Film structure and electronic device
By using the ZrO2 buffer film and the c-axis-oriented LiNbO3 or LiTaO3 piezoelectric film on the Si(100) substrate, combined with the metal film, the problem of difficulty in aligning the polarization direction on the Si(100) substrate is solved. The vertical alignment of the piezoelectric film and the improvement of the electronic device performance are achieved.
Patent Information
- Application Number
- CN202380033915.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2023-04-07
- Publication Date
- 2024-11-22
AI Technical Summary
On the Si(100) substrate, it is difficult to align the polarization direction of the piezoelectric film having an ilmenite structure to a direction perpendicular to the substrate.
Using Si(100) substrate or SOI substrate, a buffer film ZrO2 is formed, and a c-axis-oriented LiNbO3 or LiTaO3 piezoelectric film is grown thereon, combined with a metal film such as Pt, Mo, Ru or Cu, and on the piezoelectric film A SrRuO3 film is formed between the metal film to ensure that the polarization direction of the piezoelectric film is perpendicular to the substrate.
The polarization direction of the piezoelectric film on the Si(100) substrate is realized and the substrate is aligned perpendicularly, thereby improving the orientation consistency of the piezoelectric film and the performance of the electronic device.
Smart Images

Figure CN119014148A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a film structure and an electronic device. Background Art
[0002] A film structure having a substrate and a piezoelectric film formed on the substrate, and an electronic device having the film structure are known. In addition, as a piezoelectric film, a piezoelectric film having an ilmenite structure such as lithium niobate (LiNbO3) is known.
[0003] In Japanese Patent Gazette No. 2013-173647 (Patent Document 1), the following technology is disclosed: in a dielectric stacked thin film, on a single crystal Si (111) substrate surface, at least one layer of epitaxially grown base film having zirconium oxide (ZrO2) as a main component is formed, and on the base film, an epitaxially grown ilmenite structure film composed of a dielectric material having an ilmenite structure is formed.
[0004] In Japanese Patent Gazette No. 2016-109856 (Patent Document 2), the following technology is disclosed: it has a single crystal substrate, a dielectric layer, and a buffer layer arranged between the single crystal substrate and the dielectric layer, the dielectric layer is lithium niobate (LiNbO3) or lithium tantalate (LiTaO3), the c-axis of the crystals constituting the dielectric layer is roughly parallel to the main surface of the single crystal substrate, and the buffer layer is hexagonal LiNbO2 or LiTaO2, and the c-axis of the crystals constituting the buffer layer is roughly parallel to the main surface of the single crystal substrate.
[0005] Prior Art Literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2013-173647
[0008] Patent Document 2: Japanese Patent Application Publication No. 2016-109856 Summary of the invention
[0009] -Problems to be solved by the invention-
[0010] In the technology described in the above-mentioned patent document 1, on a Si(111) substrate, the piezoelectric film, i.e., the LiNbO3 film, is c-axis oriented, and the polarization direction of the piezoelectric film is oriented perpendicular to the substrate. In this way, on a Si(111) substrate, the polarization direction of the piezoelectric film having an ilmenite structure can be aligned in a direction perpendicular to the substrate. On the other hand, there is also the following situation: instead of the Si(111) substrate, preferably on a Si(100) substrate which is a general and inexpensive semiconductor substrate, the polarization direction of the piezoelectric film having an ilmenite structure is aligned in a direction perpendicular to the substrate, but it is difficult to align the orientation direction of the piezoelectric film having an ilmenite structure on a Si(100) substrate in a direction perpendicular to the substrate.
[0011] The present invention is proposed to solve the problems of the prior art as mentioned above, and its purpose is to provide a membrane structure in which, in a membrane structure having a piezoelectric film formed on a substrate, the polarization direction of the piezoelectric film can be aligned in a direction perpendicular to the substrate even when the substrate is a Si (100) substrate and the piezoelectric film has an ilmenite structure.
[0012] -Methods for solving problems-
[0013] The outline of the representative aspects of the invention disclosed in this application will be briefly described as follows.
[0014] A membrane structure as one embodiment of the present invention comprises: a substrate; a buffer film formed on the substrate; and a piezoelectric film formed on the buffer film, wherein the substrate is a Si (100) substrate or an SOI substrate, wherein the SOI substrate comprises a base composed of a Si substrate, an insulating layer on the substrate, and an SOI layer composed of a Si (100) film on the insulating layer, wherein the buffer film comprises ZrO2, and the piezoelectric film comprises c-axis oriented LiNbO3 or LiTaO3.
[0015] Furthermore, as another embodiment, the film structure may include a metal film formed between the buffer film and the piezoelectric film.
[0016] In addition, as another embodiment, the metal film may include (100)-oriented Pt.
[0017] In addition, as another embodiment, the metal film may be a Pt film, a Mo film, a W film, a Ru film, or a Cu film.
[0018] In addition, as another embodiment, the film structure may include a SrRuO 3 film formed between the metal film and the piezoelectric film, wherein the SrRuO 3 film has a cubic crystal structure and is (100) oriented.
[0019] An electronic device as one embodiment of the present invention is an electronic device including the film structure.
[0020] An electronic device as one embodiment of the present invention is an electronic device including the film structure, wherein the film structure has a comb-tooth electrode formed on the upper surface or the lower surface of the piezoelectric film.
[0021] Furthermore, as another embodiment, the film structure may include a matching layer formed on the substrate.
[0022] In addition, as another aspect, a hollow portion may be provided at the lower portion of the piezoelectric film.
[0023] In another embodiment, the film structure may include an upper electrode formed on the upper portion of the piezoelectric film and a lower electrode formed on the lower portion of the piezoelectric film.
[0024] In addition, as another aspect, the area of the overlapping portion between the upper electrode and the lower electrode may be smaller than the area of the hollow portion.
[0025] In addition, as another aspect, the area of the overlapping portion between the upper electrode and the lower electrode may be equal to or less than 1 / 2 of the area of the hollow portion.
[0026] Furthermore, as another embodiment, the film structure may include a matching layer formed on the substrate.
[0027] In another aspect, the matching layer may be made of a material whose hardness increases with an increase in temperature.
[0028] In addition, as another embodiment, the material may be a Si compound.
[0029] -Effects of the Invention-
[0030] By applying one method of the present invention, in a film structure having a piezoelectric film formed on a substrate, even when the substrate is a Si (100) substrate and the piezoelectric film has an ilmenite structure, the polarization direction of the piezoelectric film can be aligned in a direction perpendicular to the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a cross-sectional view of the membrane structure according to the first embodiment.
[0032] Figure 2 This is a cross-sectional view of the membrane structure according to the first embodiment.
[0033] Figure 3 This is a cross-sectional view of the membrane structure according to the first embodiment.
[0034] Figure 4 This is a cross-sectional view of the membrane structure according to the first embodiment.
[0035] Figure 5This is a cross-sectional view of the membrane structure according to the first embodiment.
[0036] Figure 6 This is a cross-sectional view of the membrane structure according to the first embodiment.
[0037] Figure 7 This is a cross-sectional view of an electronic device according to the second embodiment.
[0038] Figure 8 This is a cross-sectional view of an electronic device according to the second embodiment.
[0039] Fig. 9 This is a cross-sectional view of an electronic device according to the second embodiment.
[0040] Fig.10 This is a cross-sectional view of an electronic device according to the second embodiment.
[0041] Fig.11 This is a cross-sectional view of an electronic device according to the second embodiment.
[0042] Fig.12 This is a cross-sectional view of an electronic device according to the second embodiment.
[0043] Fig.13 This is a cross-sectional view of an electronic device according to the second embodiment.
[0044] Fig.14 This is a cross-sectional view of an electronic device according to the second embodiment.
[0045] Fig.15 This is a perspective view of an electronic device according to a third embodiment.
[0046] Fig.16 This is a perspective view of an electronic device according to a third embodiment.
[0047] Fig.17 This is a perspective view of an electronic device according to a third embodiment.
