curing with the light of a metal halide lamp. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the blue light reflecting layer after curing became 2.5 μm.
[0652] In this way, the optical film 1 was produced.
[0653] The reflective layer coating liquid, amount of chiral agent, reflection center wavelength and film thickness used for producing the optical film 1 are shown in the following table.
[0654] Here, the reflection center wavelength refers to the characteristic of a light-reflecting film having a reflection band using a cholesteric liquid crystal phase, and refers to the midpoint of the spectral band reflected by the film. Specifically, it can be obtained by calculating the average value of the wavelength on the short wavelength side and the wavelength on the long wavelength side showing half the peak reflectivity. The reflection center wavelength (center wavelength of reflected light) was confirmed by making a film coated with only a single layer. The film thickness was confirmed by SEM.
[0655] Reflective layer (cholesteric liquid crystal layer) of optical film 1
[0656] [Table 3-1]
[0657]
[0658] [Production of optical film 2]
[0659] Optical film 2 was produced by the same method as that of reflective circular polarizer 1 except that the number of layers was increased to 8 and the reflective layer coating liquid, amount of chiral agent, reflection center wavelength and film thickness were changed as shown in the following table.
[0660] Reflective layer of optical film 2 (cholesteric liquid crystal layer)
[0661] [Table 3-2]
[0662]
[0663] [Production of Optical Film 3 and Optical Film 4]
[0664] In the production process of the optical film 1 , the optical film 3 was produced without performing isomerization exposure using an exposure mask used when producing the reflective layer (cholesteric liquid crystal layer).
[0665] In the production process of the optical film 2 , the optical film 4 was produced without performing isomerization exposure using an exposure mask used when producing the reflective layer (cholesteric liquid crystal layer).
[0666] [Production of optical film 5]
[0667] Optical film 5 increases the number of reflective layers (cholesteric liquid crystal layers) to 5 layers, and changes the reflective layer coating solution and film thickness as shown in Table 3-3 below. In addition, as a photo-alignment film for aligning cholesteric liquid crystals, a light interference layer (positive C plate layer) made with the light interference layer coating solution shown below was used.
[0668] <Coating liquid PC-1 for optical interference layer>
[0669] The composition shown below was stirred and dissolved in a container maintained at a temperature of 60° C. to prepare a coating liquid PC-1 for an optical interference layer.
[0670]
[0671] Photopolymerization initiator C
[0672] [Chemical formula 11]
[0673]
[0674] Photoacid generator
[0675] [Chemical formula 12]
[0676]
[0677] Hydrophilic polymer
[0678] [Chemical formula 13]
[0679]
[0680] Vertical alignment agent
[0681] [Chemical formula 14]
[0682]
[0683] Viscosity reducer
[0684] [Chemical formula 15]
[0685]
[0686] Materials for interlayer photo-alignment films
[0687] [Chemical formula 16]
[0688]
[0689] Stabilizer
[0690] [Chemical formula 17]
[0691]
[0692] As a support, a TAC film (triacetylcellulose film (TG60, manufactured by FUJIFILM Corporation)) having a thickness of 60 μm was prepared.
[0693] The optical interference layer coating liquid PC-1 prepared above was applied onto the support (TAC film) using a wire bar coater, and then dried at 80° C. for 60 seconds.
[0694] Then, the samples were irradiated at 300 mJ / cm2 in a low oxygen atmosphere (100 ppm) at 78°C. 2 The liquid crystal compound was cured by ultraviolet LED light (wavelength 365 nm), and the cleavable groups of the interlayer photo-alignment film material were cleaved. Then, the fluorine atom-containing substituent was removed by heating at 115° C. for 25 seconds.
[0695] Thus, a positive C plate layer as a light interference layer having a cinnamoyl group on the outermost surface and having a film thickness of 80 nm was formed.
[0696] The refractive index nI measured by an interferometer film thickness meter OPTM (manufactured by Otsuka Electronics Co., Ltd., least square analysis) was 1.57. The Rth at a wavelength of 550 nm measured by Axoscan (manufactured by Axometrics, Inc.) was -8 nm.
[0697] Next, the C-plate side was irradiated with an illumination of 7 mW / cm 2 , irradiation dose 7.9mJ / cm 2 Polarized UV (wavelength 313nm).
[0698] Polarized UV at a wavelength of 313 nm is obtained by allowing ultraviolet light emitted from a mercury lamp to pass through a bandpass filter having a transmission band at a wavelength of 313 nm and a wire grid polarizer.
[0699] After the reflective layer coating liquid R-5 was applied by a wire bar coater, it was dried at 110°C for 72 seconds. Thereafter, it was irradiated at 100°C with an illuminance of 80 mW / cm 2 、Irradiation 500mJ / cm 2The green light reflecting layer (first light reflecting layer) composed of a cholesteric liquid crystal layer was cured by light from a metal halide lamp. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the green light reflecting layer after curing became 2.4 μm.
[0700] Next, the discharge rate was 150W·min / m 2 After the surface of the green light reflecting layer was subjected to corona treatment, the reflecting layer coating liquid D-5 was applied to the corona treated surface using a wire bar coater. Next, the coating film was dried at 70°C for 2 minutes to vaporize the solvent, and then heated and aged at 115°C for 3 minutes to obtain a uniform orientation state.
[0701] Then, the coating film was maintained at 45° C. and irradiated with ultraviolet light (300 mJ / cm 2 ) to cure, thereby forming a blue light reflecting layer (second light reflecting layer) on the green light reflecting layer. The light irradiation is performed from the cholesteric liquid crystal layer side. At this time, the coating thickness is adjusted so that the film thickness of the blue light reflecting layer after curing becomes 1.7 μm.
[0702] Next, the reflective layer coating liquid D-6 was applied to the blue light reflective layer using a wire bar coater. Next, the coating film was dried at 70°C for 2 minutes to vaporize the solvent, and then heated and aged at 115°C for 3 minutes to obtain a uniform orientation state. Thereafter, the coating film was maintained at 45°C and irradiated with ultraviolet light (300 mJ / cm 2 ) to cure, thereby forming a second blue light reflecting layer (third light reflecting layer) on the blue light reflecting layer. The light irradiation is performed from the cholesteric liquid crystal layer side. At this time, the coating thickness is adjusted so that the film thickness of the blue light reflecting layer after curing becomes 3.8 μm.
[0703] Next, the reflective layer coating liquid R-6 was applied onto the second blue light reflective layer using a wire bar coater, and then dried at 110° C. for 72 seconds.
