Adsorbent for air separation and preparation method and application thereof
By combining sodium-based or sodium-potassium-based X-type molecular sieve with kaolin and other materials, it is solved to solve the problem of inconvenience in operation and performance reduction of Li-LSX molecular sieve powder in industrial use, and efficient adsorption for air separation is prepared. , improve adsorption performance and safety.
Patent Information
- Application Number
- CN202411147227.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
The existing Li-LSX molecular sieve adsorbents are inconvenient to operate and health hazards in industrial use due to the fine powder form, and the adsorption performance and utilization rate are reduced due to the influence of the added binder.
By mixing the sodium-based or sodium-potassium-based X-type molecular sieve raw powder with kaolin, molding additives and silicon source solution, after multiple kneading, drying and crushing, the amorphous metakaolin is transformed into an X-type molecular sieve, and air is prepared by ion exchange Adsorbents for separation improve adsorption performance and safety.
The prepared adsorbent for air separation has a high nitrogen-oxygen separation coefficient and nitrogen adsorption capacity, which improves the active ingredient content and compressive resistance of the adsorbent, and improves the overall preparation efficiency through lithium ion utilization and lithium phosphate recovery.
Smart Images

Figure BDA0005002528200000131
Abstract
Description
Technical Field
[0001] The invention relates to the field of molecular sieves, and in particular to an adsorbent for air separation and a preparation method and application thereof. Background Art
[0002] Oxygen is an important industrial raw material. Pressure swing adsorption (VPSA / PSA) oxygen production has the advantages of simple equipment, low investment, simple process, stability, reliability, rapid oxygen production, small footprint, few equipment, and high degree of automation. It is widely used in medical oxygen, household oxygen, oxygen-enriched combustion, metal smelting and other fields. In the process of oxygen production by pressure swing adsorption, the oxygen-producing molecular sieve adsorbent plays the role of nitrogen absorption and oxygen production (selective adsorption of nitrogen and enrichment of oxygen) by its selective adsorption of nitrogen.
[0003] Li-LSX molecular sieve adsorbent has a high nitrogen adsorption capacity and nitrogen-oxygen separation coefficient, and has always been the preferred adsorbent for air separation in pressure swing adsorption (PSA) or vacuum pressure swing adsorption (VPSA) processes.
[0004] Artificially synthesized Li-LSX molecular sieves are generally in powder form, only a few microns. Fine molecular sieve crystals have advantages such as good adsorption performance, ion exchange performance, selectivity and catalytic performance. However, fine powder products will produce excessive pressure drop in industrial use, which is inconvenient to operate and will also endanger the health of the operator. Therefore, the molecular sieve powder must be prepared into aggregates with a certain shape and size. Generally, 10% to 20% of a binder is added to the molecular sieve powder to make particles with a certain mechanical strength and shape. Due to the presence of the binder, the effective components of the molecular sieve are reduced, thereby reducing the utilization rate and adsorption performance of the Li-LSX molecular sieve aggregates. Summary of the invention
[0005] The present invention provides an adsorbent for air separation, a preparation method and application thereof. The adsorbent for air separation prepared by the present invention has the performance of high nitrogen-oxygen separation coefficient, high nitrogen adsorption capacity and high PSA / VPSA oxygen production.
[0006] The present invention provides a method for preparing an adsorbent for air separation, comprising the following steps:
[0007] The sodium-based or sodium-potassium-based X-type molecular sieve raw powder, kaolin, a molding aid and a first silicon source solution are mixed and kneaded to obtain a matrix material;
[0008] Drying and crushing the matrix material to obtain crushed powder;
[0009] Repeatedly mixing, kneading, drying and crushing the crushed powder with a second silicon source solution to obtain N-times crushed powder;
[0010] The N-th-time crushed powder is mixed with a third silicon source solution and then molded to obtain an intermediate;
[0011] The intermediate is subjected to a first drying and roasting to obtain a primary roasting intermediate containing amorphous metakaolin;
[0012] The primary calcined intermediate containing amorphous metakaolin is mixed with a silicon-containing alkaline aqueous solution for aging and crystallization, and the amorphous metakaolin is converted into an X-type molecular sieve to obtain a sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve;
[0013] The sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve is mixed with a lithium-ion-containing aqueous solution for ion exchange to obtain an exchange intermediate; the ion exchange is carried out in an exchange column: the sodium-based or sodium-potassium-based molecular sieve is loaded in the exchange column, and the lithium-ion-containing aqueous solution flows in from the lower part of the exchange column and flows out from the upper part;
[0014] The exchange intermediate is dried and calcined for a second time to obtain the adsorbent for air separation.
[0015] Preferably, the silicon-aluminum ratio of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder is 1.9 to 2.1;
[0016] The silicon-aluminum ratio of the kaolin is 1.75-2.1.
[0017] Preferably, based on dry weight, the mass of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder is 90-95% of the total mass of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder and kaolin.
[0018] Preferably, the molding aid comprises tannin extract and pore former.
[0019] Preferably, the water content of the matrix material and the matrix material obtained by kneading in each repeated process is independently 36 to 39 wt %;
[0020] The water content of the crushed powder and the crushed powder obtained in each repeated crushing process is independently ≤12wt%;
[0021] The water content of the intermediate is 36-42 wt%.