[0048] Fig.18 This is a diagram showing the crystal structure of c-axis oriented LiNbO 3.
[0049] Fig.19 This is a graph showing an example of the ω-2θ spectrum of the film structure of Example 1 obtained by the XRD method.
[0050] Fig. 20 This is a graph showing an example of the ω-2θ spectrum of the film structure of Example 2 obtained by the XRD method.
[0051] Fig.21 This is a graph showing an example of the ω-2θ spectrum of the film structure of Example 3 obtained by the XRD method.
[0052] Fig. 22This is a graph showing the results of reciprocal lattice mapping of the film structure of Example 1.
[0053] Fig.23 This is a graph showing the results of reciprocal lattice mapping of the film structure of Example 2.
[0054] Fig.24 The XRD results of the film structure of Example 1 are shown. Graph of an example of a scan spectrum.
[0055] Fig.25 The XRD results of the film structure of Example 2 are shown. Graph of an example of a scan spectrum.
[0056] Fig.26 The rotation angle of the rotation component and the symmetry of the crystal structure composed of hexagonal and trigonal crystals are shown. This is a table in which the apparent symmetry of the crystal structure determined by the number of diffraction peaks observed in the scanning spectrum is classified and organized.
[0057] Fig. 27 This is a graph showing the voltage dependence of polarization of the film structure of Example 2. DETAILED DESCRIPTION
[0058] Hereinafter, embodiments of the present invention will be described with reference to the drawings.
[0059] In addition, the present disclosure is only an example, and any suitable changes that can be easily thought of by those skilled in the art to maintain the gist of the present invention are of course included in the scope of the present invention. In addition, in order to make the description clearer, the drawings sometimes schematically show the width, thickness, shape, etc. of each part compared with the embodiment, but this is only an example and does not limit the interpretation of the present invention.
[0060] In addition, in this specification and each figure, about the figure which has already appeared, the same code|symbol is attached|subjected to the element similar to the above-mentioned element, and the detailed description may be abbreviate|omitted suitably.
[0061] Furthermore, in the drawings used for the embodiments, hatching added to distinguish structures may be omitted depending on the drawings.
[0062] In the following embodiments, when a range is shown as A to B, it means A or more and B or less unless otherwise specified.
[0063] (Implementation Method 1)
[0064] First, a film structure according to Embodiment 1 which is one embodiment of the present invention will be described. Figures 1 to 6 This is a cross-sectional view of the membrane structure according to the first embodiment.
[0065] like Figure 1 As shown, the film structure 10 of the first embodiment is a film structure having a piezoelectric film 11 and a substrate 12, and is characterized in that the polarization direction of the piezoelectric film 11, that is, the piezoelectric film portion is preferentially oriented perpendicular to the substrate 12. Figure 1 In the figure, the polarization direction is shown by the polarization direction DP1 (in Figure 2 as well as Figures 7 to 17 The same is true in FIG. 1 . By orienting the polarization direction of the piezoelectric film 11 preferentially to be perpendicular to the substrate 12 , a film structure can be realized in which the polarization direction of the piezoelectric film is aligned in a direction perpendicular to the substrate.
[0066] Or, if Figure 2 As shown, the film structure 10 of the present embodiment 1 is a film structure having a piezoelectric film 11, an electrode 13, and a substrate 12, and is characterized in that the polarization direction of the piezoelectric film 11, that is, the piezoelectric film portion is preferentially oriented to be perpendicular to the substrate 12. As described above, by preferentially oriented the polarization direction of the piezoelectric film 11 to be perpendicular to the substrate 12, a film structure can be realized in which the polarization direction of the piezoelectric film is aligned in a direction perpendicular to the substrate.
[0067] In addition, in the present application specification, the polarization direction of the piezoelectric film 11 is preferentially oriented to be perpendicular to the substrate 12, which means that the portion of the piezoelectric film 11 whose polarization direction is oriented perpendicular to the substrate 12 exceeds 50% of the entire piezoelectric film 11 in terms of volume fraction, for example, when measuring the θ-2θ spectrum of the X-ray Diffraction (XRD) method, in the measured θ-2θ spectrum, the peak intensity of the maximum peak representing the portion whose polarization direction is oriented perpendicular to the substrate 12 is higher than the peak intensity of the maximum peak representing the portion whose polarization direction is not oriented perpendicular to the substrate 12. In addition, the so-called case where the polarization direction becomes perpendicular to the substrate 12 includes not only the case where the polarization direction is completely perpendicular to the upper surface of the substrate 12, but also the case where the angle formed by the direction perpendicular to the upper surface of the substrate 12 and the polarization direction is less than 20°.
[0068] In the film structure 10 of the present embodiment 1, the piezoelectric film 11 contains lithium niobate (LiNbO3, hereinafter also referred to as "LN") or lithium tantalate (LiTaO3) oriented in the c-axis direction, that is, it contains it as a main component. Alternatively, in the film structure 10 of the present embodiment 1, the piezoelectric film 11 may contain a solid solution of lithium niobate (LiNbO3) and lithium tantalate (LiTaO3) oriented in the c-axis direction, or it may contain it as a main component. LiNbO3 or LiTaO3 has an ilmenite structure as a trigonal structure, and is polarized in the c-axis direction.
[0069] By allowing LiNbO 3 or LiTaO 3 to be c-axis oriented, LiNbO 3 or LiTaO 3 can be oriented so that the c-axis direction, which is the polarization direction of LiNbO 3 or LiTaO 3 , is perpendicular to the substrate 12 .
[0070] In addition, in the present application specification, the piezoelectric film 11 containing LiNbO3 or LiTaO3 as a main component means that the content of LiNbO3 or LiTaO3 in the piezoelectric film 11 exceeds 50 weight%, or the content of LiNbO3 or LiTaO3 in the piezoelectric film 11 exceeds 50 mol%.
[0071] Suitably, such as Figure 3 As shown, the substrate 12 has a structure in which a Si layer and a ZrO2 layer are stacked in sequence. Si represents silicon, and ZrO2 represents zirconium oxide. ZrO2 acts as a buffer film, which helps to form a piezoelectric material formed thereon with good crystallinity. That is, by making the buffer film contain ZrO2 formed on the Si layer, the polarization direction of the piezoelectric film can be aligned in a direction perpendicular to the substrate, and the orientation direction of the piezoelectric film can also be aligned in the in-plane direction along the upper surface of the substrate.
[0072] Suitably, the substrate 12 includes a (100)-oriented Si layer 12a and a ZrO2 layer 12b formed on the Si layer 12a. The ZrO2 layer 12b suitably includes a (200)-oriented ZrO2 and a (002)-oriented ZrO2. As the Si layer 12a of the substrate 12, a (100)-oriented Si substrate, i.e., a Si(100) substrate, can be used. In such a case, a piezoelectric film 11 mainly composed of c-axis-oriented lithium niobate or lithium tantalate, the piezoelectric film 11 having a polarization direction perpendicular to the substrate 12 and epitaxially grown can be easily formed on the substrate 12. Furthermore, since a (100)-oriented Si substrate can be used as the Si layer 12a of the substrate 12, an electronic device can be formed on an inexpensive semiconductor substrate in which the polarization direction of the piezoelectric film 11 is aligned in a direction perpendicular to the substrate and the orientation direction of the piezoelectric film is also aligned in an in-plane direction along the upper surface of the substrate. That is, even when the substrate is a Si (100) substrate and the piezoelectric film has an ilmenite structure, the polarization direction of the piezoelectric film can be aligned in a direction perpendicular to the substrate.
