Composite film as well as preparation method and application thereof

By using a composite film composed of graphene oxide and polyaniline fibers in water purification, a Janus structure is formed to improve the efficiency of photothermal water evaporation, and the problem of insufficient purification effect of existing photothermal conversion materials in water bodies is solved, achieving high efficiency and environmental protection water purification effect.

CN119015898APending Publication Date: 2024-11-26XINJIANG AGRI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411154361.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing photothermal conversion materials have insufficient water purification effect, especially the poor purification effect of sewage, and the high-energy-consuming water desalination technology seems to be ineffective when energy problems are highlighted, especially in underdeveloped areas.

Method used

The composite film arranged in a laminated manner includes a porous graphene oxide film as a water transport layer and a photothermal conversion layer composed of graphene oxide and polyaniline fibers. The combination formed by positive and negative charge changes the binding force during solvent evaporation. Form a Turing structure, improve surface roughness, and form a Janus structure to block pollutants and improve photothermal water evaporation efficiency.

Benefits of technology

It has achieved excellent purification effects on heavy metals, simulated seawater and organic wastewater, with removal rates reaching 99.6%, 99.3% and 100%. The materials are environmentally friendly and low-cost, comply with WHO drinking water standards, and are suitable for photothermal evaporation purification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015898A_ABST
    Figure CN119015898A_ABST
Patent Text Reader

Abstract

The invention provides a composite film as well as a preparation method and application thereof, and belongs to the technical field of water purification. Hydrophilic polyaniline fibers are introduced into the photothermal conversion layer, the polyaniline fibers and graphene oxide are combined together in a solvent under the action of positive and negative charges, and the formed combination body can obtain a Turing structure similar to a dry crack ground due to the change of the binding force between the polyaniline fibers and the graphene oxide in the solvent evaporation process; the surface roughness of the composite film is improved through patterning of the surface Turing structure, so that a hydrophobic surface is obtained, a Janus structure is formed by the hydrophobic surface and the hydrophilic porous water transmission layer, the composite film can block pollutants from passing through in the water evaporation process, and the composite film has excellent water purification performance; the rough structure on the surface of the composite film can enhance the light absorption function, so that the light-hot water evaporation efficiency is improved, and the water purification effect is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water purification, and in particular relates to a composite film and a preparation method and application thereof. Background Art

[0002] Traditional water desalination technologies such as membrane filtration and thermal distillation have been industrialized, which has alleviated the problem of fresh water shortage to a certain extent. However, there are still problems such as high energy consumption and high cost. Moreover, as energy problems become more prominent, high-energy-consuming water resource desalination technology has become increasingly insufficient, especially in underdeveloped areas.

[0003] Light-driven interfacial evaporation is a low-carbon way to solve the shortage of freshwater resources. Its development will also help promote the progress of water desalination and purification, and the performance of photothermal conversion materials is an important factor affecting the performance of interfacial evaporation. Current photothermal conversion materials include carbon black, carbon nanotubes, nanogold particles or graphene, which can be used for efficient solar water evaporation for sewage purification, but their water purification effect is poor. Therefore, how to improve the water purification effect of photothermal conversion materials has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0004] The purpose of the present invention is to provide a composite film and a preparation method and application thereof. The composite film provided by the present invention has an excellent pollutant removal rate.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a composite film, comprising a water transmission layer and a light-to-heat conversion layer stacked in layers;

[0007] The water transport layer is a porous graphene oxide membrane;

[0008] The components of the light-to-heat conversion layer include graphene oxide and polyaniline fibers.

[0009] Preferably, the composite film has a thickness of 30 to 52 μm.

[0010] Preferably, the thickness of the water transfer layer is 7-12 μm, and the thickness of the light-to-heat conversion layer is 23-40 μm.

[0011] Preferably, the diameter of the polyaniline fiber is 150-300 nm, and the length of the polyaniline fiber is 0.5-5 μm.

[0012] Preferably, the mass ratio of graphene oxide to polyaniline fibers in the light-to-heat conversion layer is (2-4):(6-15).

[0013] Preferably, the mass ratio of graphene oxide to polyaniline fiber in the light-to-heat conversion layer is 3:(9-12).

