Magnetic control rare earth anion film and preparation method thereof

By introducing magnetron technology and the combination of rare earth materials and tourmaline into rare earth negative ion membranes, the problem of low conversion efficiency of negative oxygen ion in the prior art is solved, the concentration and coverage of negative oxygen ions are significantly improved, and the indoor air is improved Purification effect.

CN119015908APending Publication Date: 2024-11-26MIANYANG LIANGGU TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411130091.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art cannot effectively control the electrostatic field, resulting in low conversion efficiency of negative oxygen ions generated by rare earth materials in indoor air, insufficient concentration, and unable to significantly improve the effect of a healthy environment.

Method used

Magnetic control rare earth negative ion film is used, and the magnetic ring and rare earth negative oxygen ion layer are set on the polyester layer, and the magnetic field is used to guide the movement of electrical particles to improve the release efficiency and concentration of negative oxygen ions, and combine rare earth materials and tourmaline to improve the excitation performance. .

Benefits of technology

It has achieved efficient guidance and high-energy electron transition for rare earth negative oxygen ions, significantly improving the concentration and coverage of negative oxygen ions, and enhancing the indoor air purification effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015908A_ABST
    Figure CN119015908A_ABST
Patent Text Reader

Abstract

The invention discloses a magnetic control rare earth anion membrane and a preparation method thereof, and relates to the field of rare earth anion membranes, a plurality of grooves are formed in a first polyester layer, magnetic rings are arranged in the grooves, each magnetic ring comprises an upper magnetic layer and a lower magnetic layer, through grooves are formed in the center of the upper magnetic layer and the center of the lower magnetic layer, the upper magnetic layer is an S pole, and the lower magnetic layer is an N pole; the axis of the magnetic ring coincides with the center line of the groove. A rare earth negative oxygen ion layer is arranged in the groove and located in the through groove of the magnetic ring. According to the invention, electrons in the rare earth negative oxygen ion layer can be guided, so that more electric particles are combined with oxygen molecules in indoor air, and efficient negative oxygen ions are generated. And the emission distance of electrons in the rare earth negative oxygen ion layer can be farther.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of negative oxygen ion membranes, and in particular to a magnetically controlled rare earth negative ion membrane and a preparation method thereof. Background Art

[0002] In recent years, the human living environment has been polluted by certain indoor building materials and daily necessities, making the content of harmful substances indoors 10-100 times higher than outdoors, posing a huge threat to human health.

[0003] Negative oxygen ions, also known as "air vitamins", can sterilize and remove dust, and have a certain effect on the disinfection and purification of the air. They can regulate the human autonomic nerves, improve cardiopulmonary function, increase breathing depth, promote human metabolism, are beneficial to human health, and can enhance human immunity. According to research by environmentalists, when the concentration of negative oxygen ions in the air is below 20 per cubic centimeter, people will feel tired and dizzy; when the number of negative oxygen ions in the air is between 1,000 and 10,000 per cubic centimeter, people will feel calm and peaceful.

[0004] A natural nano-composite material capable of releasing negative oxygen ions with application number 201510268784.0 discloses a natural nano-composite material capable of releasing negative oxygen ions, wherein the main raw materials and auxiliary raw materials are some natural organic plants, and the carrier matrix is ​​a crystalline hydrated magnesium aluminum silicate mineral, and the composite material can release negative oxygen ions; A negative oxygen ion generating material containing germanium and rare earth with application number 201610288784.1 discloses a material prepared by high-temperature calcination of a mixture of germanium as the main material and some rare earth compounds, which has the function of generating negative oxygen ions.

[0005] The existing technology adds rare earth materials to tourmaline and coats it on a polyester film substrate. Adding rare earth materials to tourmaline can improve its ability to stimulate the production of negative oxygen ions. However, the existing technology cannot control the electrostatic field in one direction, and only half of the negative ions can combine with oxygen molecules in the indoor air to form negative oxygen ions. Therefore, the conversion efficiency is too low, and the concentration of the negative oxygen ions produced is low, and no obvious health environment effect can be produced. Summary of the invention

[0006] One object of the present invention is to provide a magnetically controlled rare earth anion membrane and a preparation method thereof, so as to improve the release efficiency and concentration of negative oxygen ions.