[0073] like Figure 3As shown, the electrode 13 has a structure in which a Pt (200) layer, i.e., a Pt (100) layer, and a SrRuO3 (100) layer are stacked in sequence. Pt represents platinum, and SrRuO3 (SRO) represents strontium ruthenate. In other words, suitably, the electrode 13 includes: a Pt layer 13a, formed on the substrate 12 and having a (200) orientation, i.e., a (100) orientation; and a SRO layer (SrRuO3 film) 13b, formed on the Pt layer 13a, having a cubic crystal structure and a (100) orientation. That is, the metal film (Pt layer 13a) includes Pt in a (100) orientation, the SrRuO3 film is formed between the metal film (Pt layer 13a) and the piezoelectric film 11, and the SrRuO3 film (SRO layer 13b) has a cubic crystal structure and a (100) orientation. In such a case, the piezoelectric film 11 mainly containing c-axis oriented LiNbO 3 or LiTaO 3 can be easily formed on the substrate 12 via the electrode 13 serving as the lower electrode.
[0074] In addition, if Figure 4 As shown in FIG. 1 , the electrode 13 may not have a SrRuO3(100) layer, but may have only a Pt(200) layer, i.e., a Pt(100) layer (Pt layer 13a). Figure 1 As shown, the membrane structure 10 in the first embodiment does not have the electrode 13 (see Figure 2 ), if Figure 5 As shown, the piezoelectric film 11 may be formed directly on the ZrO 2 layer 12 b .
[0075] In addition, the present invention is not limited to the case where the Si layer 12a is (100) oriented, is not limited to the case where the ZrO2 layer 12b is (200) oriented or (002) oriented, is not limited to the case where the Pt layer 13a is (200) oriented, and is not limited to the case where the electrode 13 is formed on the Pt layer 13a and includes the SRO layer 13b with a (100) orientation.
[0076] For example, the substrate 12 may include a (iii)-oriented Si layer 12a and a ZrO2 layer 12b formed on the Si layer 12a. The ZrO2 layer 12b suitably includes, for example, (iii)-oriented ZrO2. As the Si layer 12a of the substrate 12, a (iii)-oriented Si substrate, i.e., a Si(iii) substrate, may be used. In such a case, the piezoelectric film 11 containing c-axis-oriented LiNbO3 or LiTaO3 as a main component may also be easily formed on the substrate 12. In addition, the electrode 13 includes a (iii)-oriented Pt layer 13a formed on the substrate 12.
[0077] In addition, the Si layer 12a of the substrate 12 can be regarded as a substrate. In this case, the film structure 10 of the present embodiment 1 is a film structure as follows, having: a substrate (Si layer 12a) as a Si substrate; a buffer film (ZrO2 layer 12b) formed on the substrate (Si layer 12a) and containing ZrO2; and a piezoelectric film 11 formed on the buffer film (ZrO2 layer 12b) via a metal film (Pt layer 13a), the piezoelectric film 11 containing c-axis oriented LiNbO3 or LiTaO3, and the polarization direction of the piezoelectric film 11 is preferentially oriented perpendicular to the upper surface of the substrate 12. In addition, the piezoelectric film 11 is a piezoelectric film formed on Pt / ZrO2 / Si. Therefore, the metal film (Pt layer 13a) is formed between the buffer film (ZrO2 layer 12b) and the piezoelectric film 11. In addition, when the electrode 13 includes a Pt layer 13a and an SRO layer 13b, that is, when the membrane structure 10 also includes a metal film (Pt layer 13a) on the buffer film (ZrO2 layer 12b) and also includes an SRO film (SRO layer 13b) on the metal film (Pt layer 13a), the piezoelectric film 11 is a piezoelectric film formed on a substrate (Si layer 12a) which is a Si substrate, with a ZrO2 film (ZrO2 layer 12b), a Pt film (Pt layer 13a) and an SRO film (SRO layer 13b) interposed in sequence from the bottom.
[0078] like Figure 6 As shown, instead of a Si (100) substrate, an SOI (Silicon On Insulator) substrate as a semiconductor substrate can be used as the Si layer 12a of the substrate 12. When the SOI substrate is used as the substrate 12, the substrate 12 includes: a base 12c composed of a Si substrate; a BOX (Buried Oxide) layer 12d as a buried oxide film, i.e., an insulating layer, formed on the base 12c; and an SOI (Silicon On Insulator) layer, i.e., the Si layer 12a, composed of a Si (100) film, formed on the BOX layer 12d. Thus, a film structure having excellent dielectric constant characteristics and withstand voltage characteristics of a piezoelectric film can be formed on the SOI substrate, and an electronic device composed of a micro-electromechanical system (MEMS) having a plurality of piezoelectric elements formed with good shape accuracy can be easily formed on the SOI substrate.
[0079] Furthermore, when an SOI substrate is used instead of a Si (111) substrate, an SOI layer composed of a Si (111) film can be used as the (111)-oriented Si layer 12 a of the substrate 12 .
[0080] In addition, the Si layer 12a of the substrate 12 can be regarded as a substrate. In this case, the film structure 10 of the present embodiment 1 is a film structure having: a substrate (Si layer 12a) as an SOI substrate; a buffer film (ZrO2 layer 12b) formed on the substrate (Si layer 12a) and containing ZrO2; and a piezoelectric film 11 formed on the buffer film (ZrO2 layer 12b) via a metal film (Pt layer 13a), the piezoelectric film 11 containing c-axis oriented LiNbO3 or LiTaO3, and the polarization direction of the piezoelectric film 11 is preferentially oriented perpendicular to the upper surface of the substrate 12. In addition, the piezoelectric film 11 is a piezoelectric film formed on Pt / ZrO2 / Si on SOI. In addition, when the electrode 13 includes a Pt layer 13a and an SRO layer 13b, that is, when the membrane structure 10 also includes a metal film (Pt layer 13a) on the buffer film (ZrO2 layer 12b) and also includes an SRO film (SRO layer 13b) on the metal film (Pt layer 13a), the piezoelectric film 11 is a piezoelectric film formed on a substrate (Si layer 12a) which is an SOI substrate, interposed from the bottom with a ZrO2 film (ZrO2 layer 12b), a Pt film (Pt layer 13a) and an SRO film (SRO layer 13b).
[0081] In addition, the electrode 13 can also include a Mo layer 13c or a W layer 13d instead of the Pt layer 13a. In this case, the electrode 13 includes an SRO layer 13b formed on the Mo layer 13c or the W layer 13d. In addition, in this case, the film structure 10 of the present embodiment 1 has a piezoelectric film 11, which is formed on a substrate (Si layer 12a) that is a Si substrate or an SOI substrate, and is sequentially interposed from the bottom with a ZrO2 film (ZrO2 layer 12b) and a Mo film (Mo layer 13c) or a W film (W layer 13d). In addition, in this case, as in the case where the electrode 13 includes the Pt layer 13a, a piezoelectric material such as a piezoelectric film 11 having a piezoelectric film 11 with a polarization direction perpendicular to the substrate 12 and epitaxially grown can be easily formed on the substrate 12 via the electrode 13 that is the lower electrode. In addition, as the material of the electrode 13a, 13c or 13d, in addition to the materials described above, a Ru layer (Ru film) or a Cu layer (Cu film) may be used. These materials are generally used as electrode materials.
[0082] (Implementation Method 2)
[0083] Next, an electronic device according to Embodiment 2 as one embodiment of the present invention will be described. The electronic device according to Embodiment 2 is a bulk acoustic wave (BAW) filter or a piezoelectric thin film resonator (FBAR) including the film structure according to Embodiment 1. Figures 7 to 14 This is a cross-sectional view of an electronic device according to the second embodiment.
[0084] like Figure 7 As shown, the electronic device 20 of the second embodiment is an electronic device including a film structure 10 having a piezoelectric film 11 , two electrodes, and a substrate 12 , and is characterized in that the polarization direction of the piezoelectric film 11 is preferentially oriented perpendicular to the substrate 12 .
[0085] The film structure 10 included in the electronic device 20 of the second embodiment can also include the piezoelectric film 11, the electrode 13, and the substrate 12, similarly to the film structure 10 of the first embodiment. That is, the electronic device 20 of the second embodiment includes the electrode 13 and the piezoelectric film 11 on the substrate 12. Therefore, the description of the parts of the piezoelectric film 11, the electrode 13, and the substrate 12 included in the film structure 10 that are the same as those of the piezoelectric film 11, the electrode 13, and the substrate 12 included in the film structure 10 of the first embodiment may be omitted.