[0022] Preferably, the volume ratio of the mass of the primary calcined intermediate on a dry basis to the silicon-containing alkaline aqueous solution is 1 kg: 2.2 to 3 L;
[0023] The OH in the silicon-containing alkaline aqueous solution - The concentration of is 2.26-2.90 mol / L, and the concentration of silicon source calculated as SiO2 is 5-19 g / L;
[0024] The aging and crystallization are carried out in a crystallization column: the primary calcined intermediate is loaded in the crystallization column, and the silicon-containing alkaline aqueous solution cyclically flows in from the lower part and out from the upper part of the crystallization column.
[0025] Preferably, the concentration of lithium ions in the lithium ion-containing aqueous solution is 0.35 to 2.5 mol / L, and the pH of the lithium ion-containing aqueous solution is 8 to 12;
[0026] The temperature of the ion exchange is 90-100°C;
[0027] The flow rate of the lithium ion aqueous solution is 0.5 to 3 m 3 / h.
[0028] Preferably, after the ion exchange, the process further comprises: separating the product obtained by the ion exchange, centrifuging the obtained waste liquid, mixing it with an alkali solution, and then mixing it with a precipitant to perform a precipitation reaction, and then filtering and drying the product obtained by the precipitation reaction to obtain crude lithium phosphate;
[0029] The obtained solid is washed and dried to obtain the exchange intermediate.
[0030] The present invention also provides an adsorbent for air separation prepared by the preparation method described in the above technical scheme, wherein the silicon-aluminum ratio of the adsorbent for air separation is 1.9-2.1, the content of type A impurity crystals is ≤1%, the static nitrogen adsorption capacity (25°C, 760mmHg) is ≥1.29mmol / g, and the nitrogen-oxygen separation coefficient is ≥6.55.
[0031] The present invention also provides the air separation adsorbent described in the above technical solution for application in the field of PSA / VPSA air separation oxygen production.
[0032] The present invention provides a method for preparing an adsorbent for air separation, comprising the following steps:
[0033] The sodium-based or sodium-potassium-based X-type molecular sieve raw powder, kaolin, a molding aid and a first silicon source solution are mixed and kneaded to obtain a matrix material;
[0034] Drying and crushing the matrix material to obtain crushed powder;
[0035] Repeatedly mixing, kneading, drying and crushing the crushed powder with a second silicon source solution to obtain N-times crushed powder;
[0036] The N-th-time crushed powder is mixed with a third silicon source solution and then molded to obtain an intermediate;
[0037] The intermediate is subjected to a first drying and roasting to obtain a primary roasting intermediate containing amorphous metakaolin;
[0038] The primary calcined intermediate containing amorphous metakaolin is mixed with a silicon-containing alkaline aqueous solution for aging and crystallization, and the amorphous metakaolin is converted into an X-type molecular sieve to obtain a sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve;
[0039] The sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve is mixed with a lithium-ion-containing aqueous solution for ion exchange to obtain an exchange intermediate; the ion exchange is carried out in an exchange column: the sodium-based or sodium-potassium-based molecular sieve is loaded in the exchange column, and the lithium-ion-containing aqueous solution flows in from the lower part of the exchange column and flows out from the upper part;
[0040] The exchange intermediate is dried and calcined for a second time to obtain the adsorbent for air separation.
[0041] The present invention uses a single roasting to convert the inert kaolin used as a binder into reactive metakaolin, and then uses an alkali-containing silicon source solution to crystallize the metakaolin into a sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve, which becomes a component of the sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve, and then the obtained sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve is ion exchanged to prepare an adsorbent for air separation. That is, the present invention converts the binder kaolin into an X-type molecular sieve to prepare an adsorbent for air separation, thereby increasing the effective component content and nitrogen adsorption of the adsorbent. The results of the embodiment show that the silicon-aluminum ratio of the adsorbent for air separation prepared by the present invention is 1.9-2.1, the content of type A impurities is ≤1%, the static nitrogen adsorption capacity (25°C, 760mmHg) is ≥1.29mmol / g, and the nitrogen-oxygen separation coefficient is ≥6.55 (25°C, 760mmHg).
[0042] At the same time, repeated mixing, kneading, drying and crushing improve the pressure resistance of the adsorbent for air separation, and the countercurrent exchange in the ion exchange column improves the utilization rate of lithium ions.
[0043] Furthermore, the present invention can prepare a multi-stage porous air separation adsorbent by adding a pore-forming agent, thereby improving the separation performance of the adsorbent.
