Oxide sintered body and thin film transistor including same
By adjusting the proportion of In, Zn, and Ga elements and adding gallium oxide to form an optimized oxide sintered body, the problem of insufficient electron mobility in the low temperature process of existing oxide semiconductors is solved, and high electron mobility and stability are achieved. Suitable for large-area display and X-ray image drivers.
Patent Information
- Application Number
- CN202380032472.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-08
- Filing Date
- 2023-04-05
- Publication Date
- 2024-11-22
AI Technical Summary
The existing oxide semiconductor materials have limitations in terms of high electron mobility and durability, and it is difficult to meet the needs of large-area displays and X-ray image driving, especially oxide semiconductors with high electron mobility under low-temperature process conditions.
By adjusting the ratio of In, Zn and Ga elements in the oxide sintered body, adding an appropriate amount of gallium oxide (Ga2O3) to form an oxide sintered body of InxZnyGazO, optimizing its electron mobility and carrier concentration to ensure that it is less than 400℃ High electron mobility and stability are achieved in low-temperature processes.
It realizes an oxide semiconductor with electron mobility of more than 30cm2/Vs under low temperature process conditions. It is suitable for high-definition and high-speed driving displays and X-ray images, and improves the electron mobility and carrier concentration of oxide sintered bodies. stability.
Smart Images

Figure CN119013790A_ABST
Abstract
Description
Technical Field
[0001] This application claims the priority benefit based on Korean Patent Application No. 2022-0043793 filed on April 8, 2022, and all the contents described in the Korean patent application document are incorporated into the specification of this application as a part.
[0002] The present invention relates to an oxide sintered body and a thin film transistor comprising the same. Background Art
[0003] Oxides of post-transition metals such as In, Ga, Zn, Cd, and Zn, especially oxides of two, three, four or more components, exhibit a band gap of 2 to 3 eV or more close to that of metals and a band gap of 10 19 ~10 20 / cm 3 The above-mentioned high carrier concentration properties, combined with its transparent and electrical conductivity characteristics, have led to rapid development in the application fields requiring transparent electrodes, such as solar cells and displays.
[0004] Since the 1960s, efforts have been made to 2 O 3 ) materials by adding dopants such as Sn, Zn, Ge, Mo, Ti, Zr, Hf, Nb, Ta, W, Te or F or by adding dopants such as SnO 2 ) materials to improve conductivity, durability, chemical resistance and processability by adding dopants such as F, Sb, Nb or Ta. Finally, based on metal elements, InSnO doped with about 10 atomic % (at %) Sn and InZnO doped with 10 atomic % Zn have been used as transparent electrodes for LCD displays since 1992 and 1995, respectively, and are still in use today.
[0005] Zinc oxide (ZnO) can be used to manufacture a transparent electrode having conductivity characteristics second only to InSnO or InZnO using dopants such as Ga, Al, B, In, Y, Sc, V, Si, Ge, Ti, Zr, Hf or F. However, due to relatively low chemical resistance and durability, it is not suitable as an electrode for devices exposed to the external environment such as solar cells. On the contrary, FSnO doped with F is widely used as an external transparent electrode of solar cells due to its high durability and low manufacturing cost.
[0006] In order to use the oxide material as a semiconductor instead of the transparent electrode, the carrier concentration needs to be adjusted to 10 18 ~1019 / cm 3 Below, it is also necessary to minimize defects between grains of materials having polymorphism.
[0007] Therefore, it is known that CdO, ZnO, In 2 O 3 SnO 2 Two-component or three-component oxide materials such as InSnO, InZnO, etc. have a method of controlling oxygen vacancy defects in the film by reducing the carrier concentration to ensure semiconductor properties, however, they exhibit the property of easily crystallizing according to the thermal history of the subsequent process, and it is difficult to adjust the defect density between grains as grains of tens to hundreds of nanometers are formed. Therefore, the characteristic distribution between multiple elements is large and the process is not easy to reproduce. Therefore, there are limitations in application to large-area electronic components such as displays.
[0008] In 2004, Professor Hosono of Tokyo Institute of Technology published in Nature (Volume 432, Page 488) that the crystallization temperature of the four-component oxide material of InGaZnO reached 500-600°C. Therefore, it can remain amorphous at a temperature below 400°C and become a 7-10 cm 2 / Vs, which is more than 10 times higher than the electron mobility of hydrogenated amorphous silicon (a-Si:H), which was commonly used as a semiconductor material for display backplane thin-film transistors at the time.
[0009] In particular, the a-Si:H TFT is very fragile to current driving and therefore cannot be applied to displays such as organic light-emitting elements or inorganic light-emitting elements having pixels that require continuous application of several microamperes or tens of microamperes of current. In contrast, the IGZO TFT exhibits stable characteristics under current driving and therefore is currently used in driving elements of organic light-emitting displays, etc.