[0086] On the other hand, since the electronic device 20 of the second embodiment is a BAW filter or FBAR having the membrane structure 10 of the first embodiment, a hollow portion, namely, a hollow portion 21, is provided at the bottom of the piezoelectric film 11 for the substrate 12. In this case, since at least the central portion of the portion of the piezoelectric film 11 located above the hollow portion 21 is not constrained by the substrate 12 and can vibrate freely, bulk acoustic waves can be easily generated in the central portion. In addition, since a hollow portion is provided at the bottom of the piezoelectric film 11, when the substrate 12 is etched from the back, the Si layer 12a (see Figure 3 as well as Figure 4 ) is etched away, but the ZrO2 layer 12b (see Figure 3 as well as Figure 4 ) is not etched and remains, which can make it function as an etching stopper film. Figures 7 to 14 For the Zro2 layer 12b (refer to Figure 3 as well as Figure 4 ) is not etched and remains, and is omitted from the illustration.
[0087] In addition, in the membrane structure 10 provided in the electronic device 20 of the second embodiment, an electrode 22 is provided as an upper electrode or an upper portion electrode formed on the piezoelectric film 11. In this case, the electrode 13 is an electrode as a lower electrode or a lower portion electrode formed under the piezoelectric film 11. That is, the electrode 22 and the electrode 13 are an upper portion electrode formed on the upper portion of the piezoelectric film 11, and a lower portion electrode formed on the lower portion of the piezoelectric film 11. Figure 7 In the example shown, electrodes are formed on the upper and lower sides in contact with the piezoelectric film 11. In addition, the film structure 10 is a film structure having the piezoelectric film 11, two electrodes, namely, the electrode 13 and the electrode 22, and the substrate 12, and is characterized in that the polarization direction of the piezoelectric film 11, namely, the piezoelectric film portion is preferentially oriented perpendicular to the substrate 12. In this case, by applying a voltage such as an AC voltage between the electrode 13 and the electrode 22, an electric field such as an AC electric field in the thickness direction of the piezoelectric film 11 can be easily applied to the piezoelectric film 11, and the piezoelectric film 11 can easily generate a bulk acoustic wave. In addition, since a bulk acoustic wave having a resonant frequency determined by the elastic characteristics of the piezoelectric film 11 can be generated or passed, it can function as a resonator or a filter.
[0088] In the second embodiment, as in the first embodiment, a Si layer 12a including a (100) orientation can be used as the substrate 12 (see Figure 3 ), and a ZrO2 layer 12b formed on the Si layer 12a (refer to Figure 3 ) substrate. The ZrO2 layer 12b suitably includes (200)-oriented ZrO2 and (002)-oriented ZrO2. In this case, the Si layer 12a of the substrate 12 can be regarded as a substrate, and the electronic device 20 of the present embodiment 2 is an electronic device as follows: it has an electrode 13 on a substrate (Si layer 12a) as a Si substrate and a piezoelectric film 11, the polarization direction of the piezoelectric film 11 is preferentially oriented perpendicular to the substrate 12, and a hollow portion 21 is provided at the lower portion of the piezoelectric film 11.
[0089] Suitably, the area A of the overlapping portion of the upper and lower electrodes is smaller than the area B of the piezoelectric film 11 and the lower electrode exposed in the hollow portion. That is, the area of the overlapping portion of the electrode 22 as the upper electrode and the electrode 13 as the lower electrode is smaller than the area of the hollow portion 21. In such a case, by applying a voltage between the electrode 22 and the electrode 13, the portion of the piezoelectric film 11 to which the electric field in the thickness direction is applied can be reliably separated from the substrate 12. Therefore, the portion of the piezoelectric film 11 to which the electric field in the thickness direction is applied can vibrate freely without being constrained by the substrate 12, and bulk acoustic waves can be generated more easily.
[0090] Suitably, the area ratio of the overlapping area A of the upper and lower electrodes to the area B of the piezoelectric film 11 exposed in the hollow portion and the lower electrode, i.e., A / B, is less than 1 / 2 or less than 1 / 2. That is, the overlapping area of the electrode 22 as the upper electrode and the electrode 13 as the lower electrode is less than 1 / 2 of the area of the hollow portion 21. In such a case, by applying a voltage between the electrode 22 and the electrode 13, the portion of the piezoelectric film 11 to which the electric field in the thickness direction is applied can be more reliably separated from the substrate 12. Therefore, the portion of the piezoelectric film 11 to which the electric field in the thickness direction is applied can vibrate freely without being constrained by the substrate 12, and bulk acoustic waves can be generated more easily.
[0091] In addition, as described above, the film structure 10 included in the electronic device 20 of the second embodiment can also include the piezoelectric film 11, the electrode 13, and the substrate 12, similarly to the film structure 10 of the first embodiment. Therefore, the film structure 10 included in the electronic device 20 of the second embodiment can also include the Si layer 12a (see FIG. 1 ) as the substrate 12, similarly to the film structure 10 of the first embodiment. Figure 6 ), an SOI substrate as a semiconductor substrate can be used instead of a Si substrate, and the electrode 13 can also replace the Pt layer 13a (refer to Figure 3 ) and includes the Mo layer 13c (refer to Figure 3 ) or W layer 13d (refer to Figure 3 ). In addition, as the material of the electrode 13a, 13c or 13d, in addition to the materials described above, a Ru layer or a Cu layer may also be used. These materials are generally used as electrode materials.
[0092] In addition, in the film structure 10 of the electronic device 20 of the second embodiment, similarly to the film structure 10 of the first embodiment, the piezoelectric film 11 contains c-axis oriented lithium niobate (LiNbO 3 ) or lithium tantalate (LiTaO 3 ), that is, as a main component.
[0093] like Figure 8 As shown, it is preferable to provide a dielectric layer 23 as a dielectric layer or a matching layer between the substrate 12 and the piezoelectric film 11. That is, Figure 8 The electronic device 20 shown in FIG. Figure 7 In addition to the portion included in the electronic device 20 shown, the electronic device 20 further includes a dielectric layer 23 as a matching layer on the substrate 12 and below the lower electrode, that is, below the electrode 13. For example, when the portion other than the dielectric layer 23 in the electronic device 20 is made of a material having a property of becoming soft as the temperature rises, and the dielectric layer 23 is made of a material having a property of becoming hard as the temperature rises, the temperature dependence of the dielectric constant characteristic or the piezoelectric characteristic of the electronic device 20, that is, the temperature characteristic, can be stabilized or adjusted.
[0094] The dielectric layer 23 is preferably a Si compound, such as silicon dioxide (SiO 2 ). In this case, since the dielectric layer 23 is made of a material having high affinity with the manufacturing process of the semiconductor device, the dielectric layer 23 can be easily formed.
[0095] like Fig. 9 As shown in FIG. 1 , it is preferable to provide a dielectric layer 24 as an upper dielectric layer on the piezoelectric film 11. That is, Fig. 9 The electronic device 20 shown in FIG. Figure 7 In addition to the portion of the electronic device 20 shown, a dielectric layer 24 as an upper dielectric layer is provided on the piezoelectric film 11. For example, when the portion of the electronic device 20 other than the dielectric layer 24 is made of a material having a property of becoming soft as the temperature rises, and the dielectric layer 24 is made of a material having a property of becoming hard as the temperature rises, the temperature dependence of the dielectric constant characteristic or the piezoelectric characteristic of the electronic device 20, that is, the temperature characteristic can be stabilized or adjusted.
[0096] The dielectric layer 24 is preferably a Si compound, such as SiO 2 . In this case, since the dielectric layer 24 is made of a material having high affinity with the manufacturing process of the semiconductor device, the dielectric layer 24 can be easily formed.