[0014] The present invention also provides a method for preparing the composite film described in the above technical solution, comprising the following steps:

[0015] (1) mixing a first graphene oxide solution with a pore-forming agent, and then filtering to obtain a graphene oxide film;

[0016] (2) mixing the second graphene oxide solution with the polyaniline fiber, and then filtering on the graphene oxide membrane obtained in step (1) to obtain a composite membrane;

[0017] (3) Immersing the composite film obtained in step (2) in toluene to obtain a composite film.

[0018] Preferably, the pore-forming agent in step (1) is polystyrene microspheres.

[0019] Preferably, the mass ratio of graphene oxide to pore former in the first graphene oxide solution is (12-48): (1-6).

[0020] The present invention also provides the use of the composite film described in the above technical solution or the composite film prepared by the preparation method described in the above technical solution in water purification.

[0021] The present invention provides a composite film, comprising a water transmission layer and a photothermal conversion layer arranged in layers; the water transmission layer is a porous graphene oxide film; the components of the photothermal conversion layer include graphene oxide and polyaniline fibers. The present invention introduces hydrophilic polyaniline fibers into the photothermal conversion layer, and the polyaniline fibers and graphene oxide are combined together in the solvent through the action of positive and negative charges. The formed combination will obtain a Turing structure similar to a dry cracked ground due to the change in the binding force between them during the evaporation of the solvent. The patterning of the surface Turing structure improves the surface roughness of the composite film, thereby obtaining a hydrophobic surface, and forms a Janus structure with the hydrophilic porous water transmission layer, so that the composite film can block the passage of pollutants during the water evaporation process, so that it has excellent water purification performance; the rough structure on the surface of the composite film can enhance its light absorption function, thereby improving the light and water evaporation efficiency, thereby further improving the water purification effect. Experimental results show that the composite film provided by the present invention has a purification effect of 99.6% on heavy metals, 99.3% on simulated seawater, and 100% on organic wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a macroscopic image of the composite film prepared in Example 1;

[0023] Figure 2 This is a SEM image of the surface of the light-to-heat conversion layer in the composite film prepared in Example 1;

[0024] Figure 3 This is a cross-sectional SEM image of the composite film prepared in Example 1;

[0025] Figure 4 This is a profilometer image of the light-to-heat conversion layer in the composite film prepared in Example 1;

[0026] Figure 5 This is a contact angle test diagram of the light-to-heat conversion layer in the composite film prepared in Example 1;

[0027] Figure 6 This is a test diagram of the contact angle of the water transport layer in the composite film prepared in Example 1;

[0028] Figure 7 This is a schematic diagram of the structure of the composite film prepared in Example 1 for purifying water through photothermal water evaporation;

[0029] Figure 8 The photos of the first day of the experiment of using saline-alkali soil soaking solution, simulated seawater solution and heavy metal solution for alfalfa seed germination before and after purification;

[0030] Fig. 9 Photos of the saline-alkali soil soaking solution, simulated seawater solution and heavy metal solution before and after purification on the 7th day of the alfalfa seed germination experiment. DETAILED DESCRIPTION

[0031] The present invention provides a composite film, comprising a water transmission layer and a light-to-heat conversion layer stacked in layers;

[0032] The water transport layer is a porous graphene oxide membrane;

[0033] The components of the light-to-heat conversion layer include graphene oxide and polyaniline fibers.

[0034] The composite film provided by the present invention includes a water transport layer. In the present invention, during the photothermal water evaporation process, the water transport layer can allow water to pass through the channels formed by the sheet structure and porous structure of graphene oxide, while preventing salt, heavy metals, organic pollutants, etc. from passing through.

[0035] In the present invention, the thickness of the water transport layer is preferably 7 to 12 μm, more preferably 8 to 10 μm. In the present invention, limiting the thickness of the water transport layer to the above range can further improve the effect of water purification.

[0036] In the present invention, the water transport layer is a porous graphene oxide membrane.

[0037] The composite film provided by the present invention further comprises a light-to-heat conversion layer. In the present invention, the light-to-heat conversion layer converts light energy into heat energy, thereby evaporating the water transmitted by the water transmission layer.

[0038] In the present invention, the thickness of the light-to-heat conversion layer is preferably 23-40 μm, more preferably 35-40 μm. In the present invention, limiting the thickness of the light-to-heat conversion layer to the above range can further improve the effect of water purification.