[0007] This purpose is achieved by adopting the following technical solutions:

[0008] A magnetically controlled rare earth anion membrane and a preparation method thereof, comprising a first polyester layer, a plurality of grooves being arranged on the first polyester layer, magnetic rings being arranged in the grooves, the magnetic rings comprising an upper magnetic layer and a lower magnetic layer, through grooves being arranged at the centers of the upper magnetic layer and the lower magnetic layer, the upper magnetic layer being of S grade, and the lower magnetic layer being of N grade; the axis of the magnetic ring coincides with the center line of the groove; a rare earth negative oxygen ion layer is arranged in the groove.

[0009] The negative ion membrane of the present invention acts on a glass substrate, and the rare earth negative oxygen ion layer is located in the through groove of the magnetic ring. First, the moving direction of the electric particles can be controlled. The magnetic ring of the present invention has an upper magnetic layer of S level, a lower magnetic layer of N level, and a through groove at the center. The magnetic field distribution of the magnetic ring points from the N pole to the S pole, that is, the upper magnetic layer points to the lower magnetic layer. The magnetic field distribution at the through groove in the middle of the magnetic ring is also from the N pole to the S pole. The magnetic field distribution at the periphery of the magnetic ring is also from the N pole to the S pole. The through groove in the middle of the magnetic ring and the periphery form a closed magnetic field distribution.

[0010] Therefore, under the action of the magnetic ring, the movement of the electric particles in the rare earth negative oxygen ion layer in the through groove in the middle of the magnetic ring in the magnetic field will be affected by the Lorentz force, causing the rotation direction of the particles to change, forcing the movement direction of the electric particles to be consistent with the direction of the magnetic field, thereby completing the guiding effect on the electrons.

[0011] The existing negative ion membrane cannot control the electrostatic field in one direction, so only a small number of negative ions combine with oxygen molecules in the indoor air to form negative oxygen ions. However, under the action of the magnetic ring, the present invention can guide the electrons in the rare earth negative oxygen ion layer, so that more negative ions combine with oxygen molecules in the indoor air to form negative oxygen ions.

[0012] On the other hand, under the action of the magnetic ring of the present invention, the high-energy electrons of the rare earth material can be transferred from a low-energy state to a high-energy excited state. Since the orbital energy of the atomic nucleus will be interrupted by the strong magnetic field, the ions in the atom will be in an extremely unstable state and charge exchange may occur at any time, thereby changing the molecular structure, increasing the activity of the electron movement, making the electron emission distance farther, and thus making the concentration of negative oxygen ions higher.

[0013] Furthermore, the inner diameter of the groove of the present invention gradually decreases from top to bottom, and the diameter of the outer ring of the magnetic ring and the through groove gradually decreases from top to bottom. Therefore, the magnetic ring can make the negative ions diverge into the room at a wider angle, further enhancing the interaction between the negatively charged particles and the indoor air, thereby generating more negative oxygen ions.

[0014] Preferably, the ratio of the thickness of the magnetic ring to the inner diameter of the magnetic ring slot is 1:5-12. Under this ratio, the negative oxygen ion content released per unit negative ion membrane is higher, which is more conducive to indoor use.

[0015] Preferably, the rare earth negative oxygen ion layer comprises tourmaline, rare earth oxide and a binder. The upper magnetic layer and the lower magnetic layer comprise rare earth magnetic powder, a silane coupling agent and a binder.

[0016] Adding rare earth materials to tourmaline can improve its ability to stimulate the production of negative oxygen ions, because the outermost electron structure of the atoms of rare earth elements is the same, both with 2 electrons, and the second outermost structure is similar, while the third from the bottom has an unfilled 4f electron layer structure. There are unpaired electrons in the 4f orbit, and the two outermost electrons undergo electronic transitions, thereby generating a variety of electronic energy levels, generating holes on the atomic surface of rare earth elements, causing them to catalyze reactions with the system composed of water and air, generating O2 and OH active oxygen free radicals, ionizing molecules in the air, and thus increasing the concentration of negative ions in the air.

[0017] Rare earth materials are combined with tourmaline to improve its performance. Since rare earth materials can convert the radiant heat energy of sunlight into physical heat energy, they have a heating effect on tourmaline and can effectively improve its discharge characteristics. The prepared rare earth negative oxygen ion membrane has photothermal response function, and the purpose of controllable release of negative oxygen ions can be achieved by adjusting the light intensity and temperature.