[0097] In addition, Figures 7 to 9 In the example shown, for example Figure 7 In the example shown, it is possible to make the upper and lower parts of the piezoelectric film 11 unfixed (using the later-described Figures 15 to 17 The same also applies to the described embodiment 3).
[0098] In addition, Figures 7 to 9 In the example shown, for example Figure 8 as well as Fig. 9 In the example shown, the following can be made: one of the piezoelectric films 11 is fixed, and the opposite side is fixed weaker than the one side by a material whose hardness changes with temperature. That is, it is possible to fix either the upper or lower side of the piezoelectric film 11, and the side opposite to the upper or lower side of the piezoelectric film 11 is fixed weaker by a material whose hardness changes with temperature (using the method described later). Figures 15 to 17 The same also applies to the third embodiment described above.) Thus, it is possible to realize an electronic device that can effectively utilize the displacement in the sliding direction and can compensate for the temperature characteristics.
[0099] like Fig.10 As shown, it is preferable to provide a dielectric layer 23 as a lower dielectric layer between the substrate 12 and the piezoelectric film 11, and to provide a dielectric layer 24 as an upper dielectric layer on the piezoelectric film 11. That is, Fig.10 The electronic device 20 shown in FIG. Figure 7 In addition to the parts of the electronic device 20 shown in the figure, it also has: a dielectric layer 23 as a matching layer on the substrate 12 and below the lower electrode, that is, below the electrode 13; and a dielectric layer 24 as an upper dielectric layer on the piezoelectric film 11. Fig.10 In the example shown, the dielectric layer 24 is provided on the upper electrode, that is, the electrode 22. Fig.10 In the example shown, electrodes are also formed on the upper and lower sides in contact with the piezoelectric film 11. For example, when the portion of the electronic device 20 other than the dielectric layer 23 and the dielectric layer 24 is made of a material having a property of becoming soft as the temperature rises, and the dielectric layer 23 and the dielectric layer 24 are made of a material having a property of becoming hard as the temperature rises (a material whose hardness increases with the temperature rise), the temperature dependence of the dielectric constant characteristic or the piezoelectric characteristic of the electronic device 20, that is, the temperature characteristic can be stabilized or adjusted. As described above, the dielectric layer 23 and the dielectric layer 24 are Si compounds, such as SiO2.
[0100] like Fig.11 As shown, it is preferred that a dielectric layer 23 as a lower dielectric layer is provided between the substrate 12 and the piezoelectric film 11, a dielectric layer 24 as an upper dielectric layer is provided on the piezoelectric film 11, and an electrode 22 as an upper electrode is provided on the dielectric layer 24 as the upper dielectric layer. That is, Fig.11 The electronic device 20 shown is in Fig.10 In the electronic device 20 shown, the stacking order of the electrode 22 and the dielectric layer 24 in the vertical direction is reversed. Fig.11 The structure shown is not a structure in which electrodes are formed on the upper and lower sides in contact with the piezoelectric film 11. In such a case, it is also possible to have Fig.10 The same effect is achieved as that of the electronic device 20 shown in the figure. In addition, as mentioned above, the dielectric layer 23 and the dielectric layer 24 are Si compounds, such as SiO2.
[0101] like Fig.12 As shown, it is preferred that either the electrode 13 or the electrode 22 has a plurality of upper or lower portions so as to have two or more electric field directions in the plane. Fig.12 In the example shown, the electronic device 20 has two electrodes 22 as upper electrodes. Fig.12 In FIG. 1 , the two electrodes 22 are shown as the electrode 22a and the electrode 22b. Thus, it is easier to realize an electronic device that effectively utilizes the displacement in the sliding direction. Fig.12 Schematically shows a case where the piezoelectric film 11 has displacements in two sliding directions.
[0102] like Fig.13 As shown, the polarization direction (polarization direction DP1) of the piezoelectric film 11 is preferably oriented perpendicularly to the substrate 12 and in multiple directions, and the electrodes 22 and 13 are provided on the upper and lower parts of the piezoelectric film 11. In this case, it is also easier to realize an electronic device that effectively utilizes displacement in the sliding direction.
[0103] like Fig.14 As shown in FIG. 1 , it is preferred that a plurality of electrodes be provided on the upper or lower portion of the piezoelectric film 11. Fig.14 In the example shown, no lower electrode is provided, and two electrodes 22, namely, electrode 22a and electrode 22b are provided as upper electrodes. In such a case, an electronic device that effectively utilizes displacement in the sliding direction can be realized more easily.
[0104] (Implementation method 3)
[0105] Next, an electronic device according to Embodiment 3 which is one embodiment of the present invention will be described. The electronic device according to Embodiment 3 is a surface acoustic wave (SAW) filter including the film structure according to Embodiment 1. Figures 15 to 17 This is a perspective view of an electronic device according to a third embodiment.
[0106] like Fig.15 As shown, the electronic device 30 of the third embodiment is an electronic device having a film structure 10 including a piezoelectric film 11 , a comb-shaped electrode, and a substrate 12 , wherein the polarization direction of the piezoelectric film 11 is preferentially oriented perpendicular to the substrate 12 .
[0107] The membrane structure 10 included in the electronic device 30 of the third embodiment can also include the piezoelectric film 11 and the substrate 12, similarly to the membrane structure 10 of the first embodiment. Therefore, the description of the parts of the piezoelectric film 11 and the substrate 12 included in the membrane structure 10 that are the same as those of the piezoelectric film 11 and the substrate 12 included in the membrane structure 10 of the first embodiment is sometimes omitted.
[0108] On the other hand, since the electronic device 30 of the third embodiment is a SAW filter having the film structure 10 of the first embodiment, the electrodes 31 and 32 as comb-shaped electrodes (comb-tooth electrodes) are formed on the upper surface or the lower surface of the piezoelectric film 11, i.e., the piezoelectric body portion. That is, the electronic device 30 of the third embodiment includes the electrodes 31 and 32 on the substrate 12 and the piezoelectric film 11. In this case, by applying an AC voltage between the electrodes 31 and 32, the piezoelectric film 11 can easily generate surface acoustic waves. In addition, since the surface acoustic waves having a resonant frequency determined by the elastic characteristics of the substrate 12, the piezoelectric film 11, and the electrodes 31 and 32 can be generated or passed, it can function as a resonator or a filter.
[0109] In the third embodiment, as in the first embodiment, a substrate 12 including a Si layer 12a having a (100) orientation can be used (see Figure 3 ), and a ZrO2 layer 12b formed on the Si layer 12a (refer to Figure 3 ) substrate. The ZrO2 layer 12b suitably includes ZrO2 in a (200) orientation and ZrO2 in a (002) orientation. In this case, the Si layer 12a of the substrate 12 can be regarded as a substrate, and the electronic device 30 of the present embodiment 3 is an electronic device as follows: it has a piezoelectric film 11 on a substrate (Si layer 12a) that is a Si substrate, and the polarization direction of the piezoelectric film 11 is preferentially oriented perpendicular to the substrate 12.
[0110] exist Fig.15 In the example shown, the electrodes 31 and 32 are formed as comb-shaped electrodes on the upper surface of the piezoelectric film 11. Fig.15 In the example shown, the electrodes 31 and 32 are comb-tooth electrodes formed on the upper surface of the piezoelectric film 11. On the other hand, although not shown in the figure, the electrodes 31 and 32 as comb-shaped electrodes may be formed on the lower surface of the piezoelectric film 11. That is, the electrodes 31 and 32 may also be comb-tooth electrodes formed on the lower surface of the piezoelectric film 11.
[0111] Since the polarization direction of the piezoelectric film 11 is preferentially oriented perpendicularly to the substrate 12 , the polarization direction of the piezoelectric film 11 and the direction of the comb-shaped electrodes appropriately intersect with each other and are orthogonal.