[0010] In particular, displays or X-ray images with thousands or millions of pixels must be driven by an active matrix having scan lines and data lines in a row and column structure and in pulse form, so that independent signals are provided to individual pixels or read from individual pixels in a manner that does not interfere with each other, and in order to avoid overlap between scan lines, the pulse width of the scan signal is limited by the frame frequency and resolution, and has a characteristic that is inversely proportional to the frame frequency and resolution. Therefore, thin film transistors with high electron mobility characteristics must be used to smoothly transfer the data voltage to the pixel electrode during a scan signal with a smaller pulse width, thereby driving displays and X-ray images with high resolution and high-speed frame frequency characteristics. For example, in order to drive a 4K2K resolution display in a dual scan mode at a frame frequency of 120Hz, a 1cm 2 In order to drive the above display in a single scan mode at a frame frequency of 240 Hz, a thin film transistor with an electron mobility of more than 5 cm is required. 2 / Vs or above electron mobility (refer to Figure 1 ).
[0011] However, if Figure 1 As shown, in order to drive in a single scan mode with a frame rate of 240Hz at 8K4K resolution, a 30cm 2 / Vs or more, and in order to realize the active matrix backplane of high-definition and high-speed driving environment required for real-time display or high-definition low-dose X-ray (X-ray) detector, it is necessary to replace the electron mobility limited to 10cm 2 / Vs and has an atomic % composition ratio of 1:1:1 for InGaZnO based on the metal element, and an electron mobility of 30cm 2 / Vs and above new oxide semiconductors.
[0012] Prior Art Literature
[0013] Non-patent document 1: K.Nomura et al., "Room-temperature fabrication oftransparent flexible thin-film transistors using amorphous oxidesemiconductors", 2004, Nature, 432, p.488~492
[0014] Non-patent document 2: Y. Matsueda, Digest of Int. Transistor Conf. 28-29 January 2010, Hyogo, Japan, p. 314 Summary of the invention
[0015] Technical issues
[0016] The object of the present invention is to provide an oxide sintered body which can be used to manufacture transistor arrays, driver integrated circuits and transparent electronic components for driving backplanes for realizing large-area flat-panel or curved displays and X-ray images, and can be used in a monolithic three-dimensional semiconductor integration process using a continuous process on silicon (Si) semiconductor chips for storage semiconductors or logic elements, so as to manufacture high-performance, highly integrated and low-power semiconductor chips.
[0017] The present invention aims to provide a novel oxide sintered body having a high mobility which causes an increase in the energy of mobile charges by changing the amount of indium oxide (Indium Oxide, In-O bond enthalpy; 320.1 kJ / mol) in the oxide sintered body. 20 / cm 3 When the carrier concentration is adjusted to 10 18 / cm 3 Up to 10 19 / cm 3 The following is an optimal combination of indium-zinc oxide (IZO). In addition, gallium oxide (Gallium Oxide) with an energy level similar to that of indium oxide (InO) is added to the IZO to overcome the limitation of electron mobility.
[0018] Another object of the present invention is to provide a thin film transistor including the oxide sintered body.
[0019] Technical Solution
[0020] One embodiment of the present invention provides an oxide sintered body, which contains In element, Zn element, Ga element and oxygen, wherein the atomic ratio of In element to Zn element is 1-2:1, the atomic ratio of In element to Ga element is 3-6:1, and the atomic ratio of Zn element to Ga element is 3-6:1.
[0021] The oxide sintered body may be represented by Chemical Formula 1.
[0022] Chemical formula 1:
[0023] In x Zn y Ga z O (3x / 2+y+3z / 2)
[0024] In the chemical formula 1, x:y=1-2:1, x:z=3-6:1, y:z=3-6:1.
[0025] In the oxide sintered body, the atomic ratio of the In element to the Zn element may be 1 to 1.5:1, the atomic ratio of the In element to the Ga element may be 4 to 5:1, and the atomic ratio of the Zn element to the Ga element may be 4 to 5:1.
[0026] The relative density of the oxide sintered body may be 98.0% to 99.9%.
[0027] Another embodiment of the present invention provides a thin film transistor, which includes a substrate, a gate, an insulating film, a channel layer, a source electrode, and a drain electrode, wherein the channel layer includes the oxide sintered body.
[0028] The channel layer includes an oxide thin film formed by sputtering a target including the oxide sintered body.
[0029] The electron mobility of the channel layer can be 30 cm 2 / Vs or above.
[0030] The carrier concentration of the channel layer may be less than 1.0×10 19 / cm 3 .
[0031] Beneficial Effects
[0032] The oxide sintered body of the present invention is prepared by adding a predetermined amount of gallium oxide (Gallium Oxide; Ga) having an energy level similar to that of indium oxide (Indium Oxide; InO) to an existing In-Zn-based oxide. 2 O 3 ), it is possible to realize an oxide semiconductor that has excellent electron mobility even in a low-temperature process below 400°C and can operate within a relatively low voltage range. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The graph shows the electron mobility of a thin film transistor required according to different scanning frequencies and display resolutions.
[0034] Figure 2This is an image showing the structure of an oxide thin film transistor (TFT) in which an oxide sintered body according to an embodiment is formed as a channel layer (active layer).
[0035] Figure 3 is a graph showing the voltage-current characteristics of the thin film transistor according to Example 1 of the present invention.
[0036] Figure 4 The positive gate bias temperature stress (PBTS) reliability test results of the thin film transistor of Example 1 of the present invention are shown.
[0037] Figure 5 The negative gate bias temperature stress (NBTS) reliability test results of the thin film transistor of Example 1 of the present invention are shown.
[0038] Figure 6 is a graph showing the voltage-current characteristics of the thin film transistor of Comparative Example 1 of the present invention.