[0039] In the present invention, the components of the photothermal conversion layer include graphene oxide and polyaniline fibers. The present invention introduces hydrophilic polyaniline fibers into the photothermal conversion layer, and the polyaniline fibers and graphene oxide are combined together in the solvent through the action of positive and negative charges. The formed combination will obtain a Turing structure similar to a dry cracked ground due to the change in the binding force between them during the solvent evaporation process. The patterning of the surface Turing structure improves the surface roughness of the composite film, thereby obtaining a hydrophobic surface, and forms a Janus structure with the hydrophilic porous water transport layer, so that the composite film can block the passage of pollutants during the water evaporation process, so that it has excellent water purification performance; the rough structure on the surface of the composite film can enhance its light absorption function, thereby improving the light and water water evaporation efficiency, thereby further improving the water purification effect.

[0040] In the present invention, the diameter of the polyaniline fiber is preferably 150-300 nm; the length of the polyaniline fiber is preferably 0.5-5 μm. The present invention limits the size parameters of the polyaniline fiber to the above range, which can improve the surface roughness of the composite film, thereby further improving its light absorption function, thereby improving the light-heat water evaporation efficiency, and further improving the water purification effect.

[0041] In the present invention, the mass ratio of graphene oxide to polyaniline fiber in the light-to-heat conversion layer is preferably (2-4): (6-15), more preferably 3: (9-12), and more preferably 3: 9. In the present invention, limiting the mass ratio of graphene oxide to polyaniline fiber to the above range can further improve the water purification effect.

[0042] In the present invention, the thickness of the composite film is preferably 30 to 52 μm, more preferably 40 to 50 μm. The present invention limits the thickness of the composite film to the above range to further improve the effect of water purification.

[0043] In the process of photothermal water evaporation of the composite film provided by the present invention, the water transmission layer can allow water to pass through due to the channels formed by the sheet structure and porous structure of graphene, while preventing salt, heavy metals, organic pollutants, etc. from passing through; the photothermal conversion layer converts light energy into heat energy, and then evaporates the water transmitted by the water transmission layer, and finally the water is recovered through evaporation-condensation, while the pollutants are blocked in the original solution, thereby achieving purification.

[0044] The composite film provided by the present invention obtains a Janus structure composite film only by effectively regulating the surface roughness structure without using low surface energy materials; the material used in the present invention is simple to prepare and has environmentally friendly components, and will not cause secondary pollution to the environment. During use, effective water evaporation and water purification can be carried out only by light irradiation, and it is a low-carbon, economical and environmentally friendly new material; the composite film can be used for photothermal evaporation purification of organic and inorganic wastewater, and the purified water body meets the relevant WHO drinking water standards, and the purified water body can be used for alfalfa seed germination, which shows that the purification process is efficient and biosafe.

[0045] The composite film provided by the present invention is mainly composed of a graphene oxide film, and polyaniline fibers with low light absorption are introduced. Two hydrophilic substances are used to improve the surface roughness to improve the photothermal performance of the material and obtain a Janus structure. By adding an appropriate amount of polyaniline fibers, the light absorption performance of the material can be improved, and the water evaporation performance can be improved. At the same time, the composite film exhibits excellent continuous use, cyclic practicality and anti-pollution ability, which provides a new idea for the preparation of Janus-type photothermal evaporation functional materials and photothermal water body purification.

[0046] The present invention also provides a method for preparing the composite film described in the above technical solution, comprising the following steps:

[0047] (1) mixing a first graphene oxide solution with a pore-forming agent, and then filtering to obtain a graphene oxide film;

[0048] (2) mixing the second graphene oxide solution with the polyaniline fiber, and then filtering on the graphene oxide membrane obtained in step (1) to obtain a composite membrane;

[0049] (3) Immersing the composite film obtained in step (2) in toluene to obtain a composite film.

[0050] The present invention has no particular limitation on the sources of the raw materials, and commercially available products known to those skilled in the art may be used.

[0051] In the present invention, the first and the second have no special meanings and are only used to distinguish the raw materials.

[0052] The present invention mixes a first graphene oxide solution with a pore-forming agent, and then performs suction filtration to obtain a graphene oxide membrane.

[0053] In the present invention, the concentration of the first graphene oxide solution is preferably 2-4 mg / mL; the solvent of the first graphene oxide solution is preferably an inorganic solvent, more preferably water. The present invention has no particular limitation on the size of the graphene oxide, as long as it can be uniformly dispersed in water to form a stable dispersion.