[0018] On the other hand, there is a gap between two adjacent grooves in the present invention, and the negative ion membrane of the present invention acts on the glass. When sunlight shines on the glass, the light transmittance is improved through the gap between the two adjacent grooves. Preferably, the groove and the magnetic ring are both circular, and the two adjacent grooves are in contact with each other. When the circular magnetic ring is located in the groove, the two adjacent magnetic rings are in contact with each other, and at the same time, there is a gap between two magnetic rings of the same size.

[0019] Secondly, the upper end of the first polyester layer is provided with a second polyester layer and a wear-resistant layer in sequence from bottom to top.

[0020] The lower end of the first polyester layer is provided with a protective layer and an adhesive layer in sequence from bottom to top.

[0021] On the other hand, the present invention provides a method for preparing a magnetically controlled rare earth anion membrane, which comprises first pressing a plurality of grooves on a first polyester layer, then filling the grooves with magnetic rings, and finally filling the through grooves of the magnetic rings with a rare earth anion layer.

[0022] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0023] The present invention provides a magnetically controlled rare earth anion membrane and a preparation method thereof. The movement of electric particles in a magnetic field will be affected by the Lorentz force, causing the movement trajectory to bend and form a spiral line, so that the rotation direction of the particles is changed, forcing the movement direction of the electric particles to be consistent with the direction of the magnetic field, guiding the electrons in the rare earth negative oxygen ion layer, allowing more electric particles to combine with oxygen molecules in the indoor air to produce efficient negative oxygen ions.

[0024] Secondly, the present invention adopts magnetron technology to transfer high-energy electrons from a low-energy state to a high-energy excited state. The ions in the atoms will be in an extremely unstable state, which increases the activity of electron movement and makes the electron emission distance in the rare earth negative oxygen ion layer farther.

[0025] The use of rare earth materials combined with tourmaline improves its performance and further promotes the release of negative oxygen ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:

[0027] Figure 1 Schematic diagram of the negative ion membrane structure in Example 1;

[0028] Figure 2 It is a schematic diagram of the magnetic ring structure;

[0029] Figure 3 This is a schematic diagram of the structure when the magnetic ring is on the first polyester layer;

[0030] Figure 4 The schematic diagram of the negative ion membrane structure is when the inner diameter of the groove gradually decreases from top to bottom, and the diameters of the outer ring of the magnetic ring and the through groove gradually decrease from top to bottom;

[0031] Figure 5 It is a schematic diagram of the structure of the second polyester layer, the wear-resistant layer, the first polyester layer, the protective layer and the adhesive layer;

[0032] Figure 6 This is a schematic diagram of the structure of the preparation device in Example 4;

[0033] Figure 7 This is a schematic diagram of the structure of the two conveying rods and the magnetic powder conveyor belt in Example 4.

[0034] Marks and corresponding parts names in the attached drawings:

[0035] 1-first polyester layer, 2-magnetic ring, 3-rare earth negative oxygen ion layer, 4-second polyester layer, 5-wear-resistant layer, 6-adhesive layer, 7-protective layer, 8-glass substrate, 9-transmission plate, 10-convex column, 11-first telescopic rod, 12-second telescopic rod, 13-outer cover, 131-magnetic powder conveyor belt, 132-transmission rod. DETAILED DESCRIPTION

[0036] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0037] In the description of the present invention, it should be understood that the terms "front", "rear", "left", "right", "up", "down", "vertical", "horizontal", "high", "low", "inside", "outside", etc., indicating directions or positional relationships are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as limiting the scope of protection of the present invention.

[0038] Example 1

[0039] like Figure 1 As shown, it includes a first polyester layer 1 , a plurality of grooves are arranged on the first polyester layer 1 , magnetic rings 2 are arranged in each groove, a rare earth negative oxygen ion layer 3 is arranged in the groove, and the rare earth negative oxygen ion layer 3 is located in the through groove of the magnetic ring 2 .

[0040] The structure of magnetic ring 2 is as follows Figure 2 As shown, the magnetic ring 2 includes an upper magnetic layer and a lower magnetic layer, and a through groove is provided at the center of the upper magnetic layer and the lower magnetic layer. The upper magnetic layer is of level S, and the lower magnetic layer is of level N. When the magnetic ring 2 is located in the groove, the axis of the magnetic ring 2 coincides with the center line of the groove.