[0039] Figure 7 The positive gate bias temperature stress (PBTS) reliability test results of the thin film transistor of Comparative Example 1 of the present invention are shown.
[0040] Figure 8 The negative gate bias temperature stress (NBTS) reliability test results of the thin film transistor of Comparative Example 1 of the present invention are shown. DETAILED DESCRIPTION
[0041] In the drawings, the thickness is exaggerated to clearly indicate multiple layers and regions, and when a layer, film, region, plate or other portion is "above" another portion, it includes not only the case where it is "directly above" another portion, but also the case where there is another portion in between. Conversely, when a portion is "directly above" another portion, it means that there is no other portion between them.
[0042] The term "nano" described in the present invention means nanoscale, including a size of 1 μm or less.
[0043] Hereinafter, an oxide sintered body according to an embodiment will be described.
[0044] The present invention relates to an oxide sintered body which can be used for a high-definition large-area display due to high electron mobility and low driving voltage.
[0045] An oxide sintered body in one implementation example is an oxide sintered body containing In element, Zn element, Ga element and oxygen, wherein the atomic ratio of In element to Zn element can be 1 to 2:1, the atomic ratio of In element to Ga element can be 3 to 6:1, and the atomic ratio of Zn element to Ga element can be 3 to 6:1.
[0046] InGaZnO oxide thin film transistors, one of the existing transparent oxide semiconductors, can achieve stable device characteristics. On the contrary, as the size of displays increases, it is difficult to drive displays with the low mobility of InGaZnO. Therefore, it is necessary to develop a 20cm 2 / Vs or higher oxide semiconductors with high mobility can be applied to devices that can be mounted on large displays.
[0047] The present invention aims to solve the above-mentioned problem. x Zn y O (3x / 2+y) A specified content of gallium oxide (GaO) is added to an In-Zn-based oxide (x:y=(1~1.5):1 atomic %) to form an oxide sintered body with high electron mobility having an optimized combination ratio of indium (In) element, zinc (Zn) element, gallium (Ga) element and oxygen (O), thereby providing an oxide sintered body having high electron mobility for an active matrix backplane for realizing a high-definition, high-speed driving environment in large displays, etc., and a thin film transistor including the same.
[0048] Specifically, the oxide sintered body may be represented by Chemical Formula 1.
[0049] Chemical formula 1:
[0050] In x Zn y Ga z O (3x / 2+y+3z / 2)
[0051] In the chemical formula 1, x:y=1-2:1, x:z=3-6:1, y:z=3-6:1.
[0052] That is, the oxide sintered body of one embodiment is an In-Zn-Ga type oxide represented by the chemical formula 1. At this time, the atomic ratios of the indium (In) element, the zinc (Zn) element, and the gallium (Ga) element can be optimized respectively, the atomic ratio of the In element to the Zn element is 1 to 2:1, the atomic ratio of the In element to the Ga element is 3 to 6:1, and the atomic ratio of the Zn element to the Ga element is 3 to 6:1.
[0053] Preferably, in the oxide sintered body represented by the chemical formula 1, more specifically, the atomic ratio of the In element to the Zn element can be 1 to 1.5:1, the atomic ratio of the In element to the Ga element can be 4 to 5:1, and the atomic ratio of the Zn element to the Ga element can be 4 to 5:1, thereby, the element characteristics of the thin film transistor containing the oxide sintered body can show high electron mobility and excellent carrier concentration. At this time, in the oxide sintered body, when the atomic ratio of the Ga element to the Zn element is less than the above range, the effect of the added Ga element is small, and the improvement of the element characteristics is not obvious, so it may be difficult to show a high electron mobility that can be applied to large displays. When it is greater than the above range, the relative density and resistivity characteristics of the oxide sintered body are reduced, thereby reducing the electron mobility of the thin film transistor.
[0054] The relative density of the oxide sintered body of the present invention having the above composition may be 98.0% to 99.9%. When the relative density of the oxide sintered body is less than 98.0%, when a target including the oxide sintered body is used as a sputtering target for forming a transistor film, nodules may be generated, thereby increasing the probability of abnormal discharge.
[0055] At this time, the "relative density" of the oxide sintered body can be defined by Mathematical Formula 1.
[0056] Mathematical formula 1:
[0057] Relative density of oxide sintered body = (measured density of oxide sintered body / theoretical density of oxide sintered body) × 100
[0058] In the above-mentioned Mathematical Formula 1, the measured density of the oxide sintered body can be represented by a value obtained by measuring the oxide sintered body in water at 1 atm and 4° C.
[0059] The oxide sintered body of the present invention can be manufactured by methods commonly used in the art, for example, it can be manufactured by the following method, which includes the following steps: a raw material powder preparation step; a step of mixing the raw material powder to prepare a spherical powder; a molded body preparation step and a sintered body preparation step.
[0060] An embodiment of the method for preparing the oxide sintered body may include the following steps: a step of grinding and drying indium oxide powder, zinc oxide powder and gallium oxide powder to prepare a slurry after mixing them; a step of pressurizing the pulverized product to form a mold; and a step of sintering the molded body.
[0061] The preparation method is described below according to each step.
[0062] First, raw material powders of indium oxide powder, zinc oxide powder and gallium oxide powder are prepared, and each raw material powder is weighed to obtain a target combination, such as an oxide sintered body represented by the chemical formula 1, and then put into a mixer for pulverization and mixing to prepare slurry.