[0054] In the present invention, the pore former is preferably polystyrene microspheres; the particle size of the polystyrene microspheres is preferably 0.1 to 1 μm, more preferably 0.1 μm, 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm and 1.0 μm. The use of polystyrene microspheres of different particle sizes in the present invention facilitates the pore construction of the water transport layer, forming pores and pores of different sizes.

[0055] In the present invention, the mass ratio of the polystyrene microspheres with particle sizes of 0.1 μm, 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm and 1.0 μm is preferably 1:1:1:1:1:1:1.

[0056] In the present invention, the mass ratio of graphene oxide to pore former in the first graphene oxide solution is preferably (12-48): (1-6), and more preferably (27-35): (1-3). The present invention can regulate the pore structure of the water transport layer by limiting the mass ratio of graphene oxide to pore former in the first graphene oxide solution to the above range, thereby further improving the water purification effect.

[0057] The present invention has no special limitation on the mixing of the first graphene oxide solution and the pore-forming agent, and a technical scheme for preparing a mixed material well known to those skilled in the art may be adopted.

[0058] In the present invention, the filtration is preferably performed using a 0.22 μm cellulose filter membrane. The present invention has no particular limitation on the specific operation of the filtration, and the operation well known to those skilled in the art can be used.

[0059] In the present invention, the filtration is preferably carried out using a 0.5L or 1L liquid mobile phase filtration device; the vacuum degree of the filtration is preferably -0.07 to -0.09 MPa.

[0060] After obtaining the graphene oxide membrane, the present invention mixes the second graphene oxide solution with the polyaniline fiber, and then performs suction filtration on the graphene oxide membrane to obtain a composite membrane.

[0061] In the present invention, the concentration of the second graphene oxide solution is preferably 2-4 mg / mL; the solvent of the second graphene oxide solution is preferably water, ethanol or an aqueous solution of ethanol; the volume ratio of ethanol to water in the aqueous solution of ethanol is preferably (3-7): (7-3), more preferably 5: 5. The present invention has no particular limitation on the size of the graphene oxide, as long as it can be uniformly dispersed in the solvent to form a stable dispersion.

[0062] In the present invention, the mass ratio of graphene oxide to polyaniline fiber in the second graphene oxide solution is preferably (2-4): (6-15), more preferably 3: (9-12), and more preferably 3: 9. In the present invention, limiting the mass ratio of graphene oxide to polyaniline fiber to the above range can further improve the water purification effect.

[0063] The present invention has no special limitation on the operation of mixing the second graphene oxide solution with the polyaniline fiber, and a technical solution for preparing a mixed material well known to those skilled in the art may be used.

[0064] In the present invention, the filtration is preferably performed using a 0.22 μm cellulose filter membrane. The present invention has no particular limitation on the specific operation of the filtration, and the operation well known to those skilled in the art can be used.

[0065] In the present invention, the filtration is preferably carried out using a 0.5L or 1L liquid mobile phase filtration device; the vacuum degree of the filtration is preferably -0.07 to -0.09 MPa.

[0066] After the filtration is completed, the present invention preferably dries the product obtained by filtration and removes the filter membrane in sequence to obtain a composite membrane. The present invention can remove the solvent in the composite membrane by drying after filtration.

[0067] In the present invention, the drying temperature is preferably 20-25° C., more preferably 22° C., and the drying humidity is preferably 20%. The present invention has no particular limitation on the drying time, and the composite film can be dried to a constant weight.

[0068] The present invention has no particular limitation on the operation of separating the filter membrane, and any operation well known to those skilled in the art may be used.

[0069] After obtaining the composite film, the present invention soaks the composite film in toluene to obtain a composite film. The present invention soaks the composite film in toluene to remove polystyrene microspheres in the composite film, thereby obtaining porous graphene oxide.

[0070] The present invention has no particular limitation on the operation of immersing the composite membrane in toluene, and the operation well known to those skilled in the art may be adopted.

[0071] After being immersed in toluene, the composite film is preferably fished out first and then dried to obtain a composite film.

[0072] The present invention has no special limitation on the operation of fishing out the composite membrane and then drying it, and the operation well known to those skilled in the art can be adopted.

