Zinc oxide / polyacid nano composite material for producing hydrogen peroxide through photocatalysis and preparation method of zinc oxide / polyacid nano composite material

Preparation of zinc oxide/polyacid nanocomposites by hydrothermal-calcination method, solving the shortcomings of existing photocatalysts in ZnO particle size and morphology control, and achieving high-efficiency photocatalytic hydrogen peroxide production and good cycle stability .

CN119016040AActive Publication Date: 2024-11-26LIAONING NORMAL UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411321054.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-26
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

When existing photocatalysts produce hydrogen peroxide, it is difficult to accurately control the size and morphology of ZnO particles, resulting in limited photocatalytic performance and the polyoxygenate is not combined with nano ZnO for photocatalytic hydrogen peroxide production.

Method used

The zinc oxide/polyacid nanocomposite was prepared by hydrothermal calcining method, and ZnO powder was prepared by hot bath stirring and warming of muffle furnace, and hydrothermal impregnation with polymetallic acid salt to form uniform morphology Phase-pure zinc oxide/polyacid nanocomposites optimize crystal growth and photochemical activity.

Benefits of technology

The optimal control of ZnO size and morphology is achieved, the photocatalytic activity is improved, the photogenesis and transfer rate is promoted, and the hydrogen peroxide yield of 700 μM per hour and excellent cycling stability is obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016040A_ABST
    Figure CN119016040A_ABST
Patent Text Reader

Abstract

The invention discloses a zinc oxide / polyacid nano composite material for photocatalytic production of hydrogen peroxide and a preparation method thereof, a hydrothermal-calcination method is adopted to prepare a ZnO nano material with uniform size, and the ZnO nano material and POMs are compounded through hydrothermal dipping to obtain the zinc oxide / polyacid nano composite material with uniform product morphology and pure phase. In the preparation process, the influence of polyacid on the growth of ZnO crystals can be optimized under the conditions of specific reaction temperature, reactant mass ratio and the like, so that the optimal control on the size and morphology of ZnO is realized; meanwhile, through a hydrothermal-calcining-hot bath dipping synthesis process, the synthesized composite material can make up the defects of nano-zinc oxide, introduce more photochemical active sites, effectively reduce electron-hole recombination, accelerate the generation and transfer rate of photo-induced electrons and promote the catalytic activity of the zinc oxide nano-material; the hydrogen peroxide yield of 700 [mu] M per hour and excellent cycling stability are obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation and photocatalytic hydrogen peroxide production, and in particular to a zinc oxide / polyacid nanocomposite material for photocatalytic hydrogen peroxide production and a preparation method thereof. Background Art

[0002] Hydrogen peroxide (H2O2) is a multifunctional green catalyst that has been widely used in the fields of pharmaceutical disinfection, environmental remediation, chemical synthesis and automotive batteries. Traditionally, hydrogen peroxide is produced by the anthraquinone method (AQ), which has limitations such as environmental pollution, high energy consumption and low economic benefits, and is not in line with the country's current sustainable development strategy. Therefore, photocatalytic generation of hydrogen peroxide has received widespread attention as a green and sustainable production method.

[0003] Photocatalytic generation of hydrogen peroxide mainly utilizes the electrons and holes generated by photocatalysts under light conditions to react with oxygen and water to generate hydrogen peroxide. Currently reported photocatalysts include metal oxides such as TiO2 and ZnO, carbon nitride (g-C3N4), covalent organic frameworks (COFs), etc. Among them, ZnO has attracted the attention of the industry due to its low cost, high stability, and high carrier distribution efficiency. Existing methods for synthesizing ZnO include sol-gel method, hydrothermal method, and vapor deposition method, all of which cannot accurately control the size and morphology of ZnO particles, and it is difficult to achieve the regulation of crystal surface active sites, resulting in limited photocatalytic performance.

[0004] Polyoxometalates (POMs) are widely used in the field of photoelectrocatalysis due to their unique redox activity, excellent photochemical activity, reversible multi-electron transfer ability, good chemical stability and adjustable ability. However, to date, there has been no report on the composite of polyoxometalates with nano-ZnO to prepare zinc oxide / polyoxometalates nanocomposites and their application in photocatalytic production of hydrogen peroxide. Summary of the invention

[0005] The present invention aims to solve the above technical problems existing in the prior art and provides a zinc oxide / polyacid nanocomposite material for photocatalytic production of hydrogen peroxide and a preparation method thereof.

[0006] The technical solution of the present invention is: a zinc oxide / polyacid nanocomposite material for photocatalytic hydrogen peroxide production is prepared by placing ZnO powder and polyoxometalate in deionized water and stirring them in a hot bath, and the morphology is cotton-like and the size is 30-130 nm.