[0063] In the present invention, the indium oxide powder, zinc oxide powder and gallium oxide powder can be any conventional component in the art without limitation. For example, the indium oxide can be In 2 O 3 The zinc oxide may be ZnO, the gallium oxide may be GaO, etc., and each of the raw materials may be a powder having an average particle size of 1 to 10 μm, for example.
[0064] When the above-mentioned various raw material powders are mixed, conventional additives in the art, such as a binder, a dispersant, a defoaming agent, etc., may be further added as needed.
[0065] The purpose of adding a dispersant is to keep the crushed raw material particles uniformly and stably dispersed in the solution for a long time, and at the same time, finely crush the particles. Non-limiting examples of usable dispersants include organic acids with carboxyl groups such as citric acid, polyacrylic acid (PAA) or its salts, copolymers, or combinations thereof. The dispersant can be used in an amount of 0.01 to 1% by weight relative to the weight of the powder in the slurry.
[0066] In addition, the binder is added to maintain the molding strength of the molded body during the molding process after the slurry is dried into powder. As non-limiting examples, there are polymers such as polyvinyl alcohol and polyethylene glycol. The amount of the binder used can be less than 2% by weight, specifically, greater than or equal to 0.01% by weight and less than 2% by weight, relative to a total of 100% by weight of the powder in the slurry.
[0067] The defoamer is used to remove the foam in the slurry, and silicone oil, octanol, sodium sulfate, etc. are commonly used. The usage amount of the defoamer can be in the range of 0.001 to 0.01 weight % relative to the powder in the slurry.
[0068] The above-mentioned indium oxide powder, zinc oxide powder, gallium oxide powder, water and one or more additives are mixed to prepare slurry, and the slurry is ground and dried to prepare dry powder.
[0069] At this time, grinding (crushing) can be performed using a conventional ball mill, bead mill, etc. in the art. In addition, there is no particular limitation on the crushing conditions. As an example, the crushing speed can be 1,000 to 2,500 rpm, and the time can be 5 to 10 hours. Preferably, the viscosity of the slurry obtained by grinding is maintained in the range of 250 to 450 Cps, and the amount of the binder is adjusted to less than 2 weight %.
[0070] The ground slurry can be spray dried using a conventional spray dryer in the art to obtain a dry powder in the form of particles. In this case, the spray drying may refer to a method of spraying the slurry into hot air or air at high pressure through a nozzle to form particles. The produced granular powder can be further subjected to a sieving process using a sieve of 120 mesh or less to make it uniform.
[0071] After that, a molding step is performed, in which the dried granular powder is manufactured into a molded body having a predetermined shape. After the granular powder is put into a molding die, a molded body having a desired shape is manufactured, for example, preferably by cold isostatic pressing (CIP). At this time, the pressurizing conditions are not particularly limited, and for example, the pressurizing is performed in the range of 200 to 350 MPa.
[0072] Next is the step of sintering the molded body to prepare an oxide sintered body.
[0073] The sintering step may be carried out at a temperature of 1,200 to 1,600° C. for 10 to 40 hours in an atmosphere (air) or oxygen. At this time, air or oxygen is injected into the atmosphere gas, and this gas plays a role in preventing oxides from being gasified during the sintering step.
[0074] The oxide sintered body having the above combination according to the present invention can be used as a sputtering target, for example, to form an oxide thin film with high electron mobility. The thin film can be used as a channel layer of a thin film transistor, which can ensure high electron mobility characteristics and provide a thin film transistor (TFT) with stability.
[0075] In the process of film formation by the sputtering process, for example, after the manufactured oxide sintered body is processed into a predetermined size and shape, it is attached to a cooling metal plate or a backing plate to be used as a sputtering target. Thereafter, while supplying argon gas mixed with oxygen in the range of 0 to 1% into a vacuum container at a rate of 80 sccm, the sputtering target is sputtered to manufacture an oxide semiconductor thin film used as a channel layer of a thin film transistor.
[0076] Another embodiment of the present invention provides a thin film transistor, which includes a substrate, a gate, an insulating film, a channel layer, a source electrode and a drain electrode, wherein the channel layer includes the oxide sintered body. In addition to the above-mentioned components, the thin film transistor may further include a sacrificial layer, an etch stop layer or a protective layer known in the art as needed.
[0077] The thin film transistor of one embodiment has a channel layer formed by the oxide sintered body of the present invention, and thus can exhibit a 30 cm 2 / Vs or higher, and the carrier concentration can be less than 1.0×10 19 / cm 3 Specifically, the carrier concentration of the thin film transistor may be 1.0×10 16 / cm 3 ~1.0×10 19 / cm 3 , 1.0×10 16 / cm 3 ~1.0×10 18 / cm 3 or 1.0×10 16 / cm 3 ~1.0×10 17 / cm 3 .
[0078] The thin film transistor (TFT) is an active element having a function of applying a voltage to a gate, controlling a current flowing through a channel layer, and switching the current between a source electrode and a drain electrode.
[0079] In addition to using an oxide thin film formed by the oxide sintered body of the above combination as a channel layer, the thin film transistor may include a conventional structure in the art. In this case, the channel layer may be an oxide thin film formed by sputtering a target material comprising the oxide sintered body of the present invention. The type of such a thin film transistor is not particularly limited, and as an example, it may be a bottom gate type or an etch stop type.