[0044] Furthermore, the present invention utilizes a precipitation method to treat crude lithium-containing exchange waste liquid, so that the water-soluble lithium salt is converted into crude lithium phosphate, thereby improving the utilization rate of lithium in the entire preparation method. The lithium phosphate content in the obtained by-product crude lithium phosphate is ≥92%, and the utilization rate of lithium in the entire preparation method is ≥96%. DETAILED DESCRIPTION
[0045] The present invention provides a method for preparing an adsorbent for air separation, comprising the following steps:
[0046] The sodium-based or sodium-potassium-based X-type molecular sieve raw powder, kaolin, a molding aid and a first silicon source solution are mixed and kneaded to obtain a matrix material;
[0047] Drying and crushing the matrix material to obtain crushed powder;
[0048] Repeatedly mixing, kneading, drying and crushing the crushed powder with a second silicon source solution to obtain N-times crushed powder;
[0049] The N-th-time crushed powder is mixed with a third silicon source solution and then molded to obtain an intermediate;
[0050] The intermediate is subjected to a first drying and roasting to obtain a primary roasting intermediate containing amorphous metakaolin;
[0051] The primary calcined intermediate containing amorphous metakaolin is mixed with a silicon-containing alkaline aqueous solution for aging and crystallization, and the amorphous metakaolin is converted into an X-type molecular sieve to obtain a sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve;
[0052] The sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve is mixed with a lithium-ion-containing aqueous solution for ion exchange to obtain an exchange intermediate; the ion exchange is carried out in an exchange column: the sodium-based or sodium-potassium-based molecular sieve is loaded in the exchange column, and the lithium-ion-containing aqueous solution flows in from the lower part of the exchange column and flows out from the upper part;
[0053] The exchange intermediate is dried and calcined for a second time to obtain the adsorbent for air separation.
[0054] The invention mixes sodium-based or sodium-potassium-based X-type molecular sieve raw powder, kaolin, a molding aid and a first silicon source solution and kneads them to obtain a matrix material.
[0055] In the present invention, the silicon source in the first silicon source solution preferably includes one or more of white carbon black, silica gel powder, sodium silicate and silica sol, and more preferably silica sol; the concentration of the silicon source in terms of SiO2 in the first silicon source solution is preferably 2.0 to 6.0 g / L, and more preferably 3.2 to 4.0 g / L;
[0056] In the present invention, the mass of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder is 90-95% of the total mass of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder and kaolin, based on dry weight; the proportion of inert kaolin is relatively small, which is beneficial to reducing the content of type A impurities in the sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve and improving the exchange degree. At the same time, the molding process can make the intermediate have a higher crushing resistance, ensuring that the finished product will not be pulverized when used; the silicon-aluminum ratio of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder is preferably 1.9-2.1, and more preferably 1. 95~2.1; the sodium-based or sodium-potassium-based X-type molecular sieve raw powder with a silicon-aluminum ratio in the above range has a higher nitrogen adsorption capacity; the D50 of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder is preferably 3.0~3.5μm; the D50 of the sodium-based or sodium-potassium-based X-type raw powder is selected to facilitate the diffusion of lithium ions into the crystal structure of the molecular sieve, thereby increasing the ion exchange rate of the molecular sieve, and will not cause the base material to be insufficiently compacted and difficult to form due to too small D50; the silicon-aluminum ratio of the kaolin is preferably 1.75~2.1, and more preferably 1.8~2.1.
[0057] In the present invention, the molding aid comprises tannin extract and / or pore former; the mass of the tannin extract is preferably 3-8‰ of the total mass of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder and the kaolin on a dry basis, more preferably 4-6‰;
[0058] The mass of the pore former is preferably 0.5-4% of the total mass of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder and the kaolin on a dry basis, more preferably 1.5-2.5%; the pore former preferably includes corn starch and / or wheat starch.
[0059] In the present invention, the shape of the matrix material preferably includes sphere or strip; the specification of the strip preferably includes 1 / 16 strip or 1 / 8 strip, and the water content of the matrix material is preferably 36-39wt%, and the water content also determines the amount of silicon source solution added.
[0060] After obtaining the matrix material, the present invention dries and crushes the matrix material to obtain crushed powder.
[0061] In the present invention, the water content of the crushed powder is preferably ≤12wt%, and the particle size is preferably <0.075mm.
[0062] After obtaining the crushed powder, the present invention repeatedly mixes, kneads, dries and crushes the crushed powder with the second silicon source solution to obtain N-times crushed powder.
[0063] In the present invention, the silicon source in the second silicon source solution preferably includes one or more of white carbon black, silica gel powder, sodium silicate and silica sol, and more preferably silica sol; the concentration of the silicon source in terms of SiO2 in the second silicon source solution is preferably 2.0 to 6.0 g / L, and more preferably 3.2 to 4.0 g / L;
[0064] In the present invention, N is the number of repetitions, preferably 2≤N≤5, the shape of the matrix material kneaded in each repetition process preferably includes spherical or bar shapes independently; the specifications of the bar shape preferably include 1 / 16 bar or 1 / 8 bar, the water content of the matrix material kneaded in each repetition process preferably independently is 36-39wt%; the water content of the crushed powder obtained by crushing in each repetition process preferably independently is ≤12wt%, and the particle size of the crushed powder obtained by crushing in each repetition process independently is <0.075mm. Repeated kneading, drying and crushing can improve the compactness of the matrix material, and the intermediate after molding has a higher crushing resistance.
[0065] After obtaining the N-times crushed powder, the present invention mixes the N-times crushed powder with the third silicon source solution and then shapes it to obtain the intermediate.
[0066] In the present invention, the silicon source in the third silicon source solution preferably includes one or more of white carbon black, silica gel powder, sodium silicate and silica sol, and is more preferably silica sol; the concentration of the silicon source in terms of SiO2 in the third silicon source solution is preferably 2.0 to 6.0 g / L, and more preferably 3.2 to 4.0 g / L.