[0704] Afterwards, the samples were irradiated at 100°C with an illumination of 80 mW and an irradiation dose of 500 mJ / cm in a low oxygen atmosphere (less than 100 ppm). 2 The red light reflecting layer (the fourth light reflecting layer) is formed on the second blue light reflecting layer by curing with the light of a metal halide lamp. The light irradiation is performed from the cholesteric liquid crystal layer side. At this time, the coating thickness is adjusted so that the film thickness of the red light reflecting layer after curing becomes 4.8 μm.
[0705] Next, the discharge rate was 150W·min / m 2After the red light reflecting layer surface was subjected to corona treatment, the reflecting layer coating liquid D-7 was applied to the corona treated surface using a wire bar coater.
[0706] Next, the coating film was dried at 70° C. for 2 minutes to vaporize the solvent, and then heated and aged at 115° C. for 3 minutes, thereby obtaining a uniform orientation state.
[0707] Then, the coating film was maintained at 45° C. and irradiated with ultraviolet light (300 mJ / cm 2 ) was cured to form a yellow light reflecting layer (fifth light reflecting layer) on the red light reflecting layer. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the yellow light reflecting layer after curing became 3.3 μm.
[0708] Regarding each reflective layer of the produced optical film 5 , the reflective layer coating liquid, the amount of the chiral agent, the reflection center wavelength, and the film thickness are shown in the following table.
[0709] Reflective layer (cholesteric liquid crystal layer) of optical film 5
[0710] [Table 3-3]
[0711]
[0712] [Preparation of optical film 6]
[0713] As the optical film 6 having optical isotropy used in the molding test, a PMMA film (polymethacrylate film) having a film thickness of 50 μm was prepared.
[0714] [Forming method 1]
[0715] The optical film 2 was bonded to the PMMA film via a pressure-sensitive adhesive sheet (NCF-D692(5)) manufactured by LINTEC Corporation, and the film was set in a molding device in a state where a release film was peeled off from the pressure-sensitive adhesive sheet to expose the pressure-sensitive adhesive surface.
[0716] The molding space in the molding device is composed of mold box 1 and mold box 2 separated by optical film 1. On mold box 1 located on the lower side of optical film 2, a convex meniscus lens LE1076-A (2 inches in diameter, focal length 100 mm, and curvature radius of 65 mm on the concave side) manufactured by Thorlabs, Inc. is arranged as a mold with the concave side facing upward.
[0717] Furthermore, a transparent window is provided at the upper portion of the mold box 2 located on the upper side of the optical film 1, and an IR light source for heating the optical film is provided outside the transparent window.
[0718] An annular pattern infrared reflection filter is arranged between the IR light source and the optical film 2. The annular pattern infrared reflection filter is obtained by cutting a cholesteric liquid crystal layer that reflects infrared light with a wavelength of 2.2 μm to 3.0 μm at a reflectivity of about 50% according to the outer peripheral shape of the mold and further cutting the center portion into a circular shape with a diameter of 1 inch. At this time, the pattern infrared reflection filter is arranged so that the center portion is located at the center portion of the mold when viewed from directly above.
[0719] Next, the inside of the mold box 1 and the mold box 2 were evacuated by a vacuum pump until the pressure became 0.1 atmosphere or less.
[0720] Next, as a step of heating the optical film 2, infrared rays were irradiated to heat the optical film 1 until the center reached 108° C. and the ends reached 99° C. The PMMA film used as a support has a glass transition temperature Tg of 105° C., so the goal was to achieve a state in which the center was easily stretched but the ends were not easily stretched during molding.
[0721] Next, as a step of pressing the optical film 2 against the mold and deforming it along the shape of the mold, gas was flowed from a cylinder into the mold box 2 and pressurized to 300 kPa to press the optical film 2 against the mold. The optical film 2 was attached to the mold via an adhesive sheet and used as a composite lens 1 directly.
[0722] Finally, the optical film is cut out from the portion protruding from the lens as the mold, thereby obtaining the optical film 2 molded into a curved surface in a state of being bonded to the lens.
[0723] [Forming method 2]
[0724] The optical film 2 was bonded to the PMMA film via a pressure-sensitive adhesive sheet (NCF-D692(5)) manufactured by LINTEC Corporation, and the film was set in a molding device in a state where a release film was peeled off from the pressure-sensitive adhesive sheet to expose the pressure-sensitive adhesive surface.
[0725] The molding space in the molding device is composed of a mold box 1 and a mold box 2 separated by an optical film 2. On the mold box 1 located below the optical film 2, an object formed by expanding the periphery of a convex meniscus lens LE1076-A (2 inches in diameter, 100 mm in focal length, and 65 mm in radius of curvature on the concave side) manufactured by Thorlabs, Inc. with clay is arranged as a mold with the concave side facing upward. Based on the expansion of the clay, the curved surface of the concave side of the lens is extended in a state of substantially almost the same curvature, so that the shape of the mold including the lens and the clay becomes 3 inches in diameter and 65 mm in radius of curvature of the concave side.
[0726] Furthermore, a transparent window is provided at the upper portion of the mold box 2 located on the upper side of the optical film 2 , and an IR light source for heating the optical film 2 is provided outside the transparent window.
[0727] Next, the inside of the mold box 1 and the mold box 2 were evacuated by a vacuum pump until the pressure became 0.1 atmosphere or less.
[0728] Next, as a step of heating the optical film 2, infrared rays were irradiated to heat the center of the optical film 2 until it reached 108°C. The glass transition temperature Tg of the PMMA film used as a support is 105°C, so a temperature higher than that is targeted.
[0729] Next, as a step of pressing the optical film 2 against the mold and deforming it along the shape of the mold, gas is flowed from a cylinder into the mold box 2 and pressurized to 300 kPa to press the optical film 2 against the mold. The optical film 2 is attached to the lens portion in the mold via an adhesive sheet and used directly as a composite lens 2, and the clay disposed outside the lens is removed.
[0730] Finally, the optical film 2 was cut out from the protruding portion of the lens, thereby obtaining an optical film 2 formed into a curved surface in a state of being bonded to the lens. The diameter of the cut optical film 2 at this time was 67% of the diameter of the mold formed by the lens and clay.
[0731] [Forming method 3]
[0732] The optical film 2 was bonded to the PMMA film via a pressure-sensitive adhesive sheet (NCF-D692(5)) manufactured by LINTEC Corporation, and the film was set in a molding device in a state where a release film was peeled off from the pressure-sensitive adhesive sheet to expose the pressure-sensitive adhesive surface.
[0733] The molding space in the molding device is composed of mold box 1 and mold box 2 separated by optical film 1. On mold box 1 located on the lower side of optical film 2, a convex meniscus lens LE1076-A (2 inches in diameter, focal length 100 mm, and curvature radius of 65 mm on the concave side) manufactured by Thorlabs, Inc. is arranged as a mold with the concave side facing upward.