[0080] According to an implementation example of the present invention, the thin film transistor may be a bottom gate type further comprising a sacrificial layer formed on the channel layer and having a source and a drain formed on the sacrificial layer. Preferably, the gate is located below the channel layer and the source and the drain are located on the sacrificial layer in a manner of contacting both ends of the channel layer.
[0081] According to another implementation example of the present invention, the thin film transistor may be an etch stop type (ESL) further including an etch stop layer (ESL) formed on the channel layer and a source and a drain formed on the ESL layer. Preferably, the gate is located below the channel layer, the source and the drain are located on the etch stop layer (ESL), and the two electrodes are in contact with both ends of the channel layer. At this time, the source and the drain are in contact with the channel layer by conventional methods in the art, such as through vias.
[0082] The substrate may be made of any material commonly used for semiconductor device substrates, and is not limited thereto. For example, silicon (Si), glass, inorganic materials, organic materials, or metals may be used without limitation.
[0083] At this time, there is no particular restriction on the thickness of the substrate. When a flexible substrate is used, the thickness is preferably in the range of 50 μm to 500 μm. When the thickness of the flexible substrate is less than 50 μm, it is difficult to maintain sufficient flatness of the substrate itself. When the thickness of the flexible substrate is greater than 500 μm, the flexibility of the substrate itself is insufficient, and therefore, it is difficult to flexibly bend the substrate itself.
[0084] The substrate may also form a moisture barrier layer (gas barrier layer) on its surface or back to prevent water vapor and oxygen from penetrating. The material of the moisture barrier layer (gas barrier layer) may appropriately use inorganic substances such as silicon nitride and silicon oxide. The moisture barrier layer (gas barrier layer) may be formed, for example, by a high-frequency sputtering method. In addition, when a thermoplastic substrate is used, a hard coating layer, a primer layer, etc. may be further formed as needed.
[0085] The gate is used to apply a voltage for turning on / off the thin film transistor. The gate may be formed using a conductive material such as a metal or a metal oxide, and as an example, may be formed using a metal such as Pt, Ru, Au, Ag, Mo, Al, W, or Cu, or an alloy thereof, a metal such as IZO (InZnO) or AZO (AlZnO), or a conductive oxide, and an organic conductive compound such as polyaniline, polythiophene, polypyrrole, or a mixture thereof.
[0086] Based on the reliability of TFT characteristics, the gate electrode is preferably made of Mo, Mo alloy or Cr. The thickness of the gate electrode may be, for example, in the range of 10 nm to 1,000 nm.
[0087] There is no particular limitation on the method for forming the gate. For example, the gate is formed by a wet method such as a printing method, a coating method, a physical method such as a vacuum deposition method, a sputtering method, an ion plating method, a chemical method such as a CVD method, a plasma CVD method, etc. Among them, the method for forming the material suitable for forming the gate can be appropriately selected. For example, when Mo or a Mo alloy is used to form the gate, a DC sputtering method is used. In addition, when an organic conductive compound is used in the gate, a wet film forming method can be used.
[0088] The gate insulating film can be formed using a conventional insulating material used for semiconductor elements, and silicon oxide or silicon nitride can be used. For example, SiO 2 Or the dielectric constant is higher than SiO 2 High-K material is HfO 2 、Al 2 O 3 、Si 3 N 4 、SiNx、YsO 3 、 2 O 5 Alternatively, a double-layer film formed of these materials or a polymer insulator such as polyimide can also be used.
[0089] There is no particular limitation on the thickness of the gate insulating film. As an example, it is preferably in the range of 10 nm to 10 μm. The gate insulating film needs to be thicker to a certain extent to improve voltage tolerance and thus reduce leakage current. However, when the thickness of the gate insulating film increases, the driving voltage of the TFT increases. Therefore, when the gate insulating film is an inorganic insulator, its thickness is more preferably 50 nm to 1,000 nm, and when it is a polymer insulator, it is more preferably 0.5 μm to 5 μm.
[0090] In addition, when using HfO 2 When an insulator with a high dielectric constant is used as the gate insulating film, the transistor can be driven at a low voltage even if the film thickness is increased. Therefore, it is preferable to use an insulator with a high dielectric constant as the gate insulating film.
[0091] The source and drain can be formed using conductive materials, respectively. For example, metals such as Pt, Ru, Au, Ag, Mo, Al, W, Cu, Cr, Ta, Ti or their alloys, alloys such as Al-Nd, APC, tin oxide, zinc oxide, indium oxide, indium tin oxide (ITO), indium zinc oxide (IZO) or AZO (AlZnO) can be used to form the conductive materials. Based on the reliability of TFT characteristics and the etching speed of the sacrificial layer, molybdenum (Mo) or Mo alloy is preferably used as the material of the source and drain. In addition, the thickness of the source and drain can be in the range of 10nm to 1,000nm.
[0092] The source electrode and the drain electrode can be formed by a conventional method in the art. For example, they can be formed by forming a film, forming a resist pattern on the film using photolithography, and then etching the film.
[0093] In addition, there is no particular limitation on the method for forming the film consisting of the source and drain electrodes. As an example, it can be formed using wet methods such as printing and coating, physical methods such as vacuum deposition, sputtering, and ion plating, and chemical methods such as CVD and plasma CVD.