[0067] In the present invention, the shape of the intermediate preferably includes a spherical shape or a bar shape.
[0068] In the present invention, the water content of the intermediate is preferably 36-42wt%, more preferably 38-40wt%. The water content of the intermediate can determine the amount of silicon source solution added; the spherical specification is preferably φ0.4-2.5mm, and the strip specification is preferably 1 / 16 or 1 / 8.
[0069] After the intermediate is obtained, the present invention performs a first drying and roasting on the intermediate to obtain a primary roasted intermediate containing amorphous metakaolin.
[0070] Before the primary calcined intermediate is mixed with the silicon-containing alkaline aqueous solution, the primary calcined intermediate is preferably soaked in water and then drained. The purpose of draining after soaking in water is that the primary calcined intermediate will release a lot of heat after soaking in water. If it is directly soaked in water in the crystallization column, the crystallization liquid will be severely heated, exceeding the aging and crystallization process temperature.
[0071] In the present invention, the first drying and roasting preferably includes sequentially performing a first drying and a first roasting;
[0072] The temperature of the first drying is preferably 80-200° C., more preferably 100-150° C., and the time is preferably 0.5-4 h, more preferably 1-2 h; the first drying fully removes the surface water in the intermediate.
[0073] The temperature of the first calcination is preferably 620-750° C., more preferably 660-700° C., and the time is preferably 0.5-4 h, more preferably 1-3 h.
[0074] When the intermediate contains a pore former, the pore former is removed during the first calcination process, and an intermediate containing multi-level pores is generated.
[0075] The kaolin added during the molding process will reduce the effective adsorption capacity of the unit mass of the adsorbent. After the first calcination treatment, the reaction-inert kaolin with a stable structure can be converted into amorphous reactive metakaolin. Within the range of the first calcination temperature and time of the present invention, the inert kaolin in the intermediate can be completely converted into active metakaolin.
[0076] After obtaining a primary calcined intermediate containing amorphous metakaolin, the present invention mixes the primary calcined intermediate containing amorphous metakaolin with a silicon-containing alkaline aqueous solution for aging and crystallization, converting the amorphous metakaolin into a sodium-based or sodium-potassium-based X-type molecular sieve to obtain a sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve.
[0077] In the present invention, the aging and crystallization are preferably performed in a crystallization column: the primary calcined intermediate is loaded in the crystallization column, and the silicon-containing alkaline aqueous solution cyclically flows in from the lower part and out from the upper part of the crystallization column.
[0078] The volume ratio of the mass of the primary calcined intermediate to the silicon-containing alkaline aqueous solution on a dry basis is preferably 1 kg: 2.2 to 3 L, more preferably 1 kg: 2.5 to 2.8 L;
[0079] The OH in the silicon-containing alkaline aqueous solution - The concentration of OH is preferably 2.26 to 2.90 mol / L, more preferably 2.58 to 2.75 mol / L; - Preferably from KOH and / or NaOH;
[0080] The concentration of the silicon source in the silicon-containing alkaline aqueous solution calculated as SiO2 is preferably 5-19 g / L, more preferably 8-14 g / L; the silicon source preferably includes one or more of white carbon black, silica gel powder, sodium silicate and silica sol, more preferably silica sol.
[0081] In the present invention, the aging temperature is preferably 50 to 70°C, more preferably 55 to 65°C; the time is preferably 1 to 4 hours, more preferably 2 to 3 hours; during the aging, the flow rate of the silicon-containing alkaline aqueous solution is preferably 1 to 4 m / s. 3 / h, more preferably 2.0 to 3.5 m 3 / h; the present invention obtains crystal nuclei with suitable particle size by controlling the aging time, thereby improving the performance of the product.
[0082] In the present invention, the crystallization temperature is preferably 90 to 100°C, more preferably 94 to 98°C; the time is preferably 3.5 to 7 hours, more preferably 4 to 6 hours; during the crystallization, the flow rate of the silicon-containing alkaline aqueous solution is preferably 1 to 4 m / s. 3 / h, more preferably 2.0 to 3.5 m 3 / h.
[0083] The silicon-containing alkaline aqueous solution cyclically flows in from the lower part and out from the upper part of the crystallization column, which is beneficial to the conversion of metakaolin into X-type molecular sieve, while ensuring the uniformity and consistency of the content of type A impurity crystals in the sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve (the nitrogen adsorption amount of type A impurity crystals is relatively low).
[0084] The alkaline source in the silicon-containing alkaline aqueous solution provides an alkaline environment for aging and crystallization, and can also make up for the deficiency that the activated kaolin cannot be converted into a molecular sieve due to the lack of Na2O in the activated kaolin. The silicon source can make up for the deficiency that the activated kaolin cannot be converted into an X-type molecular sieve due to the low silicon source content in the activated kaolin, thereby reducing the content of impure crystals, so that the content of type A impure crystals in the sodium-based or sodium-potassium-based X fully crystalline molecular sieve is ≤1%;
[0085] The aging step forms crystal nuclei in the activated kaolin, and the crystallization step gradually grows the crystal nuclei into sodium-based or sodium-potassium-based X-type molecular sieves with a certain grain size and silicon-aluminum ratio;
[0086] In the countercurrent circulation process (the silicon-containing alkaline aqueous solution cyclically flows in from the lower part of the crystallization column and flows out from the upper part), the silicon-containing alkaline aqueous solution can flow fully, which can ensure the uniformity of the silicon-containing alkaline aqueous solution, and can make the first calcined intermediate fully and evenly contact with the silicon-containing alkaline aqueous solution, thereby ensuring the uniformity and consistency of the impurity crystal content of the sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve.