[0041] The first polyester layer 1 is provided with a magnetic ring and a rare earth negative oxygen ion layer to obtain a negative ion membrane.

[0042] The first polyester layer is arranged on the glass substrate, so that the rare earth negative oxygen ion layer 3 on the first polyester layer releases negative oxygen ions, thereby increasing the concentration of negative oxygen ions in the indoor air.

[0043] Among them, the magnetic ring 2 and the rare earth negative oxygen ion layer 3 are existing materials, and the inventors do not limit their specific ratios as long as they can achieve their respective effects.

[0044] In some embodiments, the upper magnetic layer and the lower magnetic layer of the magnetic ring 2 include magnetic powder, a silane coupling agent and a binder. The magnetic powder may include but is not limited to SmFeN, NdFeB or SmCo rare earth magnetic powder. The rare earth magnetic powder is more preferably SmFeN magnetic powder, which has better heat resistance than NdFeB and has the advantage of not containing rare metals than SmCo. The SmFeN magnetic powder may be a nitride having the following characteristics: a 2-zinc 17-type crystal structure and containing rare earth metal Sm, iron (Fe) and nitrogen (N), such as the formula: Smx Fe 100-x-y Ny wherein the value "x" representing the atomic percentage (%) of the rare earth metal Sm is in the range of 8.1 to 10 (at%); the value "y" representing the atomic percentage (%) of N is in the range of 13.5 to 13.9 (at%); the remainder is mainly Fe. Furthermore, the magnetic powder may be a combination of SmFeN magnetic powder and NdFeB or SmCo rare earth magnetic powder or ferrite magnetic powder.

[0045] In some embodiments, the upper magnetic layer and the lower magnetic layer are both composed of coupled pure high-abundance rare earth magnetic powder, rubber and vulcanizing agent, wherein the weight of the coupled pure high-abundance rare earth magnetic powder is 10 to 90 parts, the weight of the rubber is 10 parts, and the weight of the vulcanizing agent is 0.1 to 0.5 parts. Preferably, the composition of the pure high-abundance rare earth magnetic powder of the present invention is [(CeaLa1-a)bY1-b]cFe95-c-dB6Nd in terms of atomic ratio, wherein N is at least one of Nb, Al, Ga, Cu, Zr, Si, Ti, Ge, a is in the range of 0.4 to 0.9, b is in the range of 0.5 to 0.8, c is in the range of 14 to 18, and d is in the range of 0.1 to 2.

[0046] In some embodiments, the upper magnetic layer and the lower magnetic layer both include NdFeB magnetic powder, rubber coupling agent and other additives. Specifically, 90%wt of NdFeB magnetic powder, 9%wt of rubber, and 1%wt of coupling agent and other additives are mixed and crushed into particles of uniform size. The particles are put into a rubber extruder and extruded through a die with arcs at both ends to obtain rare earth magnetic strips of corresponding sizes. A 0.2mm thick thermoplastic flexible elastic layer is extruded on the surface of the rare earth magnetic strip to obtain a flexible rare earth magnetic strip. Then, the length is cut according to the specifications and injection molding is performed at both ends to form a flexible head.

[0047] In some embodiments, the rare earth negative oxygen ion layer 3 includes tourmaline, rare earth oxide and a binder. Among them, titanium dioxide powder, activated carbon and diatomaceous earth powder are added to anhydrous ethanol and dispersed evenly, and then silica gel and synthetic resin are added and stirred to form a latex, and then tourmaline powder is added and ultrasonically vibrated to make the tourmaline powder evenly dispersed in the latex to obtain a rare earth negative oxygen ion glue.

[0048] In some embodiments, the rare earth negative oxygen ion layer 3 includes raw materials of nano photocatalytic material, negative oxygen ion releasing material, modifier and binder and deionized water, and the nano photocatalytic material is selected from nano TiO2, and preferably, the particle size of nano TiO2 is 10-25nm. The negative oxygen ion releasing material includes tourmaline and rare earth oxide, and the average particle size of tourmaline is 5-20μm. The rare earth oxide is cerium oxide (CeO2) and / or lanthanum oxide (La2O3), and preferably, the average particle size is 1-5nm. The modifier is selected from one or more of polyethylene glycol, ammonium polymethyl acrylate or ammonium polyacrylate; the binder is selected from one or more of nano copper, nano zinc, and nano tin, and preferably, the particle size is selected from 5-20nm.