[0094] In the present invention, when Mo or Mo alloy is used to form the source and drain, as an example, after a Mo film or Mo alloy film is formed by DC sputtering, a photolithography method is used to form an anti-etching pattern on the Mo film or Mo alloy film, and then the Mo film or Mo alloy film is etched with an etching solution to form the source and drain.
[0095] If necessary, the present invention may further include a sacrificial layer or an etch stopper layer (ESL) to effectively protect the channel layer.
[0096] The composition of the sacrificial layer is not particularly limited, as long as it is known in the art. As an example, an amorphous oxide thin film can be formed by sputtering using an oxide sintered body having a composition similar to that of the oxide sintered body constituting the channel layer. In this case, the film thickness of the sacrificial layer is preferably adjusted to scope.
[0097] In addition, the etching stop layer can be formed using an inorganic insulating material, for example, a material selected from SiO, SiN, Al 2 O 3 and TiO 2 The etch stop layer can be patterned by dry etching.
[0098] In addition to the above-mentioned configurations, the present invention may further include a protection layer to protect the channel layer, the source electrode and the drain electrode and to insulate the transistor from electronic devices fabricated on the transistor.
[0099] The protective layer can be formed by curing a conventional photosensitive resin composition or thermosetting resin composition in the art, or a resin composition in which metal oxides, metal nitrides, metal fluorides, etc. are added.
[0100] There is no particular limitation on the method for forming the protective layer. For example, it can be formed by vacuum deposition, sputtering, reactive sputtering, MBE (molecular beam epitaxy), cluster ion beam, ion plating, plasma polymerization (high-frequency excitation ion plating), plasma CVD, laser CVD, thermal CVD, gas source CVD, coating, printing or transfer.
[0101] The thin film transistor of the present invention can be manufactured by conventional methods in the art. As an example, it can be manufactured by the following processes: a process of forming a gate on a substrate; a process of forming a gate insulating layer on the gate; a process of forming a channel layer formed of an oxide semiconductor on the gate insulating layer; a process of forming a source and a drain on the channel layer; and a process of making the source and the drain contact the two ends of the channel layer.
[0102] At this time, as needed, a process of forming a sacrificial layer or an etch stop layer on the channel layer may be further included.
[0103] The thin film transistor of the present invention as described above can be used as an electrode, an active layer, a switching element, or a driving element in a flat panel display such as a liquid crystal display (LCD) and an organic light emitting display (OLED).
[0104] As described above, the mobility of the channel layer of the transistor of the present invention is 30 cm 2 / Vs or above, and the carrier concentration is stable at less than 1.0×10 19 / cm 3 Therefore, when it is used for a flat panel display, the reliability of the flat panel display can be improved. In particular, even if the size of the display is increased, it can be used stably.
[0105] Implementation
[0106] Hereinafter, a plurality of specific embodiments of the present invention are proposed. However, the plurality of embodiments described below are only used to specifically illustrate or describe the present invention, and the present invention is not limited thereto. In addition, the contents not recorded here can be derived by those skilled in the art, and therefore, the detailed description thereof is omitted.
[0107] [Example 1]
[0108] (1) Weigh 1,152 g of indium oxide (In 2 O 3 ) powder, 680g of zinc oxide (ZnO) powder and 173g of gallium oxide (Ga 2 O 3 ) powder as a raw material, mixed with ultrapure water (de-ionized water), and then dispersed in a bead mill mixer using 0.3 mm zirconium dioxide beads to prepare a wet slurry. The dispersed slurry was spray dried to obtain a density of 1.54 g / cm 3 Spherical powder for molding.
[0109] The molding was performed by cold isostatic pressing (CIP) at a pressure of 250 MPa.
[0110] The molded body was then sintered at 1,450°C for 10 hours and oxygen gas was injected at a flow rate of 40 L / min. The relative density of the oxide sintered body of Example 1 produced in the above manner was measured to be 98.7%.
[0111] The oxide sintered body was analyzed using inductively coupled plasma mass spectrometry (ICP-MS), and it was confirmed that an atomic ratio of In:Zn:Ga:O=4.5:4.5:1:12.75 was formed.
[0112] (2) In order to manufacture a thin film transistor using the manufactured oxide sintered body, Mo metal was deposited on a 6-inch silicon wafer, patterned, and a silicon (Si)-based gate insulating film was deposited.
[0113] Then, the oxide sintered body produced in (1) was installed in a DC magnetron sputtering apparatus, and the initial vacuum degree in the chamber was adjusted to 1×10 -6 Torr or less, and then, at atmospheric temperature, a thin film with a thickness of 100nm was manufactured on the silicon wafer with the above pattern formed. After that, after depositing the source and drain electrodes, the pattern was formed, and finally a protective film was formed, thereby manufacturing a thin film transistor.
[0114] (3) The current-voltage characteristics of the thin film transistor manufactured in (2) were measured, and the results are shown in FIG. Figure 3The turn on voltage was confirmed to be -0.25±0.13V, and the subthreshold swing (SS) value was 0.26±0.0V / dec. In addition, the electron mobility and carrier concentration were measured by Hall effect measurement, and the electron mobility was 32.2cm 2 / Vs, carrier concentration is 1.0×10 16 ~1.0×10 17 / cm 3 .