[0087] After the crystallization, the present invention preferably separates the obtained product, and then washes the separated solid to obtain the sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve;
[0088] In the present invention, the waste liquid obtained by separation is preferably recycled into the preparation of the silicon-containing alkaline aqueous solution.
[0089] After obtaining the sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve, the present invention mixes the sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve with a lithium ion-containing aqueous solution to perform ion exchange to obtain an exchange intermediate.
[0090] In the present invention, the ion exchange is preferably carried out in an exchange column: the sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve is loaded in the exchange column, and the lithium ion-containing aqueous solution preferably flows in from the lower part and out from the upper part of the exchange column.
[0091] In the present invention, the ion exchange is preferably a mobile serial exchange.
[0092] In the present invention, the total number of exchange columns in the mobile serial exchange is preferably 10 to 18, more preferably 14 to 18; each exchange column in the mobile serial exchange system is filled with a sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve.
[0093] The mobile serial exchange preferably includes: when the concentration of the lithium ion-containing aqueous solution flowing out of the last exchange column in the exchange column undergoing ion exchange is 20-40% of the concentration of the lithium ion-containing aqueous solution flowing in, the next single column is connected. The outlet of the last exchange column in the exchange column undergoing ion exchange is connected to the inlet of the next single column.
[0094] When the Li of the sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve in the ion exchange column is + When the exchange degree is ≥98.5%, the present invention preferably washes the exchange column and then refills it with sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve, and then connects the exchange column refilled with sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve when the concentration of the lithium ion-containing aqueous solution flowing out of the last exchange column in the exchange column undergoing ion exchange is 20-40% of the concentration of the lithium ion-containing aqueous solution flowing in.
[0095] In the present invention, the initial number of the exchange columns undergoing ion exchange is preferably one.
[0096] The mobile series exchange process reduces the cumulative effect of sodium ions and potassium ions and speeds up the exchange rate.
[0097] In the present invention, the concentration of lithium ions in the lithium ion-containing aqueous solution is preferably 0.35 to 2.5 mol / L, more preferably 0.4 to 1.0 mol / L; the pH of the lithium ion-containing aqueous solution is preferably 8 to 12, more preferably 9 to 11;
[0098] In the present invention, the lithium ion-containing aqueous solution is preferably obtained by reacting lithium hydroxide and / or a lithium salt with an inorganic acid.
[0099] In the present invention, the lithium salt preferably includes lithium carbonate; the inorganic acid preferably includes one or more of hydrochloric acid, sulfuric acid and nitric acid.
[0100] In the present invention, during the mobile serial exchange, the temperature of the ion exchange is preferably independently 90 to 100° C., more preferably 95 to 98° C.; during the ion exchange, the lithium ion-containing aqueous solution is preferably heated to the ion exchange temperature.
[0101] During mobile serial exchange, the flow rate of the aqueous solution containing lithium ions is preferably 0.5 to 3 m 3 / h, more preferably 2.0 to 2.5 m 3 / h.
[0102] The present invention has no particular limitation on the time of the ion exchange, as long as the Li + The exchange degree should be ≥ 98.5%. In ion exchange, lithium ions are exchanged with sodium ions and potassium ions. The exchange degree is the molar amount of lithium ions / the total molar amount of (lithium ions, sodium ions and potassium ions)*100%.
[0103] In the present invention, after the ion exchange, the process preferably further comprises: separating the product obtained by the ion exchange, centrifuging the obtained waste liquid and first mixing it with an alkaline solution, and then mixing it with a precipitant to perform a precipitation reaction, and then filtering and drying the product obtained by the precipitation reaction to obtain crude lithium phosphate;
[0104] The obtained solid is washed and dried to obtain the exchange intermediate.
[0105] In the present invention, the pH value of the solution obtained by mixing the waste liquid with the alkali solution after centrifugation is preferably ≥9, more preferably ≥10; the alkali solution preferably includes sodium hydroxide solution and / or potassium hydroxide solution;
[0106] In the present invention, mixing with a precipitant preferably comprises: adding the precipitant to the solution obtained by mixing the waste liquid with an alkali solution after centrifugation of the waste liquid in multiple portions;
[0107] The temperature of mixing with the precipitant is preferably 60-95°C, more preferably 75-95°C; the precipitant preferably includes one or more of Na3PO4·12H2O, Na2HPO4·12H2O, NaH2PO4·2H2O, K3PO4, soluble phosphates and phosphoric acid; the precipitant PO4 3- The molar amount is preferably Li in the waste liquid after centrifugation + 0.35 to 0.60 times the molar amount, more preferably 0.43 to 0.46 times;
[0108] The temperature of the precipitation reaction is preferably 60 to 95° C., more preferably 75 to 95° C.; the time is preferably 1 to 6 hours, more preferably 4 to 6 hours.