[0734] Furthermore, a transparent window is provided at the upper portion of the mold box 2 located on the upper side of the optical film 2, and an IR light source for heating the optical film is provided outside the transparent window.
[0735] Next, the inside of the mold box 1 and the mold box 2 were evacuated by a vacuum pump until the pressure became 0.1 atmosphere or less.
[0736] Next, as a step of heating the optical film 2 , infrared rays were irradiated to heat the optical film 2 until the center portion thereof reached 108° C.
[0737] Next, as a process of pressing the optical film 2 against the mold and deforming it along the shape of the mold, gas is flowed from the cylinder into the mold box 2 and pressurized to 300 kPa, and the optical film 2 is pressed against the mold. At this time, the pressurization speed until 300 kPa is adjusted so that the temperature of the center portion immediately after being pressed against the mold becomes 99°C. The glass transition temperature Tg of the PMMA film used as a support is 105°C, so the goal is to keep the center portion easy to stretch during molding and change the end portion to a state that is not easy to stretch during molding.
[0738] The optical film 2 is attached to the mold via an adhesive sheet and directly used as the composite lens 3 .
[0739] Finally, the optical film 2 is cut out from the portion protruding from the lens as the mold, thereby obtaining the optical film 2 molded into a curved surface in a state of being bonded to the lens.
[0740] [Forming method 4]
[0741] The optical film 2 was bonded to the PMMA film via a pressure-sensitive adhesive sheet (NCF-D692(5)) manufactured by LINTEC Corporation, and the release film was peeled off from the pressure-sensitive adhesive sheet to expose the pressure-sensitive adhesive surface.
[0742] As a mold having a concave surface shape, a convex meniscus lens LE1076-A (2 inches in diameter, focal length 100 mm, curvature radius of the concave surface side 65 mm) manufactured by Thorlabs, Inc. was placed with the concave surface facing upward.
[0743] The optical film 2 was placed on the mold with the adhesive surface facing downward. Thereby, the optical film 2 was restrained by the edge of the concave mold.
[0744] Next, a convex mold with a curvature radius of 65 mm was prepared, and the mold was heated to 120° C. in an oven.
[0745] Next, the convex mold is arranged so that the apex of the convex part is located at the center of the concave mold when viewed from above, and the optical film 2 is slowly pressed. As a result, during molding, the temperature of the center part first rises and becomes a state that is easy to stretch, and as the convex surface is pressed in, the high temperature area spreads to the end.
[0746] The optical film 2 is attached to the mold via an adhesive sheet and directly used as the composite lens 4. Finally, the portion of the optical film protruding from the lens as the mold is cut to obtain the optical film 2 formed into a curved surface in a state attached to the lens.
[0747] The optical films 1, 3, 4 and 5 are formed by the forming method 1 to produce composite lenses 5, 6, 7 and 8, respectively.
[0748] [Production of polarizing plate laminate]
[0749] [Production of positive C plate 1]
[0750] The film thickness was adjusted with reference to the method described in paragraphs 0132 to 0134 of Japanese Patent Application Laid-Open No. 2016-053709 to produce a positive C plate 1. In the positive C plate 1, Re=0.2 nm, Rth=-310 nm.
[0751] [Preparation of phase difference layer 1]
[0752] The anomalous dispersion retardation layer 1 was prepared by referring to the method described in paragraphs 0151 to 0163 of Japanese Patent Application Laid-Open No. 2020-084070. In the retardation layer 1, Re=146 nm, and Rth=73 nm.
[0753] 〔Fabrication of Linear Polarizer〕
[0754] [Production of Cellulose Acylate Film 1]
[0755] (Preparation of Core Layer Cellulose Acylate Dopant)
[0756] The following composition was placed in a mixing tank and stirred to dissolve the components, thereby preparing a cellulose acetate solution to be used as a doping agent for the cellulose acylate in the core layer.
[0757]
[0758] Compound F
[0759] [Chemical formula 18]
[0760]
[0761] (Preparation of outer layer cellulose acylate dopant)
[0762] To 90 parts by mass of the core layer cellulose acylate doping agent was added 10 parts by mass of the following matting agent solution to prepare a cellulose acetate solution as an outer layer cellulose acylate doping agent.
[0763]
[0764] (Production of Cellulose Acylate Film 1)
[0765] After filtering the core layer cellulose acylate dopant and the outer layer cellulose acylate dopant using filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm, a total of three layers of the core layer cellulose acylate dopant and the outer layer cellulose acylate dopant on both sides thereof are simultaneously cast from a casting port onto a drum at 20° C. (belt casting machine).
[0766] Next, the film was peeled at a solvent content of about 20% by mass, and both ends of the film in the width direction were clamped by a tenter clip, stretched in the transverse direction at a stretching ratio of 1.1 times, and dried.
[0767] Thereafter, the film was carried between rolls of a heat treatment device and further dried to produce an optical film having a thickness of 40 μm, which was referred to as a cellulose acylate film 1. The in-plane retardation of the obtained cellulose acylate film 1 was 0 nm.
[0768] <Formation of Photo-Alignment Layer PA1>
[0769] The coating liquid S-PA-1 for forming an alignment layer described later was continuously coated on the cellulose acylate film 1 using a wire bar. The support body with the coating film formed was dried with warm air at 140° C. for 120 seconds, and then the coating film was irradiated with polarized ultraviolet rays (10 mJ / cm 2 , using an ultra-high pressure mercury lamp), thereby forming a photo-alignment layer PA1 with a film thickness of 0.3 μm.
[0770]
[0771] Polymer M-PA-1
[0772] [Chemical formula 19]
[0773]
[0774] Acid Generator PAG-1
[0775] [Chemical formula 20]
[0776]
[0777] Acid Generator CPI-110F
[0778] [Chemical formula 21]
[0779]
[0780] <Formation of light absorption anisotropic layer P1>
[0781] The following coating liquid SP-1 for forming an anisotropic light absorbing layer was continuously coated on the obtained orientation layer PA1 using a wire bar. Next, the coating layer P1 was heated at 140°C for 30 seconds and cooled to room temperature (23°C). Next, it was heated at 90°C for 60 seconds and cooled to room temperature again. Thereafter, an LED lamp (central wavelength 365nm) was used at an illumination of 200mW / cm 2 The light absorption anisotropic layer P1 was formed on the alignment layer PA1 under the irradiation condition of 2 seconds. The film thickness was 1.6 μm.