[0007] A method for preparing the above-mentioned zinc oxide / polyacid nanocomposite material for photocatalytic production of hydrogen peroxide is carried out in the following steps: Step 1. Dissolve zinc salt and ammonium salt in deionized water at a mass ratio of 0.5-30:1 to form a mixed solution, heat the mixed solution in a 40-100°C hot bath and stir, then transfer the mixed solution to an autoclave and heat at 90-180°C for 4-36 h, wash and dry the reaction product, place it in a muffle furnace and heat it to 300-900°C at a heating rate of 5°C / min and keep it for 1-5 h to obtain white ZnO powder; Step 2. Put ZnO powder and polyoxometalate in a mass ratio of 1:0.25-40 into deionized water and stir in a hot bath at 50-100°C to obtain a composite material POMs@ZnO.

[0008] The preferred technical solution is that the zinc salt is zinc sulfate or zinc sulfide, the ammonium salt is ammonium chloride or ammonium carbonate, and the polyoxometalate is tungstoboric acid (BW 12 ), tungstosilicic acid (SiW 12 ) or tungstophosphoric acid (PW 12 ).

[0009] A further preferred technical solution is that the zinc salt is zinc sulfate, the ammonium salt is ammonium carbonate, and the polyoxometalate is BW 12 The mass ratio of the ZnO powder to the polyoxometalate is 1:1.

[0010] The invention adopts a hydrothermal-calcination method to prepare a ZnO nanomaterial with uniform size, and composites the ZnO nanomaterial with POMs through hydrothermal impregnation, so as to obtain a zinc oxide / polyacid nanocomposite material with uniform morphology and pure phase. The specific reaction temperature and reactant mass ratio and other conditions in the preparation process of the invention can optimize the effect of polyacid on ZnO crystal growth, thereby achieving the best control of ZnO size and morphology; at the same time, through the synthesis process of hydrothermal-calcination-hot bath impregnation, the synthesized composite material can make up for the defects of nano zinc oxide, introduce more photochemical active sites, and effectively reduce electron-hole recombination, accelerate the generation and transfer rate of photogenerated electrons, promote the catalytic activity of zinc oxide nanomaterials, and obtain a hydrogen peroxide yield of 700 μM per hour and excellent cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 The ZnO and BW of the present invention are 12 @SEM image of ZnO.

[0012] Figure 2 The ZnO and BW of the present invention are 12 , BW 12 Fourier transform infrared spectrum of @ZnO and 400 -1800 cm -1 A partial enlarged view of .

[0013] Figure 3 The ZnO and BW of the present invention are 12 , BW 12 @XRD pattern of ZnO.

[0014] Figure 4 The ZnO and BW of the present invention are 12 @ZnO, BW 12 , 0.5BW 12 @ZnO, 2BW 12 @Yield diagram of H2O2 produced by photocatalysis of ZnO.

[0015] Figure 5 This is an embodiment of the present invention. 12 @ZnO photocatalytic hydrogen peroxide production cycle test diagram. DETAILED DESCRIPTION

[0016] All raw materials in the examples of the present invention are not particularly limited in their sources and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0017] There is no particular limitation on the purity of all raw materials in the examples of the present invention, and analytically pure materials are preferably used in the present invention.

[0018] To make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention. Example 1

[0019] The preparation method of the zinc oxide / polyacid nanocomposite material for photocatalytic hydrogen peroxide production of the present invention is carried out in the following steps: Step 1. Dissolve 2.87 g ZnSO4·7H2O and 0.567 g (NH4)2·CO3 in deionized water to form a mixed solution, stir the mixed solution in a 40°C hot bath for 30 min, transfer it to a polytetrafluoroethylene liner while hot and seal it in an autoclave, then place it in an oven and heat it at 100°C for 5 h, wash the reaction product, dry it at 60°C, place it in a muffle furnace, heat it to 700°C at a heating rate of 5°C / min, and hold it for 2 h to obtain white ZnO powder; Step 2. Mix ZnO powder with BW 12 The mixture was placed in 30 mL of deionized water at a mass ratio of 1:1 and stirred at 80 °C for 24 h to obtain BW 12 @ZnO; Polyacid used BW 12 (K5BW 12 O 40 xH2O) was prepared by the following method: Dissolve 100 g Na2WO4·2H2O and 5 g H3BO3 in 100 mL water, stir vigorously, add 60 mL 6 mol / L HCl solution, the pH of the mixed solution is 6, boil for several hours and add water continuously to remove solid Na 10 W 12 O 41 ·xH2O (byproduct) was filtered off, the filtrate was acidified to pH = 2 with 6 mol / L HCl solution and boiled for half an hour, 20 g of solid KCl was added to obtain a white precipitate, which was washed with ether to obtain 71 g of crude product, which was recrystallized in 50 mL of 60 ℃ aqueous solution with a yield of 57 g.

[0020] ZnO and BW prepared in Example 1 12 @ZnO SEM picture Figure 1 As shown in a and b, through Figure 1 a ZnO nanomaterials with uniform size can be observed. Figure 1 b It can be seen that after ZnO is loaded with polyacid, its morphology changes from granular to cotton-like, with a size of 30-130 nm, indicating that BW 12 It plays a role in morphology regulation in the entire synthesis process.