[0109] In the present invention, the detergent used for washing preferably includes deionized water.
[0110] In the present invention, the second drying and roasting preferably includes sequentially performing a second drying and a second roasting;
[0111] The temperature of the second drying is preferably 50 to 200° C., more preferably 80 to 150° C., and further preferably 100 to 120° C.; the time is preferably 1 to 2 hours, and more preferably 1.5 to 1.8 hours.
[0112] The temperature of the second calcination is preferably 350-520°C, more preferably 400-500°C, and further preferably 450-480°C; the time is preferably 3-8h, more preferably 4-5h; the rate of heating to the second calcination temperature is preferably 5-15°C / min, more preferably 10°C / min. The second drying calcination can remove surface water and crystal water, so that the adsorbent has adsorption properties.
[0113] After the second drying and calcining, the present invention preferably cools the obtained high-temperature air separation adsorbent to obtain the air separation adsorbent.
[0114] The present invention also provides an adsorbent for air separation prepared by the preparation method described in the above technical scheme, wherein the silicon-aluminum ratio of the adsorbent for air separation is 1.9-2.1, the content of type A impurity crystals is ≤1%, the static nitrogen adsorption capacity (25°C, 760mmHg) is ≥1.29mmol / g, and the nitrogen-oxygen separation coefficient is ≥6.55 (25°C, 760mmHg).
[0115] The present invention also provides the adsorbent for air separation described in the above technical solution for application in the field of PSA / VPSA air separation oxygen production.
[0116] The air separation adsorbent provided by the present invention, its preparation method and application are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0117] Example 1
[0118] (1) 40 kg of sodium-based X-type molecular sieve raw powder (silicon-aluminum ratio of 2.05, D50 of 3.2 μm), 3.5 kg of kaolin (silicon-aluminum ratio of 1.95), 0.17 kg of molding auxiliary agent tannin extract, and 0.7 kg of pore-forming agent corn starch were mixed with a molding liquid (the SiO2 content in the molding liquid was 3.5 g / L, and the silicon source was silica sol) and kneaded to extrude 1 / 8 of the matrix material (the moisture content of the matrix material was 37%). The matrix material was dried and crushed to obtain a primary crushed powder (the moisture content of the crushed powder was 6%, and the particle size was ≤0.065 mm). , knead the primary crushed powder and the molding liquid (the SiO2 content in the molding liquid is 3.5g / L, and the silicon source is silica sol) into 1 / 8 strips (the moisture content of the matrix material is 38%), and dry and crush the matrix material again to obtain the secondary crushed powder (the moisture content of the crushed powder is 8%, and the particle size is ≤0.065mm); add the secondary crushed powder and the molding solution (the SiO2 content is 3.5g / L, and the silicon source is silica sol) into the ball-forming equipment, roll into balls, and sieve out 2.5kg of the intermediate product with a diameter of φ1.0-2.0mm and a moisture content of 37wt%.
[0119] (2) 2.5 kg of the dry intermediate was dried at 150°C for 1 h and then calcined in a muffle furnace at 720°C for 1.5 h to obtain a primary calcined intermediate.
[0120] (3) After immersing 2 kg of the dry primary calcined intermediate in water and draining, the intermediate was immersed in a crystallization column containing 5.5 L of a silicon-containing alkaline aqueous solution (NaOH content of 2.7 mol / L, SiO2 content of 10.5 g / L) and then heated at a flow rate of 3 m / s. 3 / h, countercurrent circulation crystallization at 62 ° C for 2 h, and then at a flow rate of 3m 3 / h, countercurrent circulation crystallization at 95°C for 5h, and washing with water until the pH of the washing liquid is 10.8 to obtain a sodium-based fully crystalline X-type molecular sieve.
[0121] (4) 1.5 kg of dry sodium-based fully crystalline X-type molecular sieve was immersed in the exchange column and Li + A 2 mol / L lithium ion aqueous solution (made from analytical pure hydrochloric acid HCl and battery grade lithium hydroxide monohydrate LiOH·H2O, pH=11) was stirred at a flow rate of 2 m 3 / h, countercurrent exchange was carried out at a temperature of 98°C. When the waste liquid Li + When the content is 0.7mol / L, the outlet of the exchange column is connected to the inlet of the next exchange column. When the concentration of the lithium ion aqueous solution flowing out of the series exchange system in which ion exchange is being performed is 0.7mol / L, the next single column is connected to form a new mobile series exchange system until the number of exchange columns reaches 13. When the material Li on the upper part of the exchange column is +When the exchange degree is ≥99%, the exchange intermediate is obtained by washing with deionized water at room temperature after separation.
[0122] (5) The exchange intermediate was placed in an oven and dried at 120°C for 1 h. Then, an in-situ degassing / dehydration treatment was performed using a degassing activation device equipped on a Micromeritics ASAP 3020 adsorption instrument. The dried exchange intermediate was heated to 350°C and kept warm for 6 h. The heating rate was set to 10°C / min. The activated sample was naturally cooled to room temperature in a dryer to obtain an adsorbent for air separation. The silicon-aluminum ratio (SiO2 / Al2O3) was 2.03, the static nitrogen adsorption capacity (25°C, 760 mmHg) was 1.32 mmol / g, the A-type impurity crystal content was 0.6%, and the nitrogen-oxygen separation coefficient was 6.66 (25°C, 760 mmHg).