[0782]
[0783] Dichroic substance D-1
[0784] [Chemical formula 22]
[0785]
[0786] Dichroic substance D-2
[0787] [Chemical formula 23]
[0788]
[0789] Dichroic substance D-3
[0790] [Chemical formula 24]
[0791]
[0792] Polymer liquid crystal compound MP-1
[0793] [Chemical formula 25]
[0794]
[0795] Low molecular weight liquid crystal compound M-1
[0796] [Chemical formula 26]
[0797]
[0798] Surfactant F-1
[0799] [Chemical formula 27]
[0800]
[0801] The obtained phase difference layer 1 is bonded to the side of the obtained positive C plate 1 opposite to the support.
[0802] Next, the light absorption anisotropic layer P1 was transferred so that the layer on the opposite side of the dummy support of the light absorption anisotropic layer P1 was located on the side of the positive C plate 1. After the transfer, the dummy support of the light absorption anisotropic layer P1 was peeled off and removed.
[0803] The light absorption anisotropic layer P1 was transferred according to the following procedure.
[0804] (1) Using a wire bar coater, UV adhesive Chemiseal U2084B (manufactured by CHEMITECH INC., with a refractive index of n1.60 after curing) was applied to the support side of the positive C plate 1 to a thickness of 2 μm. The light absorption anisotropic layer P1 was laminated thereon using a laminator so that the side opposite to the dummy support contacted the UV adhesive.
[0805] (2) After nitrogen flushing in a flushing box until the oxygen concentration becomes 100 ppm or less, the light absorption anisotropic layer P1 is cured by irradiating with ultraviolet light from a high pressure mercury lamp from the dummy support side. The illuminance is 25 mW / cm 2 , the irradiation dose is 1000mJ / cm 2 .
[0806] (3) Finally, the dummy support of the light absorption anisotropic layer P1 is peeled off.
[0807] The layers were stacked so that the slow axis of the phase difference layer 1 and the absorption axis of the light absorption anisotropic layer P1 formed an angle of 45°. Finally, the support of the positive C plate 1 was peeled off.
[0808] When right circularly polarized light was incident on the polarizing plate laminate from the positive C plate side, it was confirmed that substantially most of the visible light was absorbed, and when left circularly polarized light was incident, substantially most of the visible light was transmitted.
[0809] [Manufacturing of Laminated Optical Body 1 and Composite Lens 9]
[0810] The optical film 5 was bonded to the polarizing plate laminate with its yellow light reflecting layer (fifth light reflecting layer) side facing the surface of the polarizing plate laminate opposite to the light absorption anisotropic layer P1 via a pressure-sensitive adhesive sheet (NCF-D692(5)) manufactured by LINTEC Corporation.
[0811] After lamination, the TAC film used as a support of the optical film 5 was peeled off, and a laminated optical body 1 composed of a cholesteric liquid crystal, a retardation film, and a light absorption anisotropic layer was obtained.
[0812] The produced laminated optical body 1 is molded by the molding method 1 to produce a composite lens 9 .
[0813] At this time, the laminated optical body 1 is molded so that the surface on the optical film 5 side is located on the lens side.
[0814] [Production of Compound Lenses 11 to 14 Using Optical Film 6]
[0815] The optical film 6 was molded by molding methods 1 to 4 to produce composite lenses 11 to 14 .
[0816] [Forming a half mirror on a compound lens]
[0817] Aluminum was vapor-deposited on the convex side of the compound lens 1 (a convex meniscus lens LE1076-A (2 inches in diameter, 100 mm in focal length) manufactured by Thorlabs, Inc. with an optical film 2 bonded to the concave side) until the reflectivity reached 40% and used as a half-mirror. The reflection spectra of the center and the end of the compound lens 1 were measured using a spectrophotometer (V-550 manufactured by JASCO Corporation) equipped with a large integrating sphere device (ILV-471 manufactured by JASCO Corporation). The bandwidth deviation of the reflection spectra of the center and the end was 0.8%.
[0818] Similarly, aluminum vapor deposition was performed on the compound lenses 2 to 7 .
[0819] In addition, regarding the composite lenses 6 , 7 , and 8 using the optical films 3 , 4 , and 5 that were not photo-isomerized, the deviation in the bandwidth of the reflection spectrum between the center portion and the end portion was 2.8%.
[0820] [Examples 1 to 8]
[0821] The virtual reality display device "Huawei VR Glass" manufactured by Huawei Technologies Co., Ltd., which uses a reciprocating optical system, was disassembled and all the composite lenses were removed.
[0822] Instead of the removed composite lens, the composite lens 1 bonded with the optical film 2 is assembled into the main body, and further a polarizing plate stack is arranged between the composite lens 1 and the user's eye so that the light absorption anisotropic layer P1 side is located on the eye side, thereby producing the virtual reality display device of Example 1.
[0823] In the manufactured virtual reality display device, a black and white checkered pattern was displayed on an image display panel, and the ghosting visibility was visually evaluated in the following four stages.
[0824] <Evaluation of Double Vision>
[0825] A: Slightly visible, but not serious.
[0826] B; Weak ghosting is visible.
[0827] C; Slightly stronger double images can be seen.
[0828] D; strong ghosting is visible.
[0829] Furthermore, virtual reality display devices of Examples 2 to 8 were produced in the same manner using compound lenses 2 to 8, and the ghost visibility was evaluated. Table 4 shows the molding method and the type of optical film used in each Example.
[0830] [Example 9]
[0831] The virtual reality display device "Huawei VR Glass" manufactured by Huawei Technologies Co., Ltd., which uses a reciprocating optical system, was disassembled and all the composite lenses were removed.
[0832] Instead of the removed composite lens, the composite lens 9 to which the laminated optical body 1 was bonded was assembled to the main body, thereby manufacturing the virtual reality display device of Example 9.
[0833] In the manufactured virtual reality display device, a black and white checkered pattern was similarly displayed on the image display panel, and the ghost visibility was evaluated.
[0834] [Examples 11 to 14]
[0835] The composite lenses 11 to 14 using the optical film 6 were used in Examples 11 to 14.
[0836] <Measurement of phase difference>
[0837] Regarding the composite lenses 1 to 9 of Examples 1 to 9 and the composite lenses 11 to 14 of Examples 11 to 14, small pieces at the center and ends of the optical film were peeled off from the composite lenses and the phase difference (in-plane retardation) was measured using Axoscan.
[0838] The positions of the small pieces at the end were sampled at 8 locations at 45 degree intervals in the azimuth direction at 5 mm from the lens edge. The maximum value of the phase differences measured at the 8 sampled locations was taken as the phase difference at the end of the optical film.
[0839] In addition, in Examples 1 to 9 in which the optical film has a cholesteric liquid crystal layer, the evaluation wavelength is set by selecting the cholesteric liquid crystal layer with the shortest central wavelength. In addition, the difference in the evaluation wavelength between the end portion and the center portion is due to the difference in the half width on the short wavelength side caused by the different stretching ratios between the end portion and the center portion.