[0112] Here, the electrode 31, which is a comb-shaped electrode or a comb-tooth electrode, includes: a main body 31a extending in a direction DR1 in a plan view; and a plurality of comb teeth 31b, which protrude from the main body 31a in a direction DR2 that is appropriately intersecting and orthogonal to the direction DR1 in a plan view, and extend in the direction DR2 in a plan view, and are arranged in the direction DR1. In addition, the electrode 32, which is a comb-shaped electrode or a comb-tooth electrode, includes: a main body 32a extending in a direction DR1 in a plan view; and a plurality of comb teeth 32b, which protrude from the main body 32a in a direction DR2 that is appropriately intersecting and orthogonal to the direction DR1 in a plan view, and extend in the direction DR2 in a plan view, and are arranged in the direction DR1. In addition, the comb teeth 31b and the comb teeth 32b are alternately arranged in the direction DR1. In this case, the direction of the comb-shaped electrode refers to the direction in which the comb teeth 31b and the comb teeth 32b extend, that is, the direction DR2, and the polarization direction DP1 of the piezoelectric film 11 is a direction that appropriately intersects and is orthogonal to the direction in which the comb teeth 31b and the comb teeth 32b extend, that is, the direction DR2.
[0113] In addition, as described above, the film structure 10 included in the electronic device 30 of the third embodiment can also include the piezoelectric film 11 and the substrate 12, similarly to the film structure 10 of the first embodiment. Therefore, the film structure 10 included in the electronic device 30 of the third embodiment can also include the substrate 12 having a structure in which a Si layer and a ZrO2 layer are stacked in this order, similarly to the film structure 10 of the first embodiment, and the Si layer 12a (see Figure 6 ), an SOI substrate as a semiconductor substrate can be used instead of a Si substrate, and the electrode 13 can also replace the Pt layer 13a (refer to Figure 3 ) and includes the Mo layer 13c (refer to Figure 3 ) or W layer 13d (refer to Figure 3 ) In addition, as the material of the electrode 13a, 13c or 13d, in addition to the materials described above, a Ru layer or a Cu layer may also be used.
[0114] In addition, in the film structure 10 of the electronic device 30 of the third embodiment, similarly to the film structure 10 of the first embodiment, the piezoelectric film 11 contains c-axis oriented lithium niobate (LiNbO 3 ) or lithium tantalate (LiTaO 3 ), that is, as a main component.
[0115] like Fig.16 As shown in FIG. 1 , a dielectric layer 33 as a dielectric layer or a matching layer is preferably provided between the substrate 12 and the piezoelectric film 11 . That is, Fig.16 The electronic device 30 shown in FIG. Fig.15In addition to the parts of the electronic device 30 shown, the electronic device 30 further includes a dielectric layer 33 as a matching layer formed on the substrate 12 and below the piezoelectric film 11. Thus, acoustic matching between the substrate 12 and the piezoelectric film 11 can be achieved. In addition, for example, when the parts other than the dielectric layer 33 in the electronic device 30 are composed of a material having a property of becoming soft as the temperature rises, and the dielectric layer 33 is composed of a material having a property of becoming hard as the temperature rises, the temperature dependence of the dielectric constant characteristics or piezoelectric characteristics of the electronic device 30, that is, the temperature characteristics can be stabilized or adjusted.
[0116] The dielectric layer 33 is preferably a Si compound, such as SiO 2 . In this case, since the dielectric layer 33 is made of a material having high affinity with the manufacturing process of the semiconductor device, the dielectric layer 33 can be easily formed.
[0117] like Fig.17 As shown in FIG. 1 , it is preferable to provide a dielectric layer 34 on the piezoelectric film 11. That is, Fig.17 The electronic device 30 shown in FIG. Fig.15 In addition to the portion of the electronic device 30 shown, the electronic device 30 further includes a dielectric layer 34 as a matching layer on the piezoelectric film 11. Thus, acoustic matching between the substrate 12 and the piezoelectric film 11 can be achieved. In addition, for example, when the portion other than the dielectric layer 34 in the electronic device 30 is composed of a material having a property of becoming soft as the temperature rises, and the dielectric layer 34 is composed of a material having a property of becoming hard as the temperature rises, the temperature dependence of the dielectric constant characteristic or the piezoelectric characteristic of the electronic device 30, that is, the temperature characteristic can be stabilized or adjusted.
[0118] The dielectric layer 34 is preferably a Si compound, such as SiO 2 . In this case, since the dielectric layer 34 is made of a material having high affinity with the manufacturing process of the semiconductor device, the dielectric layer 34 can be easily formed.
[0119] Example
[0120] Hereinafter, this embodiment will be described in more detail based on examples. In addition, the present invention is not limited to the following examples.
[0121] (Example 1 to Example 3)
[0122] In the following, the following will be used in Implementation 1 Figures 1 to 6 The film structure 10 described above is formed into the film structure of Examples 1 to 3, and the following test is carried out, that is, a piezoelectric film 11 composed of c-axis oriented LiNbO3 is formed on a Si layer 12a composed of a Si substrate with a ZrO2 layer 12b interposed therebetween. Figure 3As shown, a scheme in which a Pt layer 13a and an SRO layer 13b are formed in sequence from the Si layer 12a side between the ZrO2 layer 12b and the piezoelectric film 11 is set as Example 1. Figure 4 As shown, the scheme in which only the Pt layer 13a is formed between the ZrO2 layer 12b and the piezoelectric film 11 is set as Example 2. Figure 5 As shown in FIG. 1 , a piezoelectric film 11 composed of c-axis oriented LiNbO 3 is directly formed on the ZrO 2 layer 12 b as Example 3.
[0123] [Formation of membrane structure]
[0124] The method for forming the film structure of Example 1 is described. First, as a Si layer 12a composed of a Si (100) substrate (see Figure 3 ) was prepared with a 6-inch silicon single crystal wafer having an upper surface consisting of a (100) plane.
[0125] Next, in the Si layer 12a (see Figure 3 ) is formed on a wafer by electron beam evaporation method. Figure 3 ). The conditions at this time are shown below.
[0126] Device: Electron beam evaporation device
[0127] Pressure: 7.00×10 -5 Pa
[0128] Evaporation source: Zr+O2
[0129] Acceleration voltage / emission current: 7.5kV / 1.80mA
[0130] Thickness: 60nm
[0131] Substrate temperature: 500°C
[0132] Next, on the ZrO2 layer 12b (refer to Figure 3 ) is formed by sputtering a Pt layer 13a (see Figure 3 ). The conditions at this time are shown below.
[0133] Device: DC sputtering device
[0134] Pressure: 1.20×10 -1 Pa
[0135] Evaporation source: Pt
[0136] Power: 100W
[0137] Thickness: 150nm
[0138] Substrate temperature: 450~600℃
[0139] Next, on the Pt layer 13a (refer to Figure 3 ) is formed by sputtering an SRO layer 13b (see Figure 3 ). The conditions at this time are shown below.
[0140] Device: RF magnetron sputtering device
[0141] Power: 300W
[0142] Gas: Ar
[0143] Pressure: 1.8Pa
[0144] Substrate temperature: 600°C
[0145] Thickness: 40nm
[0146] Next, on the SRO layer 13b (refer to Figure 3 ) is formed by sputtering a piezoelectric film 11 composed of LiNbO3 (refer to Figure 3 ). The conditions at this time are shown below.
[0147] Device: AC sputtering device
[0148] Pressure: 2Pa
[0149] Evaporation source (target): LiNbO3
[0150] Gas: Ar / N2
[0151] Power: 1000W
[0152] Substrate temperature: 450°C
[0153] Thickness: 500nm
[0154] On the other hand, in the film structure forming method of Example 2, unlike the film structure forming method of Example 1, the SRO layer 13b is not formed (see Figure 3 ), in the Pt layer 13a (refer to Figure 4 ) is directly formed on the piezoelectric film 11 (refer to Figure 4 ). In addition, in the film structure forming method of Example 3, unlike the film structure forming method of Example 1, the Pt layer 13a and the SRO layer 13b are not formed, and the piezoelectric film 11 is directly formed on the ZrO2 layer 12b.