[0123] (6) The crude lithium-containing waste liquid after exchange is centrifuged to obtain a refined lithium-containing waste liquid, and Li + The content is 0.94mol / L. First, 500ml of refined lithium-containing waste liquid is placed in a 1L beaker, a small amount of NaOH is added to adjust the pH to 10.5, and then the beaker is placed in a water bath and heated to 80°C, and then 80g of trisodium phosphate dodecahydrate (Na3PO4·12H2O) is added while stirring, and after Na3PO4·12H2O is completely dissolved, it is allowed to stand for 4 hours at 80°C and then filtered to obtain solid crude lithium phosphate. The lithium phosphate content is measured to be 94.6wt%, and the lithium utilization rate in the entire molecular sieve preparation process (lithium exchange and treatment of lithium-containing waste liquid) is 97.1%.
[0124] Example 2
[0125] The adsorbent for air separation is prepared and lithium recovery treatment is performed in lithium-containing waste liquid according to the method in Example 1, except that:
[0126] In step (3), the silicon-containing alkaline aqueous solution (NaOH content is 2.4 mol / L, SiO2 content is 9.4 g / L);
[0127] In step (4), the fresh lithium ion aqueous solution Li + The content is 1.6 mol / L, and the exchange temperature is 94°C;
[0128] The adsorbent for air separation in step (5) has a silicon-to-aluminum ratio (SiO2 / Al2O3) of 2.05, a static nitrogen adsorption capacity (25°C, 760 mmHg) of 1.29 mmol / g, an A-type impurity crystal content of 0.8%, and a nitrogen-oxygen separation coefficient of 6.65 (25°C, 760 mmHg);
[0129] Step (6) +The content is 0.72 mol / L, the pH is adjusted to 9.4 using KOH, the lithium phosphate content is 93.5wt%, and the lithium utilization rate in the entire molecular sieve preparation process (lithium exchange and treatment of lithium-containing waste liquid) is 96.5%.
[0130] Example 3
[0131] The adsorbent for air separation is prepared and lithium recovery treatment is performed in lithium-containing waste liquid according to the method in Example 1, except that:
[0132] In step (3), the silicon-containing alkaline aqueous solution (KOH content is 2.3 mol / L, SiO2 content is 9.8 g / L), the crystallization temperature is 92° C., and the crystallization time is 4 h;
[0133] In step (4), the fresh lithium ion aqueous solution Li + The content is 2.3 mol / L, and the exchange temperature is 98°C;
[0134] The adsorbent for air separation in step (5) has a silicon-to-aluminum ratio (SiO2 / Al2O3) of 2.01, a static nitrogen adsorption capacity (25°C, 760 mmHg) of 1.30 mmol / g, a type A impurity crystal content of 0.5%, and a nitrogen-oxygen separation coefficient of 6.64 (25°C, 760 mmHg);
[0135] Step (6) + The content is 1.1 mol / L, the pH is adjusted to 9.5 using NaOH, the lithium phosphate content is 94.4wt%, and the lithium utilization rate in the entire molecular sieve preparation process (lithium exchange and treatment of lithium-containing waste liquid) is 98.5%.
[0136] Comparative Example 1
[0137] A primary calcined intermediate was prepared according to steps (1) and (2) in Example 1;
[0138] (3) The once calcined intermediate is not subjected to step (3) in Example 1, but is directly prepared into an adsorbent for air separation according to the methods of steps (4) and (5) in Example 1, and lithium is recovered from lithium-containing waste liquid according to the method of step (6).
[0139] Comparative Example 2
[0140] The method of steps (1) to (6) in Example 1 is used to prepare an adsorbent for air separation and to recover lithium from lithium-containing waste liquid. The difference from Example 1 is that:
[0141] In step (1), the molding liquid is deionized water;
[0142] Step (3) Silicon-containing alkaline aqueous solution (NaOH content 2.7 mol / L, SiO2 content 0 g / L)
[0143] An adsorbent for air separation was obtained, which had a silicon-to-aluminum ratio (SiO2 / Al2O3) of 2.02, a nitrogen adsorption capacity (25°C, 760 mmHg) of 1.19 mmol / g, a type A impurity crystal content of 2.4%, and a nitrogen-oxygen separation coefficient of 6.32 (25°C, 760 mmHg).
[0144] Comparative Example 3
[0145] The method of steps (1) to (6) in Example 1 is used to prepare an adsorbent for air separation and to recover lithium from lithium-containing waste liquid. The difference from Example 1 is that:
[0146] The number of drying and crushing in step (1) is 1 time.
[0147] Comparative Example 4
[0148] An adsorbent for air separation was prepared according to the method of steps (1) to (5) in Example 1.