[0115] (4) In addition, the positive gate bias temperature stress (PBTS; Positive gate Bias and Temperature Stress, Vg_stress = 20V, Vd = 0.1V@60deg) and the reverse gate bias temperature stress (NBTS; Negative gate Bias and Temperature Stress, Vg_stress = -20V, Vd = 0.1V@60deg) of the thin film transistor were measured, and the results are shown in Figure 4 and Figure 5 The reliability measurement result is, βV th They were 0.45 V and -0.3 V respectively, which were very good values.
[0116] [Example 2]
[0117] (1) An oxide sintered body was prepared in the same manner as in Example 1 except that the atomic ratio was In:Zn:Ga:O=5:4:1:13, and a thin film transistor having a channel layer including the oxide sintered body was manufactured in the same manner as in Example 1.
[0118] (2) The current-voltage characteristics of the thin film transistor manufactured in (1) were measured, and the turn on voltage was -0.26±0.1V, and the subthreshold swing (SS) value was 0.23±0.0V / dec. In addition, the electron mobility and carrier concentration were measured by Hall effect measurement, and the electron mobility was 33.6cm 2 / Vs, carrier concentration is 1.0×10 17 ~1.0×10 18 / cm 3 .
[0119] (3) In addition, the reliability of the positive gate bias temperature stress (PBTS; Positive gate Bias and Temperature Stress, Vg_stress = 20V, Vd = 0.1V@60deg) and the negative gate bias temperature stress (NBTS; Negative gate Bias and Temperature Stress, Vg_stress = -20V, Vd = 0.1V@60deg) of the thin film transistor was measured. The results showed that βV th The values obtained were 0.48V and -0.32V respectively.
[0120] [Example 3]
[0121] (1) An oxide sintered body was prepared in the same manner as in Example 1 except that the atomic ratio was In:Zn:Ga:O=5.25:3.75:1:13.125, and a thin film transistor having a channel layer including the oxide sintered body was manufactured in the same manner as in Example 1.
[0122] (2) The current-voltage characteristics of the thin film transistor manufactured in (1) were measured, and the turn on voltage was -0.18±0.1V, and the subthreshold swing (SS) value was 0.19±0.02V / dec. In addition, the electron mobility and carrier concentration were measured by Hall effect measurement, and the electron mobility was 31.4cm 2 / Vs, carrier concentration is 1.0×10 16 ~1.0×10 17 / cm 3 .
[0123] (3) In addition, the reliability of the positive gate bias temperature stress (PBTS; Positive gate Bias and Temperature Stress, Vg_stress = 20V, Vd = 0.1V@60deg) and the negative gate bias temperature stress (NBTS; Negative gate Bias and Temperature Stress, Vg_stress = -20V, Vd = 0.1V@60deg) of the thin film transistor was measured. The results showed that βV th The values obtained were 0.26V and -0.28V respectively.
[0124] [Example 4]
[0125] (1) An oxide sintered body was prepared in the same manner as in Example 1 except that the atomic ratio was In:Zn:Ga:O=6:3:1:13.5, and a thin film transistor having a channel layer including the oxide sintered body was manufactured in the same manner as in Example 1.
[0126] (2) The current-voltage characteristics of the thin film transistor manufactured in (1) were measured, and the turn on voltage was -0.54±0.1V, and the subthreshold swing (SS) value was 0.12±0.01V / dec. In addition, the electron mobility and carrier concentration were measured by Hall effect measurement, and the electron mobility was 30.8cm 2 / Vs, carrier concentration is 1.0×10 16 ~1.0×10 17 / cm 3 .
[0127] (3) In addition, the reliability of the positive gate bias temperature stress (PBTS; Positive gate Bias and Temperature Stress, Vg_stress = 20V, Vd = 0.1V@60deg) and the negative gate bias temperature stress (NBTS; Negative gate Bias and Temperature Stress, Vg_stress = -20V, Vd = 0.1V@60deg) of the thin film transistor was measured. The results showed that βV th The values obtained were 0.16V and -0.62V respectively.
[0128] [Comparative Example 1]
[0129] (1) An oxide sintered body was prepared in the same manner as in Example 1 except that the atomic ratio was In:Zn:Ga:O=1:1:1:4, and a thin film transistor having a channel layer including the oxide sintered body was manufactured in the same manner as in Example 1.
[0130] (2) The current-voltage characteristics of the thin film transistor manufactured in (1) were measured, and the results are shown in FIG. Figure 6The turn on voltage is 1.53±0.22V, and the subthreshold swing (SS) value is 0.41±0.02V / dec. In addition, the electron mobility and carrier concentration were measured by Hall effect measurement, and the electron mobility was 12.0cm 2 / Vs, carrier concentration is 1.0×10 15 ~1.0×10 16 / cm 3 .
[0131] (3) In addition, the positive gate bias temperature stress (PBTS; Positive gate Bias and Temperature Stress, Vg_stress = 20V, Vd = 0.1V@60deg) and the reverse gate bias temperature stress (NBTS; Negative gate Bias and Temperature Stress, Vg_stress = -20V, Vd = 0.1V@60deg) of the thin film transistor were measured, and the results are shown in Figure 7 and Figure 8 The reliability measurement result is, βV th The values obtained were 4.02V and -0.16V respectively.