[0049] Example 2

[0050] Based on the above embodiments, Figure 3 As shown, there is a gap between two adjacent grooves. When the negative ion membrane of the present invention acts on glass, the light transmission effect can be further improved through the gap.

[0051] In some embodiments, the grooves and the magnetic rings 2 are both circular, and two adjacent grooves are in contact with each other. The magnetic rings are evenly arranged on the first polyester layer 1 to form a plurality of columns and rows, and the number of magnetic rings on each column and row is the same.

[0052] In some embodiments, Figure 4 As shown, the inner diameter of the groove gradually decreases from top to bottom, and the diameter of the outer ring of the magnetic ring 2 and the through groove gradually decreases from top to bottom. The upper end of the groove is the end facing the room, and the lower end of the groove is the end connected to the glass substrate. The diameter of the outer ring of the magnetic ring 2 and the through groove gradually decreases from top to bottom, so the magnetic ring can make the negative ions diverge into the room at a wider angle, further improve the interaction between the negative particles and the indoor air, and then produce more negative oxygen ions.

[0053] In some embodiments, the ratio of the thickness of the magnetic ring 2 to the inner diameter of the slot of the magnetic ring 2 is 1:5-12. Under this ratio, the negative oxygen ion content released per unit negative ion membrane is higher, which is more conducive to indoor use.

[0054] In some embodiments, the height of the magnetic ring 2 is greater than the height of the rare earth negative oxygen ion layer 3 , that is, when the rare earth negative oxygen ion layer 3 is located inside the magnetic ring 2 , the upper end of the magnetic ring 2 is located above the upper end of the rare earth negative oxygen ion layer 3 .

[0055] Example 3

[0056] Based on the above embodiments, Figure 5As shown, the upper end of the first polyester layer 1 is provided with a second polyester layer 4 and a wear-resistant layer 5 in sequence from bottom to top, and the lower end of the first polyester layer 1 is provided with a protective layer 7 and an adhesive layer 6 in sequence from bottom to top, and the protective layer 7 is connected to the glass substrate 8, wherein the wear-resistant layer 5, the protective layer 7 and the adhesive layer 6 are all existing materials, and the specific components and proportions of the wear-resistant layer 5, the protective layer 7 and the adhesive layer 6 can be selected from conventional materials, and the inventor does not make specific limitations here.

[0057] Example 4

[0058] Based on the above embodiment, a method for preparing a magnetically controlled rare earth anion membrane comprises the following steps:

[0059] Pressing a plurality of grooves on the first polyester layer 1;

[0060] Fill the groove with magnetic ring 2;

[0061] A rare earth negative oxygen ion layer 3 is filled in the through groove of the magnetic ring 2 to obtain a negative ion membrane;

[0062] A second polyester layer 4 and a wear-resistant layer 5 are sequentially arranged on the upper end of the first polyester layer 1 from bottom to top;

[0063] A protective layer 7 and an adhesive layer 6 are sequentially arranged at the lower end of the first polyester layer 1 from bottom to top, and the protective layer 7 is connected to the glass substrate 8 .

[0064] Among them, this embodiment includes a preparation device for preparing a negative ion membrane, the preparation device is as follows Figure 6 As shown, the preparation device includes a conveying plate 9, which is used to convey the first polyester layer. A pressing assembly and a magnetic ring assembly are arranged above the conveying plate 9. The pressing assembly gradually includes a first telescopic rod 11. An action plate 9 is arranged at the lower end of the first telescopic rod 11. A plurality of convex columns 10 are arranged on the action plate, and the convex columns 10 are cylindrical.