[0840] The composite lens, molding method, and cholesteric layer in each example are shown in Table 4 below, the evaluation results of ghost visibility are shown in Table 5 below, and the measurement results of phase difference are shown in Table 5 below.
[0841] In addition, regarding Examples 11 to 14, only the phase difference was measured, and the ghosting was not evaluated.
[0842] Table 4. Composite lens, forming method and cholesteric layer in each embodiment [Table 4]
[0843]
[0844] Table 5. Evaluation results of ghosting visual recognition [Table 5]
[0845]
[0846] As shown in Table 5, in the virtual reality display devices of Examples 1 to 4, 8, and 9, the double image was good in the entire field of view. In addition, the color change of the white part of the black and white checkered pattern was not a problem.
[0847] Regarding the ghosting in Examples 5 and 6, slightly strong ghosting was visually recognized at the end, but it was within the allowable range. In addition, in Example 6, weak ghosting was observed in the central part of the visual field. In Example 5, the color change of the white part of the black and white checkered pattern was not a problem, and in Example 6, the color change of the white part of the black and white checkered pattern was recognized. In Example 7, weak ghosting was visually recognized in the central part of the visual field, but it was not visually recognized at the end. In Example 7, the color change of the white part of the black and white checkered pattern was recognized.
[0848] Table 6. Evaluation of phase difference of each example [Table 6]
[0849]
[0850] As shown in Table 6, the optical films 1 to 5 having a cholesteric liquid crystal layer formed into the shape of a composite lens by the molding method of the present invention have a phase difference, i.e., in-plane delay, after molding that is less than 2% of the evaluation wavelength (evaluation wavelength) at the center and end (outer edge).
[0851] Furthermore, the optical film 6 using the PMMA film molded into the shape of a composite lens by the molding method of the present invention also had a phase difference, that is, in-plane retardation, of less than 11 nm at the center and end (outer edge) after molding.
[0852] As described above, according to the molding method of the present invention, even after molding, the occurrence of phase difference of the optical film, that is, the reduction of in-plane retardation can be suppressed in the center and the end portions.
[0853] [Example of the second embodiment]
[0854] [Preparation of coating solutions R-1 to R-4 for cholesterol layer]
[0855] The following compositions were stirred and dissolved in a container maintained at 70° C. to prepare cholesteric layer coating solutions R-1 to R-4, respectively. Here, R represents a coating solution using rod-shaped liquid crystals. The amount of the chiral agent contained in each cholesteric layer coating solution is shown in Table 7.
[0856]
[0857] Table 7. Amount of chiral agent in coating solution containing rod-shaped liquid crystal [Table 7]
[0858]
[0859] Mixture of rod-shaped liquid crystals
[0860] [Chemical formula 28]
[0861]
[0862] In the above mixture, the numerical values are mass %, and R is a group bonded to an oxygen atom. Furthermore, the average molar absorption coefficient of the above rod-shaped liquid crystal at a wavelength of 300 to 400 nm is 140 / mol·cm.
[0863] Chiral Reagent A
[0864] [Chemical formula 29]
[0865]
[0866] Surfactant F1
[0867] [Chemical formula 30]
[0868]
[0869] Surfactant F2
[0870] [Chemical formula 31]
[0871]
[0872] Polymerization initiator LC-1-1
[0873] [Chemical formula 32]
[0874]
[0875] Chiral reagent A is a chiral reagent whose helical twisting power (HTP: Helical Twisting Power) decreases due to light.
[0876] (Coating liquids for cholesteric layer D-1 to D-4)
[0877] The following compositions were stirred and dissolved in a container maintained at 50° C. to prepare cholesteric layer coating solutions D-1 to D-4. Here, D represents a coating solution using a discotic liquid crystal. The amount of the chiral agent contained in each cholesteric layer coating solution is shown in Table 8.
[0878]
[0879] Table 8. Amount of chiral agent in coating solution containing discotic liquid crystal [Table 8]
[0880]
[0881] Discotic liquid crystal (A)
[0882] [Chemical formula 33]
[0883]
[0884] Discotic liquid crystal (B)
[0885] [Chemical formula 34]
[0886]
[0887] Polymerizable monomer E1
[0888] [Chemical formula 35]
[0889]
[0890] Surfactant F4
[0891] [Chemical formula 36]
[0892]
[0893] [Production of Laminated Body 1]
[0894] As a pseudo support, a PET (polyethylene terephthalate) film (A4100 manufactured by TOYOBO CO., LTD.) having a thickness of 50 μm was prepared. The PET film had an easy-adhesion layer on one side.
[0895] The surface without the easy-adhesive layer of the PET film was subjected to a rubbing treatment, and the above-prepared cholesteric liquid crystal coating liquid R-1 was applied using a wire bar coater, and then dried at 110° C. for 1 minute to vaporize the solvent, and then heated and aged at 100° C. for 1 minute, thereby obtaining a cholesteric liquid crystal film in which a cholesteric liquid crystal phase with a uniform orientation state was applied to a support. The cholesteric liquid crystal film was placed on a mounting table with a rotating mechanism. Then, as a UV (ultraviolet) light source, a microwave emitting ultraviolet irradiation device (Light Hammer 10, 240 W / cm, manufactured by Fusion UV Systems Inc.) equipped with a D-Bulb having a strong luminescence spectrum at 350 to 400 nm was used, and a wire grid polarization filter (ProFlux PPL02 (high transmittance type), manufactured by MOXTEK, Inc.) was set at a position 10 cm away from the irradiation surface, and polarized UV light was irradiated through an exposure mask in a nitrogen atmosphere while rotating the cholesteric liquid crystal film heated to 80°C. The concept diagram of the exposure mask used at this time is shown in Fig.11 .
[0896] The following uses Fig.11 The exposure mask shown in FIG. 1 and the exposure method of the exposure mask are described. The exposure mask is designed to transmit polarized UV light from the center of the mask to the triangular region A symmetrical about the y-axis, and the transmittance is continuously 0% to 100% from the center to the end along the y-axis. Furthermore, the length from the center to the side orthogonal to the x-axis of the triangular shape is 1 inch.