[0155] [Off-plane measurement 1
[0156] The ω-2θ spectrum (out-of-plane X-ray diffraction pattern) of the XRD method was measured for the film structures of Examples 1 to 3. That is, the film structures of Examples 1 to 3 formed to the piezoelectric film 11 were subjected to X-ray diffraction measurement (out-of-plane measurement) of ω-2θ scanning. The out-of-plane measurement is equivalent to the case where the angle between the measurement plane and the substrate surface is less than 90°. In addition, the XRD data of Examples 1 to 3 were obtained using the X-ray diffraction device SmartLab manufactured by Rigaku Corporation.
[0157] Fig.18 The definition of a c-axis oriented plane is shown. Fig.18 : is a diagram showing the crystal structure of c-axis oriented LiNbO3. As mentioned above, LiNbO3 has an ilmenite structure which is a trigonal crystal structure and is polarized in the c-axis direction. Fig.18 In FIG. 1 , the oblique line portion represents the c-plane, and the c-axis represents the c(001) axis.
[0158] Fig.19 This is a graph showing an example of the ω-2θ spectrum of the film structure of Example 1 by the XRD method. Fig. 20 This is a graph showing an example of the ω-2θ spectrum of the film structure of Example 2 by the XRD method. Fig.21 This is a graph showing an example of the ω-2θ spectrum of the film structure of Example 3 obtained by the XRD method. Figures 19 to 21 The horizontal axis of the graph represents the angle 2θ in the ω-2θ scan, Figures 19 to 21 The vertical axis of the graph represents the intensity of detected X-rays. Figures 19 to 21 The range of 20°≤2θ≤90° is shown.
[0159] exist Fig.19 The example shown (Example 1), Fig. 20 The example shown (Example 2) and Fig.21 In any ω-2θ spectrum of the example (Example 3) shown, in addition to the peak corresponding to the Si (400) plane at around 69°, peaks corresponding to the (006) plane ((0, 0, 6) plane) and the (0012) plane ((0, 0, 12) plane) of LN displayed using the 3-index are observed. Fig.19 The example shown (Example 1) and Fig. 20In the ω-2θ spectrum of the example (Example 2) shown, a peak corresponding to the (200) plane of Pt was observed at about 46°. Therefore, in the film structures of Examples 1 and 2, it was confirmed that the Pt layer 13a was (200) oriented, i.e., (100) oriented, on the Si layer 12a formed of the Si (100) substrate, and a piezoelectric film 11 composed of c-axis oriented LiNbO3 was formed on the Pt layer 13a. In addition, in the film structure of Example 3, it was confirmed that a piezoelectric film 11 composed of c-axis oriented LiNbO3 was formed on the Si layer 12a formed of the Si (100) substrate.
[0160] In addition, Figures 19 to 21 In comparison, Fig. 20 In the ω-2θ spectrum of the example (Example 2) shown, the intensity of the diffraction peak of the (006) plane of LN is the largest at the 3-index.
[0161] In addition, Fig.19 In the ω-2θ spectrum of the example (Example 1) shown, peaks corresponding to the (012) plane ((0, 1, 2) plane), (024) plane ((0, 2, 4) plane), and (036) plane ((0, 3, 6) plane) of LN were observed. Therefore, in the film structure of Example 1, unlike the film structures of Examples 2 and 3, the piezoelectric film 11 contains a component composed of LiNbO3 oriented in the (012) direction in addition to the component composed of LiNbO3 oriented in the c-axis direction.
[0162] [Reciprocal lattice mapping]
[0163] Next, reciprocal lattice mapping was performed on the film structures of Example 1 and Example 2. The reciprocal lattice mapping is to observe the measured film three-dimensionally to confirm the fluctuation of the lattice constant and the inclination of the lattice plane.
[0164] Fig. 22 is a graph showing the results of reciprocal lattice mapping of the film structure of Example 1. Fig.23 : is a graph showing the results of the reciprocal lattice spectrum measurement of the film structure of Example 2. Fig. 22 as well as Fig.23 In each of the figures, the left half shows the result of the reciprocal lattice spectrum measurement, and the right half shows an image obtained by overlapping the simulation result and the reciprocal lattice spectrum measurement result. Fig. 22 as well as Fig.23 ,exist Fig.23 The figure shows multiple reciprocal lattice points representing the Si(400) plane, ZrO2(200) plane, Pt(200) plane and Pt(400) plane, respectively, and LN(006) plane and LN(0012) plane respectively using a 3-index display.
[0165] exist Fig. 22 The example shown (Example 1) and Fig.23 In any of the examples shown (Example 2), the six reciprocal lattice points representing the ZrO2(200) plane, the LN(006) plane indicated by the 3-index, the Pt(200) plane, the Si(400) plane, the LN(0012) plane indicated by the 3-index, and the Pt(400) plane are confirmed to be in a vertical row, and the planes are aligned. That is, in any of the X-ray reciprocal lattice space mappings of the membrane structures of Example 1 and Example 2, the six reciprocal lattice points representing the ZrO2(200) plane, the LN(006) plane indicated by the 3-index, the Pt(200) plane, the Si(400) plane, the LN(0012) plane indicated by the 3-index, and the Pt(400) plane are arranged in the Qz direction. In addition, in Fig.23 In the example shown (Example 2), the reciprocal lattice points are clear, so Fig. 22 Compared with the example shown (Example 1), it can be said that the fluctuation is also small. Although not shown in the figure, the same result was obtained for the membrane structure of Example 3.
[0166] According to the above results, in any of the film structures of Examples 1 to 3, LiNbO3 is c-axis oriented and epitaxially grown on the Si layer 12a formed by the Si (100) substrate. In addition, there is no crystal fluctuation in LiNbO3, and the lattice planes are also aligned. In other words, it can be seen that LiNbO3 formed on SRO (100) / Pt (100) / ZrO2 / Si (100), Pt (100) / ZrO2 / Si (100), and ZrO2 / Si (100) is c-axis oriented and is approximately single crystal.
[0167] [Inner channel determination]
[0168] Next, the XRD characteristics of the film structures of Example 1 and Example 2 were measured. Scanning spectrum (inner channel X-ray diffraction pattern). That is, the film structures of Example 1 and Example 2 formed to the piezoelectric film 11 were subjected to Scanning X-ray diffraction measurement (inner channel measurement) Inner channel measurement corresponds to the case where the angle between the measurement plane and the substrate surface is equal to 90°.
[0169] Fig.24 The XRD results of the film structure of Example 1 are shown. A graph of an example of a scan spectrum, Fig.25 The XRD results of the film structure of Example 2 are shown. Graph of an example of a scan spectrum. Fig.24 as well as Fig.25 The horizontal axis of the chart represents Angle in scanning Fig.24 as well as Fig.25 The vertical axis of the graph represents the intensity of the detected X-rays. Fig.24 as well as Fig.25 Shows range.
[0170] exist Fig.24 as well as Fig.25 In the example shown, the measurement was performed in a state where the angle between the measurement plane and the substrate surface was adjusted to be about 90° (inner channel measurement) and 2θ was equal to the angle (62.4°) corresponding to the diffraction peak of the LN (300) plane displayed with a 3-index. scanning.
[0171] exist Fig.24 The example shown (Example 1) and Fig.25 Any of the examples shown (Example 2) During scanning, it was observed that The 12 diffraction peaks of the LN (300) plane are arranged at intervals of 30° in the direction (horizontal axis direction) and are respectively represented by 3 indices. Therefore, in the film structures of Examples 1 and 2, it is clear that LiNbO3 has 12-fold symmetry as the symmetry of the apparent crystal structure. In addition, although the illustration is omitted, the same result is obtained for the film structure of Example 3.
[0172] Therefore, according to Scanning spectra, as well as reciprocal lattice spectra, clearly show that LiNbO3 is epitaxially grown on the Si layer 12a formed on the Si (100) substrate in the film structures of Examples 1 to 3. Fig.18 As shown, the crystal structure of LiNbO3 has three-fold symmetry around the c-axis. Therefore, it is considered that the piezoelectric film 11 included in the film structures of Examples 1 to 3 is composed of a plurality of different domains (rotation components) that rotate with each other in the LN (006) plane.