[0065] The magnetic ring assembly includes a second telescopic rod 12, a magnetic powder assembly is arranged at the lower end of the second telescopic rod 12, and the magnetic powder assembly includes an outer cover 13 and two transmission rods 132, and the two transmission rods 132 are connected in the outer cover 13. Figure 7 As shown, a magnetic powder conveyor belt 131 is provided on the conveying rod 132, and the interior of the second telescopic rod 12 is a hollow structure. The magnetic powder enters the magnetic powder conveyor belt 131 through the interior of the second telescopic rod 12. Driven by the magnetic powder conveyor belt, the magnetic powder is driven to the lower end of the magnetic powder conveyor belt 131 and enters the groove of the first polyester layer. After the magnetic powder enters the groove, the outer cover 13 scrapes off the excess magnetic powder on the first polyester layer.

[0066] In addition, the present invention can first mix the magnetic powder, rubber coupling agent and other additives and then crush them into particles of uniform size, put the particles into a rubber extruder, and extrude them through a mold to obtain magnetic rings of corresponding sizes. The magnetic rings enter the magnetic powder conveyor belt through the inside of the second telescopic rod, and the positions of the magnetic rings on the magnetic powder conveyor belt correspond to the positions of the plurality of grooves on the first polyester layer. When the upper end of the magnetic powder conveyor belt 131 is transmitted to the lower end, the magnetic rings contact with the grooves in turn and enter the grooves.

[0067] After the magnetic ring is placed in the groove, a rare earth negative oxygen ion layer 3 is filled in the through groove of the magnetic ring to obtain a negative ion membrane; the negative ion membrane is magnetized to obtain a magnetically controlled rare earth negative oxygen ion membrane. During the magnetization treatment, the charging voltage is 2000V, and a multi-stage fixture is used for magnetization, and the surface of the magnetic strip under the magnetic display sheet presents N / S alternating multi-poles.

[0068] Example 5

[0069] The negative ion membranes of Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested for negative ion release performance, wherein the grooves and magnetic rings 2 of the negative ion membrane in Example 1 were both circular, and two adjacent grooves were in contact with each other, and the ratio of the thickness of the magnetic ring 2 to the inner diameter of the through groove of the magnetic ring 2 was 1:8. The height of the magnetic ring 2 was greater than the height of the rare earth negative oxygen ion layer 3.

[0070] The grooves of the negative ion membrane and the magnetic ring 2 in comparative example 1 are both circular, and two adjacent grooves are in contact with each other, and the ratio of the thickness of the magnetic ring 2 to the inner diameter of the groove of the magnetic ring 2 is 1:1. The height of the magnetic ring 2 is equal to the height of the rare earth negative oxygen ion layer 3.

[0071] The inner diameter of the groove of the negative ion membrane in comparative example 2 gradually decreases from top to bottom, and the diameter of the outer ring and the through groove of the magnetic ring 2 gradually decreases from top to bottom. The ratio of the thickness of the magnetic ring 2 to the inner diameter of the through groove of the magnetic ring 2 is 1:8. The height of the magnetic ring 2 is greater than the height of the rare earth negative oxygen ion layer 3.

[0072] The negative ion membrane in Comparative Example 3 includes a first polyester layer and a negative oxygen ion coating. The negative oxygen ion coating includes raw materials including nano-photocatalytic materials, negative oxygen ion releasing materials, functional enhancement materials, modifiers and binders, mixed with deionized water to prepare a raw material dispersion, and then the photocatalytic negative oxygen ion releasing coating is prepared on the surface of the substrate by flame spraying. The negative oxygen ion releasing material is selected from one or more of tourmaline, quartz, and seaweed charcoal; the functional enhancement material is selected from nano-precious metal materials and / or rare earth oxide materials.

[0073] The sizes of the negative ion membranes of Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 are the same, and the numbers of the magnetic rings therein are also the same.

[0074] The negative ion membranes of Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested at room temperature of 25°C and humidity of 55%. The laboratory (5m×4m×3m) was fully ventilated and the doors and windows were closed. The negative ion membrane of Example 1 was placed in the center of the laboratory. For 15 minutes, detectors were placed at different distances from the generator along the line of the negative ion generator. The wind speed was 0, and the wind direction was perpendicular to the line of the generator. The distance was measured from the front end of the generator to the center of the detection window. The values ​​of the detector readings at different distances were recorded, and the average value was calculated. The test results are shown in Table 1;

[0075] Table 1

[0076]

[0077] It can be seen from Table 1 that the negative oxygen ion concentration of Comparative Example 1 is greater than that of Comparative Example 3 but less than that of Example 1 and Comparative Example 2. The ratio of the thickness of the magnetic ring 2 to the inner diameter of the groove of the magnetic ring 2 in Comparative Example 1 is not within the protection scope of the present invention. The concentration of negative oxygen ions generated in Comparative Example 1 is small, and the distance of electron emission is short. Therefore, the coverage range is smaller than that of Example 1 and Comparative Example 2.