[0021] ZnO, BW in Example 1 12 , BW 12 Fourier transform infrared spectrum of @ZnO and 400 -1800 cm -1 A partial enlarged picture of Figure 2 As shown in a and b. Figure 2 It can be seen that in BW 12 @ZnO belongs to BW 12 The characteristic absorption peak of BW still exists and shifts significantly. 12 Successfully loaded onto the ZnO surface and tightly bonded.

[0022] ZnO, BW in Example 1 12 , BW 12 @XRD pattern of ZnO Figure 3 Compared with the Jade database ZnO-PDF #99-0111, it can be seen that the XRD characteristic peaks of the synthesized sample correspond to the standard card of ZnO, indicating the successful synthesis of ZnO and the loading BW 12 The diffraction peak curve of the original ZnO at 2 θ = 10 ~ 15° No BW 12 diffraction peaks, but in BW 12 @The diffraction peak belonging to ZnO in ZnO is enhanced, indicating that BW 12 Dispersed evenly on ZnO and loaded with BW12 The ZnO did not change the original crystal shape of the sample, which is consistent with the infrared results. Example 2

[0023] Steps 1 and 2 are the same as in Example 1, except that in step 3, ZnO powder and BW 12 According to the mass ratio of 1:2, 2BW is obtained. 12 @ZnO. Example 3

[0024] Steps 1 and 2 are the same as in Example 1, except that in step 3, ZnO powder and BW 12 According to the mass ratio of 1:0.5, 0.5BW is obtained. 12 @ZnO.

[0025] Comparative Example 1: ZnO prepared in Examples 1-3 of the present invention.

[0026] Comparative Example 2: The polyacid BW used in Examples 1-3 of the present invention 12 (K5BW 12 O 40 ·xH2O).

[0027] Examples 1-3 of the present invention and comparative examples 1 and 2 were used as photocatalysts to perform photocatalytic synthesis of hydrogen peroxide in a quartz reactor. The specific operation was as follows: the quartz reactor was placed in an ice-water bath, and the reaction system was kept at about 10°C; 50 mg of the photocatalyst was dispersed in 90 mL of distilled water, 10 mL of ethanol was added as a hole sacrificial agent, and ultrasonic treatment was performed for 5 min; after 30 min of dark reaction, a 300 W xenon lamp (λ ≥ 320 nm) was used as the light source for the photocatalytic reaction, and O2 was kept flowing during the reaction. Samples were taken every 30 min and the concentration of H2O2 produced was determined by iodine titration. The yield of H2O2 produced by photocatalysis is shown in the figure below: Figure 4 The results show that: ZnO, BW 12 @ZnO, BW 12 , 0.5BW 12 @ZnO, 2BW 12 @ZnO Among the five materials, BW 12 @ZnO has the best photocatalytic performance for producing H2O2.

[0028] The cycle test diagram of the zinc oxide / polyacid nanocomposite material for photocatalytic production of hydrogen peroxide in Example 1 of the present invention is shown in FIG. Figure 5 As shown, after 5 hours, its H2O2 production dropped from the original 100% to 92.8%, indicating that it has good stability.

Claims

1. A zinc oxide / polyacid nanocomposite material for photocatalytic production of hydrogen peroxide, characterized in that: The method is prepared by placing ZnO powder and polyoxometalate into deionized water and stirring them in a hot bath. The method has a cotton-like morphology and a size of 30-130 nm.

2. A method for preparing the zinc oxide / polyacid nanocomposite material for photocatalytic hydrogen peroxide production as claimed in claim 1, characterized in that Follow the steps below: Step 1. Dissolve zinc salt and ammonium salt in deionized water at a mass ratio of 0.5-30:1 to form a mixed solution, heat the mixed solution in a 40-100°C hot bath and stir, then transfer the mixed solution to an autoclave and heat at 90-180°C for 4-36 h, wash and dry the reaction product, place it in a muffle furnace and heat it to 300-900°C at a heating rate of 5°C / min and keep it for 1-5 h to obtain white ZnO powder; Step 2. Put ZnO powder and polyoxometalate in a mass ratio of 1:0.25-40 into deionized water and stir in a hot bath at 50-100°C to obtain a composite material POMs@ZnO.

3. The method for preparing the zinc oxide / polyacid nanocomposite material for photocatalytic hydrogen peroxide production according to claim 2, characterized in that: The zinc salt is zinc sulfate or zinc sulfide, the ammonium salt is ammonium chloride or ammonium carbonate, and the polyoxometalate is tungstoboric acid, tungstosilicic acid or tungstophosphoric acid.

4. The method for preparing the zinc oxide / polyacid nanocomposite material for photocatalytic hydrogen peroxide production according to claim 2, characterized in that: The zinc salt is zinc sulfate, the ammonium salt is ammonium carbonate, and the polyoxometalate is BW 12 The mass ratio of the ZnO powder to the polyoxometalate is 1:1.

Citation Information

Patent Citations

  • Polyoxometallate-based oxide photocatalyst as well as preparation method and application thereof