[0132] [Comparative Example 2]
[0133] (1) An oxide sintered body was prepared in the same manner as in Example 1 except that the atomic ratio was In:Zn:Ga:O=2:2:1:6.5, and a thin film transistor having a channel layer including the oxide sintered body was manufactured in the same manner as in Example 1.
[0134] (2) The current-voltage characteristics of the thin film transistor manufactured in (1) were measured, and the turn-on voltage was 1.12±0.1V, and the subthreshold swing (SS) value was 0.38±0.02V / dec. In addition, the electron mobility and carrier concentration were measured by Hall effect measurement, and the electron mobility was 16.4cm 2 / Vs, carrier concentration is 1.0×10 15 ~1.0×10 16 / cm 3 .
[0135] (3) In addition, the reliability of the positive gate bias temperature stress (PBTS; Positive gate Bias and Temperature Stress, Vg_stress = 20V, Vd = 0.1V@60deg) and the negative gate bias temperature stress (NBTS; Negative gate Bias and Temperature Stress, Vg_stress = -20V, Vd = 0.1V@60deg) of the thin film transistor was measured. The results showed that βV th The values obtained were 3.62V and -0.26V respectively.
[0136] [Comparative Example 3]
[0137] (1) An oxide sintered body was prepared in the same manner as in Example 1 except that the atomic ratio was In:Zn:Ga:O=3:2.5:1:8.5, and a thin film transistor having a channel layer including the oxide sintered body was manufactured in the same manner as in Example 1.
[0138] (2) The current-voltage characteristics of the thin film transistor manufactured in (1) were measured, and the turn on voltage was 0.28±0.26V, and the subthreshold swing (SS) value was 0.32±0.04V / dec. In addition, the electron mobility and carrier concentration were measured by Hall effect measurement, and the electron mobility was 15.2cm 2 / Vs, carrier concentration is 1.0×10 15 ~1.0×10 16 / cm 3 .
[0139] (3) In addition, the reliability of the positive gate bias temperature stress (PBTS; Positive gate Bias and Temperature Stress, Vg_stress = 20V, Vd = 0.1V@60deg) and the negative gate bias temperature stress (NBTS; Negative gate Bias and Temperature Stress, Vg_stress = -20V, Vd = 0.1V@60deg) of the thin film transistor was measured. The results showed that βV th The values obtained were 3.8V and -0.12V respectively.
[0140] [Comparative Example 4]
[0141] (1) An oxide sintered body was prepared in the same manner as in Example 1 except that the atomic ratio was In:Zn:Ga:O=2.5:3:1:8.25, and a thin film transistor having a channel layer including the oxide sintered body was manufactured in the same manner as in Example 1.
[0142] (2) The current-voltage characteristics of the thin film transistor manufactured in (1) were measured, and the turn on voltage was 0.84±0.16V, and the subthreshold swing (SS) value was 0.64±0.02V / dec. In addition, the electron mobility and carrier concentration were measured by Hall effect measurement, and the electron mobility was 19.0cm 2 / Vs, carrier concentration is 1.0×10 15 ~1.0×10 16 / cm 3 .
[0143] (3) In addition, the reliability of the positive gate bias temperature stress (PBTS; Positive gate Bias and Temperature Stress, Vg_stress = 20V, Vd = 0.1V@60deg) and the negative gate bias temperature stress (NBTS; Negative gate Bias and Temperature Stress, Vg_stress = -20V, Vd = 0.1V@60deg) of the thin film transistor was measured. The results showed that βV th The values obtained were 5.8V and -0.29V respectively.
[0144] The preferred embodiments of the present invention are described in detail above, but the scope of the present invention is not limited thereto but is defined by the appended claims. Various modifications and improvements made by those skilled in the art using the basic concepts of the present invention also fall within the scope of the present invention.
Claims
1. An oxide sintered body comprising an In element, a Zn element, a Ga element and oxygen, in, The atomic ratio of In element to Zn element is 1 to 2:
1. The atomic ratio of In element to Ga element is 3 to 6:
1. The atomic ratio of Zn element to Ga element is 3 to 6:
1.
2. The oxide sintered body according to claim 1, in, The oxide sintered body is represented by Chemical Formula 1, Chemical formula 1: In x Zn y Ga z O (3x / 2+y+3z / 2) In the chemical formula 1, x:y=1-2:1, x:z=3-6:1, y:z=3-6:
1.
3. The oxide sintered body according to claim 1, in, In the oxide sintered body, The atomic ratio of In element to Zn element is 1 to 1.5:
1. The atomic ratio of In element to Ga element is 4 to 5:
1. The atomic ratio of Zn element to Ga element is 4 to 5:
1.
4. The oxide sintered body according to claim 1, in, The relative density of the oxide sintered body is 98.0% to 99.9%.
5. A thin film transistor comprising a substrate, a gate, an insulating film, a channel layer, a source electrode and a drain electrode, The channel layer includes the oxide sintered body according to any one of claims 1 to 4.
6. The thin film transistor according to claim 5, in, The channel layer includes an oxide thin film formed by sputtering a target including the oxide sintered body.
7. The thin film transistor according to claim 5, in, The electron mobility of the channel layer is 30 cm 2 / Vs or above.
8. The thin film transistor according to claim 5, in, The carrier concentration of the channel layer is less than 1.0×10 19 / cm 3 .