[0078] Comparative Example 3 is an existing coating, in which rare earth materials are directly added to tourmaline and coated on a polyester film substrate. Although adding rare earth materials to tourmaline can improve its performance in exciting and generating negative oxygen ions, Comparative Example 3 cannot control the electrostatic field in one direction, and only part of the negative ions combine with oxygen molecules in the indoor air to form negative oxygen ions. Therefore, the conversion efficiency is low.

[0079] The negative oxygen ion concentrations produced by Example 1 and Comparative Example 2 are the highest, and the distance of the negative oxygen ions produced by Example 1 and Comparative Example 2 is the longest and the range is wide. In Example 1 and Comparative Example 2, under the action of the magnetic ring, the electrons in the rare earth negative oxygen ion layer 3 can be guided, so that more negative ions are combined with oxygen molecules in the indoor air to form negative oxygen ions. Moreover, under the action of the magnetic ring, the molecular structure changes, which increases the activity of the electron movement, makes the electron emission distance farther, and thus makes the concentration of negative oxygen ions higher and the coverage wider.

[0080] The terms "first", "second", etc. used herein are only used to distinguish the corresponding components for the sake of clarity of description, and are not intended to limit any order or emphasize importance, etc. In addition, the term "connected" used herein, unless otherwise specified, may refer to direct connection or indirect connection via other components.

[0081] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A magnetically controlled rare earth anion membrane, characterized in that: The invention comprises a first polyester layer (1), wherein a plurality of grooves are arranged on the first polyester layer (1), wherein magnetic rings (2) are arranged in the grooves, wherein the magnetic rings (2) comprise an upper magnetic layer and a lower magnetic layer, wherein through grooves are arranged at the centers of the upper magnetic layer and the lower magnetic layer, wherein the upper magnetic layer is of S grade and the lower magnetic layer is of N grade; wherein the axis of the magnetic ring (2) coincides with the center line of the grooves; wherein a rare earth negative oxygen ion layer (3) is arranged in the grooves, wherein the rare earth negative oxygen ion layer (3) is located in the through grooves of the magnetic ring (2).

2. A magnetically controlled rare earth anion membrane according to claim 1, characterized in that: The groove and the magnetic ring (2) are both circular, and two adjacent grooves are in contact with each other.

3. A magnetically controlled rare earth anion membrane according to claim 1, characterized in that: There is a gap between two adjacent grooves.

4. A magnetically controlled rare earth anion membrane according to claim 1, characterized in that: The upper end of the first polyester layer (1) is provided with a second polyester layer (4) and a wear-resistant layer (5) in sequence from bottom to top.

5. The magnetically controlled rare earth anion membrane according to claim 1, characterized in that: The lower end of the first polyester layer (1) is provided with a protective layer (7) and an adhesive layer (6) in sequence from bottom to top.

6. The magnetically controlled rare earth anion membrane according to claim 1, characterized in that: The inner diameter of the groove gradually decreases from top to bottom, and the diameters of the outer ring of the magnetic ring (2) and the through groove gradually decrease from top to bottom.

7. The magnetically controlled rare earth anion membrane according to claim 1, characterized in that: The ratio of the thickness of the magnetic ring (2) to the inner diameter of the slot of the magnetic ring (2) is 1:5-12.

8. The magnetically controlled rare earth anion membrane according to claim 1, characterized in that: The upper magnetic layer and the lower magnetic layer include rare earth magnetic powder, a silane coupling agent and a binder.

9. The magnetically controlled rare earth anion membrane according to claim 1, characterized in that: The rare earth negative oxygen ion layer (3) comprises tourmaline, rare earth oxide and a binder.

10. The method for preparing a magnetically controlled rare earth anion membrane according to claim 1, characterized in that: The method comprises the following steps: Pressing a plurality of grooves on the first polyester layer (1); Filling the groove with a magnetic ring (2); A rare earth negative oxygen ion layer (3) is filled in the through groove of the magnetic ring (2).