[0897] The cholesteric liquid crystal film is rotated while passing through Fig.11 The cholesteric liquid crystal film is irradiated with an exposure mask Fig.11 Polarized UV parallel to the y-axis, with irradiance and irradiation amount set to 0 mW / cm in the center 2 Illuminance and 0mJ / cm 2 The irradiation amount was set to 200mW / cm at the end. 2 Illuminance and 300mJ / cm 2 As a result, a slow axis is formed that is concentric with the rotation center. The conceptual diagram of the slow axis formed is shown in Fig.12 After that, the samples were further irradiated at 100°C with an illumination of 80 mW / cm2 in a nitrogen atmosphere (less than 100 ppm). 2 、Irradiation 500mJ / cm 2 The red light reflecting layer composed of a cholesteric liquid crystal layer was cured by light from a metal halide lamp. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the film thickness of the cured red light reflecting layer was 4.5 μm.
[0898] Next, the discharge rate was 150W·min / m 2 After the red light reflecting layer surface was subjected to corona treatment, the cholesteric liquid crystal layer coating liquid D-2 was applied to the corona treated surface using a wire bar coater. Next, the coating film was dried at 100°C for 2 minutes, and after the solvent was vaporized, it was heated and aged at 115°C for 5 minutes, thereby obtaining a cholesteric liquid crystal film in which a cholesteric liquid crystal phase with a uniform orientation state was coated on a support. Thereafter, polarized UV irradiation and metal halide UV irradiation were performed through a mask in the same manner as for the red reflecting layer, thereby forming a yellow light reflecting layer on the red light reflecting layer. At this time, the coating thickness was adjusted so that the film thickness of the yellow light reflecting layer after curing became 3.3 μm.
[0899] Next, the coating liquid R-3 for the cholesteric liquid crystal layer was applied on the yellow light reflecting layer using a wire bar coater, and then dried at 110°C for 1 minute to vaporize the solvent, and then heated and aged at 100°C for 1 minute, thereby obtaining a cholesteric liquid crystal film coated on a support body with a cholesteric liquid crystal phase having a uniform orientation state. Thereafter, polarized UV irradiation and metal halide UV irradiation were performed through a mask in the same manner as for the red reflecting layer, thereby forming a green light reflecting layer on the yellow light reflecting layer. At this time, the coating thickness was adjusted so that the film thickness of the green light reflecting layer after curing was 2.7 μm.
[0900] Next, the discharge rate was 150W·min / m 2 After the green light reflecting layer surface was subjected to corona treatment, a coating liquid D-4 for a cholesteric liquid crystal layer was applied to the corona treated surface using a wire bar coater. Next, the coated film was dried at 100°C for 2 minutes, and after the solvent was vaporized, it was heated and aged at 115°C for 5 minutes, thereby obtaining a cholesteric liquid crystal film in which a cholesteric liquid crystal phase with a uniform orientation state was coated on a support. Afterwards, polarized UV irradiation and metal halide UV irradiation were performed through a mask in the same manner as the red reflecting layer, thereby forming a blue light reflecting layer on the green light reflecting layer. At this time, the coating thickness was adjusted so that the film thickness of the cured blue light reflecting layer became 2.5 μm. Thus, a laminate 1 having a multilayer cholesteric liquid crystal layer was prepared. The coating liquid and film thickness used for the cholesteric liquid crystal layer are shown in Table 9-1.
[0901] [Table 9-1]
[0902]
[0903] [Production of Laminated Body 2]
[0904] Laminated body 2 was produced by the same production method as laminated body 1 except that the number of layers was increased to 8 and the coating liquid and film thickness for the cholesteric liquid crystal layer were changed as shown in the following Table 9-2.
[0905] [Table 9-2]
[0906]
[0907] [Production of laminate 3]
[0908] In the manufacturing process of the laminated body 1 , the laminated body 3 was manufactured without performing polarized UV irradiation using an exposure mask.
[0909] [Production of Laminated Body 4]
[0910] In the manufacturing process of the laminated body 2 , the laminated body 4 was manufactured without performing polarized UV irradiation using an exposure mask.
[0911] [Production of optical laminate]
[0912] The laminate 1 was bonded to a PMMA film via a pressure-sensitive adhesive sheet "NCF-D692(5)" manufactured by LINTEC Corporation, and the PET support was peeled off to obtain an optical laminate 1. Optical laminates 2 to 4 were obtained in the same manner as for the optical laminate 1 except that the laminate 1 was used as the laminate 2 to 4.
[0913] [Evaluation of phase difference and slow axis]
[0914] The slow axis and phase difference of the optical stack 1 were measured using the ellipsometer M-2000UI manufactured by JA Woollam. The optical stack 1 has a slow axis that is substantially concentric with the rotation center of the mask during exposure. In addition, the phase difference of the optical stack 1 at the rotation center during mask exposure was measured, and the result was 0 nm. The phase difference of the optical stack 1 at a position separated by 0.2 inches from the rotation center of the mask during exposure in the radial direction of the above-mentioned concentric circle is 2 nm. The phase difference of the optical stack 1 at a position separated by 0.6 inches from the rotation center of the mask during exposure in the radial direction of the above-mentioned concentric circle is 12 nm. The phase difference of the optical stack 1 at a position separated by 0.8 inches from the rotation center of the mask during exposure in the radial direction of the above-mentioned concentric circle is 23 nm.
[0915] The results of similar evaluation of optical laminates 2 to 4 are shown in Table 10. Optical laminates 1 and 2 having a cholesteric liquid crystal layer irradiated with polarized UV through a mask by the above method have different phase differences in the plane and have substantially concentric slow axes. On the other hand, optical laminates 3 and 4 having a cholesteric liquid crystal layer not irradiated with polarized UV do not have a phase difference.
[0916] [Table 10]
[0917]
[0918] 〔Forming method〕
[0919] The optical laminate 1 was formed on the concave surface of a convex meniscus lens LE1076-A (2-inch diameter, 100 mm focal length, 65 mm radius of curvature on the concave side) manufactured by Thorlabs, Inc. by vacuum forming via an adhesive sheet. Finally, the portion protruding from the lens of the optical laminate 1 was cut out, thereby obtaining an optical component 1 including a cholesteric liquid crystal layer formed into a curved surface.
[0920] Optical component 2 was obtained by the same production method as that of optical component 1 except that optical layered body 2 was used instead of optical layered body 1.
[0921] Optical component 3 was obtained by the same production method as that of optical component 1 except that optical layered body 3 was used instead of optical layered body 1.
[0922] Optical component 4 was obtained by the same production method as that of optical component 1 except that optical layered body 4 was used instead of optical layered body 1.
[0923] [Production of polarizing plate laminate]
[0924] [Production of positive C plate 1]
[0925] The film thickness was adjusted with reference to the method described in paragraphs 0132 to 0134 of Japanese Patent Application Laid-Open No. 2016-053709 to produce a positive C plate 1. In the positive C plate 1, Re=0.2 nm, Rth=-310 nm.