[0149] The crude lithium-containing waste liquid after exchange was centrifuged to obtain the refined lithium-containing waste liquid, and Li + The content is 0.94mol / L. First, 500ml of refined lithium-containing waste liquid is placed in a 1L beaker, a small amount of NaOH is added to adjust the pH to 8.5, and then the beaker is placed in a water bath and heated to 55°C, and then 60g of trisodium phosphate dodecahydrate (Na3PO4·12H2O) is added while stirring, and after Na3PO4·12H2O is completely dissolved, it is allowed to stand for 4 hours at 55°C and then filtered to obtain solid crude lithium phosphate. The lithium phosphate content is measured to be 94.2wt%, and the lithium utilization rate in the entire adsorbent preparation process (lithium exchange and treatment of lithium-containing waste liquid) is 80.5%.
[0150] The crushing resistance of the molecular sieves prepared in Examples 1 to 3 and Comparative Examples 1 to 4 was analyzed using an intelligent particle strength tester. The results are shown in Table 1.
[0151] The content of type A impurity crystals in the molecular sieves prepared in Examples 1 to 3 and Comparative Examples 1 to 4 was analyzed by X-ray diffractometer. The results are shown in Table 1.
[0152] The static nitrogen adsorption (25° C., 760 mmHg) of the molecular sieves prepared in Examples 1 to 3 and Comparative Examples 1 to 4 was analyzed using a Micromeritics adsorption instrument. The results are shown in Table 1.
[0153] Table 1 Summary of the results of determination of the main indicators of the molecular sieves prepared in Examples 1 to 3 and Comparative Examples 1 to 4
[0154]
[0155] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an adsorbent for air separation, characterized in that: The following steps are involved: The sodium-based or sodium-potassium-based X-type molecular sieve raw powder, kaolin, a molding aid and a first silicon source solution are mixed and kneaded to obtain a matrix material; Drying and crushing the matrix material to obtain crushed powder; Repeatedly mixing, kneading, drying and crushing the crushed powder with a second silicon source solution to obtain N-times crushed powder; The N-th-time crushed powder is mixed with a third silicon source solution and then molded to obtain an intermediate; The intermediate is subjected to a first drying and roasting to obtain a primary roasting intermediate containing amorphous metakaolin; The primary calcined intermediate containing amorphous metakaolin is mixed with a silicon-containing alkaline aqueous solution for aging and crystallization, and the amorphous metakaolin is converted into an X-type molecular sieve to obtain a sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve; The sodium-based or sodium-potassium-based fully crystalline X-type molecular sieve is mixed with a lithium-ion-containing aqueous solution for ion exchange to obtain an exchange intermediate; the ion exchange is carried out in an exchange column: the sodium-based or sodium-potassium-based molecular sieve is loaded in the exchange column, and the lithium-ion-containing aqueous solution flows in from the lower part of the exchange column and flows out from the upper part; The exchange intermediate is dried and calcined for a second time to obtain the adsorbent for air separation.
2. The preparation method according to claim 1, characterized in that: The silicon-aluminum ratio of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder is 1.9 to 2.1; The silicon-aluminum ratio of the kaolin is 1.75-2.
1.
3. The preparation method according to claim 1 or 2, characterized in that: Based on dry weight, the mass of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder is 90-95% of the total mass of the sodium-based or sodium-potassium-based X-type molecular sieve raw powder and kaolin.
4. The preparation method according to claim 1, characterized in that: The molding aid comprises tannin extract and pore-forming agent.
5. The preparation method according to claim 1, characterized in that: The water content of the matrix material and the matrix material obtained by kneading in each repeated process is independently 36 to 39 wt %; The water content of the crushed powder and the crushed powder obtained in each repeated crushing process is independently ≤12wt%; The water content of the intermediate is 36-42 wt%.
6. The preparation method according to claim 1, characterized in that: The volume ratio of the mass of the primary calcined intermediate on a dry basis to the silicon-containing alkaline aqueous solution is 1 kg: 2.2 to 3 L; The OH in the silicon-containing alkaline aqueous solution - The concentration of is 2.26-2.90 mol / L, and the concentration of silicon source calculated as SiO2 is 5-19 g / L; The aging and crystallization are carried out in a crystallization column: the primary calcined intermediate is loaded in the crystallization column, and the silicon-containing alkaline aqueous solution cyclically flows in from the lower part and out from the upper part of the crystallization column.
7. The preparation method according to claim 1, characterized in that: The concentration of lithium ions in the lithium ion-containing aqueous solution is 0.35 to 2.5 mol / L, and the pH of the lithium ion-containing aqueous solution is 8 to 12; The temperature of the ion exchange is 90-100°C; The flow rate of the lithium ion aqueous solution is 0.5 to 3 m 3 / h.
8. The preparation method according to claim 1 or 7, characterized in that: After the ion exchange, the method further includes: separating the product obtained by the ion exchange, centrifuging the obtained waste liquid, mixing it with an alkali solution, and then mixing it with a precipitant to perform a precipitation reaction, and then filtering and drying the product obtained by the precipitation reaction to obtain crude lithium phosphate; The obtained solid is washed and dried to obtain the exchange intermediate.
9. The air separation adsorbent prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The silicon-aluminum ratio of the air separation adsorbent is 1.9-2.1, the content of type A impurity crystals is ≤1%, the static nitrogen adsorption capacity (25°C, 760mmHg) is ≥1.29mmol / g, and the nitrogen-oxygen separation coefficient is ≥6.
55.
10. The air separation adsorbent according to claim 9 is used in the field of PSA / VPSA air separation oxygen production.