[0073] The development of traditional roughness construction methods is usually restricted by factors such as cumbersome operation and high cost. The present invention prepares a composite film by a simple double filtration-evaporation drying method. This preparation method can prepare a composite film with a Janus structure simply, at low cost and safely, improve the surface roughness of the photothermal conversion material, and then improve the photothermal water purification performance, which is used for efficient photothermal water evaporation and water purification.

[0074] The present invention also provides the use of the composite film described in the above technical solution or the composite film prepared by the preparation method described in the above technical solution in water purification.

[0075] In the present invention, the water purification includes salt water, organic wastewater or heavy metal wastewater. The present invention has no special limitation on the source, composition and concentration of the salt water, organic wastewater and heavy metal wastewater, and any substance that needs water purification known to those skilled in the art can be used.

[0076] In the present invention, the light intensity of the composite film when purifying water is preferably 500 to 2000 W / m 2 , more preferably 1000 to 1500 W / m 2 .

[0077] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0078] The graphene oxides used in the examples are all produced by Suzhou Hengqiu Graphene Technology Co., Ltd.

[0079] Example 1

[0080] The composite film is composed of a water transmission layer and a light-to-heat conversion layer arranged in layers;

[0081] The water transport layer is a porous graphene oxide membrane with a thickness of 10 μm;

[0082] The light-to-heat conversion layer is composed of graphene oxide and polyaniline fibers, and has a thickness of 40 μm;

[0083] The polyaniline fiber has a diameter of 150 to 300 nm and a length of 0.5 to 5 μm;

[0084] The mass ratio of graphene oxide to polyaniline fiber in the light-to-heat conversion layer is 1:3;

[0085] The thickness of the composite film is 50 μm;

[0086] The preparation method of the composite film comprises the following steps:

[0087] (1) 9 mL of a 3 mg / mL graphene oxide aqueous solution was mixed with 3 mg of polystyrene microspheres and filtered through a 0.22 μm cellulose filter membrane to obtain a graphene oxide membrane; wherein the particle sizes of the polystyrene microspheres were 0.1 μm, 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm and 1.0 μm, and the mass ratio of the polystyrene microspheres of each particle size was 1:1:1:1:1:1; the mass ratio of graphene oxide to polystyrene microspheres was 27:3; a 0.5 L liquid mobile phase filtration device was used for filtration, and the vacuum degree was -0.09 MPa;

[0088] (2) stirring and mixing 1 mL of a 3 mg / mL aqueous solution of graphene oxide and polyaniline fibers, filtering the mixture through a 0.22 μm cellulose filter membrane on the graphene oxide membrane obtained in step (1), and then placing the mixture in a dry environment for evaporation and drying, and then removing the filter membrane to obtain a composite membrane; wherein the mass ratio of graphene oxide to polyaniline fibers is 1:3; a 0.5 L liquid mobile phase filtration device is used for filtration, and the vacuum degree is -0.09 MPa; the drying humidity is 20%, and the temperature is 22° C.;

[0089] (3) The composite film obtained in step (2) is immersed in toluene to remove the polystyrene microspheres, and then the composite film is taken out and the solvent is evaporated to obtain a composite film with a Janus structure.

[0090] The composite film prepared in Example 1 was observed macroscopically and microscopically. Figures 1 to 3 As shown, Figure 1 This is a macroscopic image of the composite film prepared in Example 1; Figure 2 This is a SEM image of the surface of the light-to-heat conversion layer in the composite film prepared in Example 1; Figure 3 This is a cross-sectional SEM image of the composite film prepared in Example 1.

[0091] from Figures 1 to 3 It can be seen that the surface of the light-to-heat conversion layer in the composite film is rough, and a rough dry-cracked Turing structure is visible.

[0092] The light-to-heat conversion layer in the composite film prepared in Example 1 was characterized by a profilometer. The results are as follows: Figure 4 As shown, Figure 4 This is a profilometer image of the light-to-heat conversion layer in the composite film prepared in Example 1.

[0093] from Figure 4 It can be seen that the surface of the composite film presents many protruding structures, which help to improve the surface roughness of the material. The surface roughness of the composite film is as high as 21.75μm.

[0094] The contact angle test of the composite film prepared in Example 1 was carried out. The results are as follows: Figure 5 and 6 As shown, Figure 5 This is a contact angle test diagram of the light-to-heat conversion layer in the composite film prepared in Example 1; Figure 6 This is a contact angle test diagram of the water transport layer in the composite film prepared in Example 1.