[0926] [Preparation of phase difference layer 1]
[0927] The anomalous dispersion retardation layer 1 was prepared by referring to the method described in paragraphs 0151 to 0163 of Japanese Patent Application Laid-Open No. 2020-084070. In the retardation layer 1, Re=146 nm, and Rth=73 nm.
[0928] 〔Fabrication of Linear Polarizer〕
[0929] [Production of Cellulose Acylate Film 1]
[0930] (Preparation of Core Layer Cellulose Acylate Dopant)
[0931] The following composition was placed in a mixing tank and stirred to dissolve the components, thereby preparing a cellulose acetate solution to be used as a doping agent for the cellulose acylate in the core layer.
[0932]
[0933] Compound F
[0934] [Chemical formula 37]
[0935]
[0936] (Preparation of outer layer cellulose acylate dopant)
[0937] To 90 parts by mass of the core layer cellulose acylate doping agent was added 10 parts by mass of the following matting agent solution to prepare a cellulose acetate solution as an outer layer cellulose acylate doping agent.
[0938]
[0939] (Production of Cellulose Acylate Film 1)
[0940] After filtering the core layer cellulose acylate dopant and the outer layer cellulose acylate dopant using filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm, a total of three layers of the core layer cellulose acylate dopant and the outer layer cellulose acylate dopant on both sides thereof are simultaneously cast from a casting port onto a drum at 20° C. (belt casting machine).
[0941] Next, the film was peeled at a solvent content of about 20% by mass, and both ends of the film in the width direction were clamped by a tenter clip, stretched in the transverse direction at a stretching ratio of 1.1 times, and dried.
[0942] Thereafter, the film was carried between rolls of a heat treatment device and further dried to produce an optical film having a thickness of 40 μm, which was referred to as a cellulose acylate film 1. The in-plane retardation of the obtained cellulose acylate film 1 was 0 nm.
[0943] <Formation of Photo-Alignment Layer PA1>
[0944] The coating liquid S-PA-1 for forming an alignment layer described later was continuously coated on the cellulose acylate film 1 using a wire bar. The support body with the coating film formed was dried with warm air at 140° C. for 120 seconds, and then the coating film was irradiated with polarized ultraviolet rays (10 mJ / cm 2 , using an ultra-high pressure mercury lamp), thereby forming a photo-alignment layer PA1 with a film thickness of 0.3 μm.
[0945]
[0946]
[0947] Polymer M-PA-1
[0948] [Chemical formula 38]
[0949]
[0950] Acid Generator PAG-1
[0951] [Chemical formula 39]
[0952]
[0953] Acid Generator CPI-110F
[0954] [Chemical formula 40]
[0955]
[0956] <Formation of light absorption anisotropic layer P1>
[0957] The following coating liquid SP-1 for forming an anisotropic light absorbing layer was continuously coated on the obtained orientation layer PA1 using a wire bar. Next, the coating layer P1 was heated at 140°C for 30 seconds and cooled to room temperature (23°C). Next, it was heated at 90°C for 60 seconds and cooled to room temperature again. Thereafter, an LED lamp (central wavelength 365nm) was used at an illumination of 200mW / cm 2 The light absorption anisotropic layer P1 was formed on the alignment layer PA1 under the irradiation condition of 2 seconds. The film thickness was 1.6 μm.
[0958]
[0959]
[0960] Dichroic substance D-1
[0961] [Chemical formula 41]
[0962]
[0963] Dichroic substance D-2
[0964] [Chemical formula 42]
[0965]
[0966] Dichroic substance D-3
[0967] [Chemical formula 43]
[0968]
[0969] High molecular weight liquid crystal compound MP-1 [Chemical formula 44]
[0970]
[0971] Low molecular weight liquid crystal compound M-1
[0972] [Chemical formula 45]
[0973]
[0974] Surfactant F-1
[0975] [Chemical formula 46]
[0976]
[0977] The obtained phase difference layer 1 was attached to the side of the obtained positive C plate 1 opposite to the support. Next, the light absorption anisotropic layer P1 was transferred. At this time, the transfer was performed in such a way that the layer on the side of the light absorption anisotropic layer P1 opposite to the dummy support was located on the positive C plate 1 side. After the transfer, the dummy support of the light absorption anisotropic layer P1 was peeled off and removed. The transfer of the light absorption anisotropic layer P1 was performed in the following order.
[0978] (1) Using a wire bar coater, UV adhesive Chemiseal U2084B (manufactured by CHEMITECH INC., with a refractive index of n1.60 after curing) was applied to the support side of the positive C plate 1 to a thickness of 2 μm. The light absorption anisotropic layer P1 was laminated thereon using a laminator so that the side opposite to the dummy support contacted the UV adhesive.
[0979] (2) After nitrogen flushing in a flushing box until the oxygen concentration becomes 100 ppm or less, the light absorption anisotropic layer P1 is cured by irradiating with ultraviolet light from a high pressure mercury lamp from the dummy support side. The illuminance is 25 mW / cm 2 , the irradiation dose is 1000mJ / cm 2 .
[0980] (3) Finally, the dummy support of the light absorption anisotropic layer P1 is peeled off.
[0981] The layers were stacked in such a way that the slow axis of the phase difference layer 1 and the absorption axis of the light absorption anisotropic layer P1 formed a 45° angle. Finally, the support of the positive C plate 1 was peeled off. In this way, a polarizing plate laminate was obtained. When right circularly polarized light was incident on the polarizing plate laminate from the positive C plate side, it was confirmed that substantially most of the visible light was absorbed, and when left circularly polarized light was incident, substantially most of the visible light was transmitted.
[0982] [Forming a half mirror on an optical component]
[0983] Aluminum was vapor-deposited on the convex surface of the optical component 1 until the reflectance reached 40%, and the half mirror was used. Similarly, aluminum was vapor-deposited on the optical components 2 to 4.
[0984] [Example 2-1]
[0985] A virtual reality display device "Huawei VR Glass" manufactured by Huawei Technologies Co., Ltd., which uses a reciprocating optical system, was disassembled and all the composite lenses were removed. Instead, the optical component 1 was assembled to the main body, and the optical component 1 and the eye were further arranged so that the light absorption anisotropic layer P1 side of the polarizing plate stack was located on the eye side, thereby producing a virtual reality display device of Example 2-1.
[0986] Furthermore, virtual reality display devices were produced in the same procedure as in Example 2-2 and Comparative Examples 2-1 and 2-2, except that the optical article 1 was replaced with the optical articles 2 to 4, respectively.
[0987] <Evaluation of light leakage>
[0988] In the virtual reality display devices of Examples 2-1 and 2-2 and Comparative Examples 2-1 and 2-2, a black and white checkered pattern was displayed on an image display device, and the degree of light leakage was visually evaluated according to the following three stages. In addition, if there is light leakage, double images are visually recognized, and the contrast of the corresponding part is reduced.