[0173] Fig.26 The rotation angle of the rotation component and the symmetry of the crystal structure composed of hexagonal and trigonal crystals are shown. This table is a table that classifies and organizes the apparent symmetry of the crystal structure determined by the number of diffraction peaks observed in the scanning spectrum. Fig.26In the figure, the domain (rotation component) that serves as the reference is recorded as "0° rotation component", and the domains (rotation components) that are rotated 180°, 90°, and 270° from the reference domain are marked as "180° rotation component", "90° rotation component", and "270° rotation component".
[0174] like Fig.26 As shown, in a crystal structure composed of trigonal crystals, the case of having 12-fold symmetry is the case of having a domain (rotation component) obtained by rotating 90° from a domain serving as a reference, or the case of having a domain (rotation component) obtained by rotating 270° from a domain serving as a reference. In addition, in a crystal structure composed of trigonal crystals, the case of having a domain (rotation component) obtained by rotating 270° from a domain serving as a reference is the same as the case of having a domain (rotation component) obtained by rotating 90° from a domain serving as a reference. Therefore, according to Fig.24 as well as Fig.25 shown From the scanning spectra, it is considered that the film structures of Examples 1 to 3 have four domains (rotation components) consisting of a reference domain and three domains rotated from the reference domain by 90°, 180°, and 270°, respectively.
[0175] Here, the four different rotation components of the piezoelectric film 11 are referred to as the portion DM1 to the portion DM4. It is considered that due to the existence of the portion DM1 to the portion DM4, Fig.24 as well as Fig.25 shown During scanning, four groups of three diffraction peaks each having a 3-fold symmetry overlapped each other by 90°, thereby observing 12 diffraction peaks having a 12-fold symmetry. Fig.26 As shown, the portion DM1 can be set to a 0° rotation component, the portion DM2 can be set to a 90° rotation component, the portion DM3 can be set to a 180° rotation component, and the portion DM4 can be set to a 270° rotation component.
[0176] The above results are summarized as follows. Assume that the Si substrate as the Si layer 12a is a Si(100) substrate, or the SOI layer as the Si layer 12a is composed of a Si(100) film, and the piezoelectric film 11 is an LN film composed of c-axis oriented LiNbO3. In this case, the LN film preferably has epitaxially grown portions DM1 to DM4, portion DM2 is rotated 90° clockwise with respect to portion DM1 around the c-axis, portion DM3 is rotated 180° clockwise with respect to portion DM1 around the c-axis, and portion DM4 is rotated 270° clockwise with respect to portion DM1 around the c-axis.
[0177] [Voltage dependence of polarization]
[0178] In the film structure of Example 2, the piezoelectric film 11 (see Figure 4 ) is formed on an upper electrode made of Pt, and on electrode 13 (refer to Figure 4 ) is applied between the upper electrode and the voltage dependence of polarization (polarization voltage hysteresis curve) is measured. Fig. 27 : is a graph showing the voltage dependency of polarization of the film structure of Example 2. The polarization value when the voltage applied to the piezoelectric film 11 is increased from 0 to the positive side and then returned to 0 is the residual polarization value of the piezoelectric film 11 .
[0179] like Fig. 27 As shown in the graph showing the voltage dependence of polarization of the film structure of Example 2, a polarization voltage hysteresis curve showing the ferroelectricity of the piezoelectric film 11 is shown. In the polarization voltage hysteresis curve, the piezoelectric film 11 has a 70 μC / cm 2 In the initial state, the piezoelectric film 11 also has a residual polarization of -70 μC / cm 2 Therefore, when the film structure of Example 2 is used as a piezoelectric element, it is not necessary to apply polarization treatment to the piezoelectric film 11 before use. In addition, although the illustration is omitted, substantially the same results are obtained in the film structures of Example 1 and Example 3. Therefore, in the film structures of Example 1 to Example 3, it is shown that the piezoelectric film 11 has good strong dielectric properties. In addition, since the piezoelectric film 11 has strong dielectric properties and has a polarization effect, it can also be effectively used in a memory.
[0180] As mentioned above, the invention completed by the present inventors has been specifically described based on the embodiment, but the present invention is not limited to the above embodiment, and various modifications can be made without departing from the gist of the invention.
[0181] It should be understood that within the scope of the concept of the present invention, a person skilled in the art can conceive of various changes and modifications, and these changes and modifications also fall within the scope of the present invention.
[0182] For example, solutions obtained by those skilled in the art by appropriately adding, deleting or changing the design of structural elements, or by adding, omitting or changing the conditions of the above-mentioned embodiments are also included in the scope of the present invention as long as they have the gist of the present invention.
[0183] -Explanation of symbols-
[0184] 10Membrane structure
[0185] 11Piezoelectric film
[0186] 12 substrates
[0187] 12a Si layer
[0188] 12b ZrO2 layer
[0189] 12c matrix
[0190] 12d BOX layer
[0191] Electrodes 13, 22, 22a, 22b, 31, 32
[0192] 13a Pt layer
[0193] 13b SRO layer
[0194] 13c Mo layer
[0195] 13d W layer
[0196] 20, 30 Electronic devices
[0197] 21 Hollow
[0198] 23, 24, 33, 34 dielectric layer
[0199] 31a, 32a main body
[0200] 31b, 32b comb teeth
[0201] DM1~DM4
[0202] DP1 polarization direction
[0203] DR1, DR2 directions.
Claims
1. A membrane structure, characterized in that: have: substrate; a buffer film formed on the substrate; and a piezoelectric film formed on the buffer film, The substrate is a Si (100) substrate or an SOI substrate, wherein the SOI substrate comprises a base body composed of a Si substrate, an insulating layer on the base body, and an SOI layer composed of a Si (100) film on the insulating layer. The buffer film comprises ZrO2, The piezoelectric film includes c-axis oriented LiNbO 3 or LiTaO 3.
2. The membrane structure according to claim 1, wherein: The film structure includes a metal film formed between the buffer film and the piezoelectric film.
3. The membrane structure according to claim 2, wherein: The metal film includes (100)-oriented Pt.
4. The membrane structure according to claim 2, wherein: The metal film is a Pt film, a Mo film, a W film, a Ru film or a Cu film.
5. The membrane structure according to claim 3, wherein: The film structure has a SrRuO3 film formed between the metal film and the piezoelectric film. The SrRuO 3 film has a cubic crystal structure and a (100) orientation.
6. An electronic device, characterized in that: A membrane structure according to any one of claims 1 to 5.
7. An electronic device, characterized in that: A membrane structure according to claim 1, The film structure has a comb-tooth electrode formed on an upper surface or a lower surface of the piezoelectric film.
8. The electronic device according to claim 7, wherein: The film structure includes a matching layer formed on the substrate.
9. The electronic device according to claim 6, wherein: A hollow portion is provided at a lower portion of the piezoelectric film.
10. The electronic device according to claim 9, wherein: The film structure includes an upper electrode formed on an upper portion of the piezoelectric film and a lower electrode formed on a lower portion of the piezoelectric film.
11. The electronic device according to claim 10, wherein: An area of an overlapping portion of the upper electrode and the lower electrode is smaller than an area of the hollow portion.
12. The electronic device according to claim 10, wherein: An area of an overlapping portion between the upper electrode and the lower electrode is equal to or less than 1 / 2 of an area of the hollow portion.
13. The electronic device according to claim 9, wherein: The film structure includes a matching layer formed on the substrate.
14. The electronic device according to claim 8, wherein: The matching layer is composed of a material whose hardness increases with increasing temperature.
15. The electronic device according to claim 14, wherein: The material is a Si compound.
Citation Information
Cited By
Lithium niobate film MEMS traveling wave motor design structure and preparation method
CN121508360A
A lithium niobate thin film MEMS traveling wave motor design structure and a preparation method thereof
CN121508360B