[0095] from Figure 5 and 6 It can be seen that the water transfer layer is hydrophilic and the light-to-heat conversion layer is hydrophobic, so the structure of the composite film is a Janus structure.

[0096] The composite film prepared in Example 1 was used to purify water by photothermal water evaporation, and the results are shown in Table 1; wherein the test results are as follows: the contaminated solution (blue) was placed in a cup, the PE sponge (gray) was used as a temperature insulation device, the cotton cloth (red) was used as a water-conducting layer, and the composite film (black) was placed on the material, and photothermal water evaporation purification was performed under simulated sunlight. The structural schematic diagram is shown in Figure 7 As shown; the pollutant concentration in the solution before and after purification is tested by ICP-OES, TOC, HPLC, UV spectrophotometer, etc., and the removal rate is calculated according to formula I:

[0097] Pollutant removal rate % = 100*(concentration before removal - concentration after removal) / original concentration (Formula I).

[0098] Table 1 Water purification data of the composite film prepared in Example 1

[0099]

[0100] It can be seen from Table 1 that the composite film prepared by the present invention has excellent water purification effect.

[0101] The saline-alkali soil soaking solution, simulated seawater solution and heavy metal solution before and after purification in Table 1 were used in the alfalfa seed germination experiment. The photos of the saline-alkali soil soaking solution, simulated seawater solution and heavy metal solution before and after purification for the alfalfa seed germination experiment on the first day are shown in the figure. Figure 8 As shown, the photos on the 7th day are as follows Fig. 9 shown.

[0102] from Figure 8 and 9 It can be seen that before purification, the water body cannot cause seeds to germinate due to the high concentration of pollutants, but after purification, the water body can cause seeds to germinate normally. Therefore, the water body after purification is biologically safe.

[0103] Example 2

[0104] The composite film is composed of a water transmission layer and a light-to-heat conversion layer arranged in layers;

[0105] The water transport layer is a porous graphene oxide membrane with a thickness of 7 μm;

[0106] The light-to-heat conversion layer is composed of graphene oxide and polyaniline fibers, and has a thickness of 40 μm;

[0107] The polyaniline fiber has a diameter of 150 to 300 nm and a length of 0.5 to 5 μm;

[0108] The mass ratio of graphene oxide to polyaniline fiber in the light-to-heat conversion layer is 1:3;

[0109] The thickness of the composite film is 47 μm;

[0110] The preparation method of the composite film comprises the following steps:

[0111] (1) 6 mL of a 3 mg / mL graphene oxide aqueous solution was mixed with 3 mg of polystyrene microspheres and filtered through a 0.22 μm cellulose filter membrane to obtain a graphene oxide membrane; wherein the particle sizes of the polystyrene microspheres were 0.1 μm, 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm and 1.0 μm, and the mass ratio of the polystyrene microspheres of each particle size was 1:1:1:1:1:1; the mass ratio of graphene oxide to polystyrene microspheres was 18:3; a 0.5 L liquid mobile phase filtration device was used for filtration, and the vacuum degree was -0.09 MPa;

[0112] (2) stirring and mixing 1 mL of a 3 mg / mL aqueous solution of graphene oxide and polyaniline fibers, filtering the mixture through a 0.22 μm cellulose filter membrane on the graphene oxide membrane obtained in step (1), and then placing the mixture in a dry environment for evaporation and drying, and then removing the filter membrane to obtain a composite membrane; wherein the mass ratio of graphene oxide to polyaniline fibers is 1:3; a 0.5 L liquid mobile phase filtration device is used for filtration, and the vacuum degree is -0.09 MPa; the drying humidity is 20%, and the temperature is 23° C.;

[0113] (3) The composite film obtained in step (2) is immersed in toluene to remove the polystyrene microspheres, and then the composite film is taken out and the solvent is evaporated to obtain a composite film with a Janus structure.

[0114] The composite film prepared in Example 2 was used to purify water by photothermal water evaporation according to the method of Example 1. The results are shown in Table 2.

[0115] Table 2 Water purification data of the composite film prepared in Example 2

[0116]

[0117]

[0118] It can be seen from Table 2 that the composite film prepared by the present invention has excellent water purification effect.