[0989] A: Almost no double image can be seen
[0990] B: Slight double vision, but no problem
[0991] C; Ghosting is clearly visible
[0992] The results are shown in Table 11.
[0993] <Evaluation of display uniformity>
[0994] In the virtual reality display devices of Examples 2-1 and 2-2 and Comparative Examples 2-1 and 2-2 thus produced, a black and white checkered pattern was displayed on an image display device, and display uniformity was visually evaluated in the following three stages.
[0995] A; Overall uniformity
[0996] B; Part of the image is distorted unevenly
[0997] C; Most images are distorted
[0998] The results are shown in Table 11.
[0999] Table 11. Evaluation results of the virtual reality display device of the embodiment [Table 11]
[1000] Optical items Light Leakage Display uniformity Example 2-1 Optical items 1 A A Example 2-2 Optical items 2 A A Comparative Example 2-1 Optical items 3 B B Comparative Example 2-2 Optical items 4 B B
[1001] The above results show that the cholesteric liquid crystal layer after concave molding eliminates the slow axes arranged concentrically before concave molding by the concave molding, and as a result, the retardation becomes 10 nm or less, so the evaluation of light leakage and display uniformity becomes good.
[1002] According to the above results, the effect of the present invention is obvious.
[1003] Explanation of symbols
[1004] 31-the first light reflecting layer, 32-the second light reflecting layer, 33-the third light reflecting layer, 34-the fourth light reflecting layer, 100-laminated optical body, 101-anti-reflection layer, 102-positive C plate, 103-optical film, 104-positive C plate, 105-phase difference layer, 106-linear polarizer, 120-support body, 124-oriented film, 126-cholesteric liquid crystal layer, 132-liquid crystal compound, 200-lens, 300-half-mirror, 400-circular polarizer (reflective circular polarizer), 500-image display panel, 1000-light, 2000-light forming double images.
Claims
1. A forming method, which is a forming method of an optical film comprising the following steps: A heating process for heating the optical film; A forming step of pressing the optical film onto a mold and deforming the optical film along the shape of the mold; and a cutting process, cutting the optical film, The heating step is a step of heating the optical film by irradiating the optical film with infrared rays, and the irradiation amount of the infrared rays has a distribution within the surface of the optical film.
2. The forming method according to claim 1, wherein: The mold is a concave non-developable surface with a positive Gaussian curvature. When the position of the optical film in the plane is projected onto the mold from the normal direction of the main surface of the optical film, The amount of infrared light irradiating the optical film at the apex of the concave surface is greater than the amount of infrared light irradiating the optical film at the end of the concave surface.
3. A forming method, which is a forming method of an optical film comprising the following steps: A heating process for heating the optical film; A forming step of pressing the optical film onto a mold and deforming the optical film along the shape of the mold; and a cutting process, cutting the optical film, The surface of the mold in contact with the optical film is a concave surface of a non-developable surface with a positive Gaussian curvature, and the outer peripheral shape is an ellipse, The cut shape in the cutting step is an ellipse, and the major axis of the ellipse outer peripheral shape of the optical film cut out by the cutting is greater than 50% and less than 95% of the major axis of the ellipse outer peripheral shape of the mold.
4. A forming method, which is a forming method of an optical film comprising the following steps: A heating process for heating the optical film; A forming step of pressing the optical film onto a mold and deforming the optical film along the shape of the mold; and a cutting process, cutting the optical film, In the heating step, the region of the optical film in contact with the mold is heated to a temperature higher than the glass transition temperature Tg of the optical film. In the molding step, immediately after the optical film comes into contact with the mold, the pressing of the optical film against the mold is controlled so that the temperature of the region of the optical film in contact with the mold is lower than the glass transition temperature Tg.
5. A forming method, which is a forming method of an optical film comprising the following steps: A heating process is used to heat the mold; a forming step of pressing the heated mold onto the optical film and deforming the optical film along the shape of the mold; and a cutting process, cutting the optical film, The mold is a convex surface of a non-developable surface with positive Gaussian curvature, In the molding step, the apex of the convex surface of the mold is pressed against the center of the optical film.
6. The forming method according to claim 5, wherein: The cutting shape of the optical film in the cutting step is an ellipse, In the molding step, the optical film is pressed against the mold in a state where the position on the line of the oval that forms the cut shape is restricted.
7. A cholesteric liquid crystal layer, wherein: The cholesteric liquid crystal layer has a phase difference region where the phase difference increases from the center to the outside. In the phase difference region, the direction of the slow axis at one point in the phase difference region is orthogonal to the direction from the center toward the one point. 8 . An optical laminate comprising a plurality of cholesteric liquid crystal layers according to claim 7 .
9. The optical layered body according to claim 8, wherein: The cholesteric liquid crystal layer formed using a rod-like liquid crystal compound and the cholesteric liquid crystal layer formed using a discotic liquid crystal compound are alternately stacked.
10. A method for manufacturing a curved optical functional layer, comprising: a cholesteric liquid crystal layer manufacturing step, manufacturing the cholesteric liquid crystal layer according to claim 7; and The forming step is to perform curved surface forming in such a manner as to eliminate the phase difference of the cholesteric liquid crystal layer.
11. The method for producing a curved optical functional layer according to claim 10, wherein: In the forming step, the cholesteric liquid crystal layer is disposed on a forming mold having a concave forming surface so that the bottom of the concave forming surface of the forming mold coincides with the center of the cholesteric liquid crystal layer, and the cholesteric liquid crystal layer is deformed along the concave forming surface.
12. An optical film having a non-developable surface with positive Gaussian curvature, wherein: The optical film is a cholesteric liquid crystal layer, When the evaluation wavelength of the in-plane retardation is set to a wavelength obtained by subtracting 20 nm from the half-value wavelength on the shorter side than the selective reflection center wavelength of the cholesteric liquid crystal layer, The in-plane retardation A of the evaluation wavelength at the center of the cholesteric liquid crystal layer is smaller than a value of 2% of the evaluation wavelength, and The in-plane retardation B at the evaluation wavelength at the outer edge portion of the cholesteric liquid crystal layer is smaller than 2% of the evaluation wavelength.
13. An optical film having a non-developable surface with positive Gaussian curvature, wherein: The optical film does not have selective reflection properties. The in-plane retardation A of the wavelength 550 nm at the center of the optical film is less than 11 nm, and The in-plane retardation B at a wavelength of 550 nm at an outer edge portion of the optical film is less than 11 nm.
14. The optical film according to claim 12 or 13, wherein: The outer periphery of the optical film is an ellipse.