[0119] Example 3

[0120] The composite film is composed of a water transmission layer and a light-to-heat conversion layer arranged in layers;

[0121] The water transport layer is a porous graphene oxide membrane with a thickness of 10 μm;

[0122] The light-to-heat conversion layer is composed of graphene oxide and polyaniline fibers, and has a thickness of 42 μm;

[0123] The polyaniline fiber has a diameter of 150 to 300 nm and a length of 0.5 to 5 μm;

[0124] The mass ratio of graphene oxide to polyaniline fiber in the light-to-heat conversion layer is 1:4;

[0125] The thickness of the composite film is 52 μm;

[0126] The preparation method of the composite film comprises the following steps:

[0127] (1) 9 mL of a 3 mg / mL graphene oxide aqueous solution was mixed with 3 mg of polystyrene microspheres and filtered through a 0.22 μm cellulose filter membrane to obtain a graphene oxide membrane; wherein the particle sizes of the polystyrene microspheres were 0.1 μm, 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm and 1.0 μm, and the mass ratio of the polystyrene microspheres of each particle size was 1:1:1:1:1:1; the mass ratio of graphene oxide to polystyrene microspheres was 27:3; a 0.5 L liquid mobile phase filtration device was used for filtration, and the vacuum degree was -0.09 MPa;

[0128] (2) After 1 mL of a 3 mg / mL aqueous solution of graphene oxide and polyaniline fibers are stirred and mixed, the mixture is filtered on the graphene oxide membrane obtained in step (1) through a 0.22 μm cellulose filter membrane, and then placed in a dry environment for evaporation and drying, and then separated from the filter membrane to obtain a composite membrane; wherein the mass ratio of graphene oxide to polyaniline fibers is 1:4; a 0.5 L liquid mobile phase filtration device is used for filtration, and the vacuum degree is -0.09 MPa; the drying humidity is 20%, and the temperature is 23° C.;

[0129] (3) The composite film obtained in step (2) is immersed in toluene to remove the polystyrene microspheres, and then the composite film is taken out and the solvent is evaporated to obtain a composite film with a Janus structure.

[0130] The composite film prepared in Example 3 was used to purify water by photothermal water evaporation according to the method of Example 1. The results are shown in Table 3.

[0131] Table 3 Water purification data of the composite film prepared in Example 3

[0132]

[0133]

[0134] It can be seen from Table 3 that the composite film prepared by the present invention has excellent water purification effect.

[0135] It can be seen from the above examples that the composite film provided by the present invention has an excellent pollutant removal rate.

[0136] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A composite film comprising a water transmission layer and a light-to-heat conversion layer stacked in layers; The water transport layer is a porous graphene oxide membrane; The components of the light-to-heat conversion layer include graphene oxide and polyaniline fibers.

2. The composite film according to claim 1, characterized in that The thickness of the composite film is 30-52 μm.

3. The composite film according to claim 1, characterized in that The thickness of the water transfer layer is 7-12 μm, and the thickness of the light-to-heat conversion layer is 23-40 μm.

4. The composite film according to claim 1, characterized in that The diameter of the polyaniline fiber is 150-300 nm, and the length of the polyaniline fiber is 0.5-5 μm.

5. The composite film according to claim 1, characterized in that The mass ratio of graphene oxide to polyaniline fiber in the light-to-heat conversion layer is (2-4):(6-15).

6. The composite film according to claim 1 or 5, characterized in that: The mass ratio of graphene oxide to polyaniline fiber in the light-to-heat conversion layer is 3:(9-12).

7. The method for preparing the composite film according to any one of claims 1 to 6, comprising the following steps: (1) mixing a first graphene oxide solution with a pore-forming agent, and then filtering to obtain a graphene oxide film; (2) mixing the second graphene oxide solution with the polyaniline fiber, and then filtering on the graphene oxide membrane obtained in step (1) to obtain a composite membrane; (3) Immersing the composite film obtained in step (2) in toluene to obtain a composite film.

8. The preparation method according to claim 7, characterized in that: The pore-forming agent in step (1) is polystyrene microspheres.

9. The preparation method according to claim 7 or 8, characterized in that: The mass ratio of graphene oxide to pore former in the first graphene oxide solution is (12-48): (1-6).

10. Use of the composite film according to any one of claims 1 to 6 or the composite film prepared by the preparation method according to any one of claims 7 to 9 in water purification.