Volatile organic compound catalytic oxidation catalyst as well as preparation method and application thereof

The alumina coating is prepared by self-propagation combustion method and impregnated with precious metals to form a polyatom polymer, which solves the problems of single applicability of existing catalysts and poor dispersion of active components, and achieves efficient catalytic oxidation of hydrocarbon VOCs, reducing precious metals Usage and cost.

CN119016042APending Publication Date: 2024-11-26CHINA ENERGY INVESTMENT CORP LTD +1

Patent Information

Application Number
CN202310597872.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing catalysts have relatively single applicability to volatile organic compounds (VOCs), especially for hydrocarbon VOCs, which is difficult to meet the needs of catalytic reactions of different VOCs, and the smooth surface of the honeycomb ceramic support leads to poor dispersion of the active components of the catalyst.

Method used

The alumina coating is prepared by self-propagation combustion method, and precious metal salts are impregnated thereon to form a polyatomic polymer, which improves the activity and thermal stability of the catalyst and meets the needs of catalytic reactions of different VOCs.

Benefits of technology

Highly efficient catalytic oxidation of hydrocarbon VOCs, especially methane and ethylene, is achieved, which reduces the amount of precious metals used, improves the thermal stability of the catalyst and the binding force of the carrier-active components, and reduces the cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016042A_ABST
    Figure CN119016042A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a volatile organic compound catalytic oxidation catalyst. The preparation method of the catalyst comprises the following steps: 1) preparing an aluminum oxide combustion liquid; dipping a cordierite matrix in the alumina combustion liquid, drying and calcining to obtain a cordierite matrix coated with an alumina coating; and 3) dipping the cordierite matrix coated with the aluminum oxide coating in a noble metal precursor solution to adsorb corresponding noble metal salt, taking out, drying, and further calcining to obtain the catalyst. The catalyst provided by the invention has high catalytic efficiency, and can meet the requirements of different VOCs catalytic reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmentally friendly catalytic materials, and mainly relates to a volatile organic compound catalytic oxidation catalyst, a preparation method and application thereof. Background Art

[0002] Volatile organic compounds (VOCs) are a general term for organic compounds with a melting point below room temperature and a boiling point below 200-260°C under standard atmospheric pressure, mainly including hydrocarbons, esters, alcohols, benzene series, etc. The anthropogenic sources of VOCs emissions mainly include fixed combustion sources, road mobile sources, industrial process sources, solvent use sources, etc. It is an important precursor of photochemical smog and is also recognized as one of the precursors of PM2.5. VOCs can irritate the human skin, respiratory and blood systems, affect the heart and nervous system, and can even cause cancer.

[0003] VOCs emission control technologies mainly include recovery technologies (absorption, condensation, membrane separation, etc.) and destruction technologies (combustion, plasma, photocatalysis, biodegradation, etc.). Among them, catalytic combustion (catalytic oxidation) in the combustion method is to oxidize VOCs into harmless carbon dioxide and water vapor with the help of catalysts at a lower temperature, which has the advantages of high efficiency, energy saving, and easy control.

[0004] Catalytic combustion catalysts are mostly supported catalysts. Loading the catalyst on a suitable carrier matrix can improve the dispersion of the active components and enhance the thermal stability of the catalyst. Cordierite honeycomb ceramics are ideal carriers for catalytic combustion due to their low thermal expansion coefficient, reduced bed pressure, high mass transfer efficiency, and small amplification effect. However, the specific surface area of ​​the honeycomb ceramic carrier itself is small (<1m 2 / g), the smooth surface makes it difficult to fix the active components of the catalyst, and the active components of the catalyst cannot be fully dispersed. A layer of active coating material with a large specific surface area must be coated to improve the dispersibility of the active components.

[0005] CN105709719 A discloses an integral low-temperature SCR catalyst and a preparation method thereof. The integral low-temperature SCR denitration catalyst containing TiO2 and manganese oxide is synthesized and prepared by a self-propagating combustion method using cordierite honeycomb ceramics as a carrier. The catalyst is suitable for purifying nitrogen oxides in automobile exhaust and boiler flue gas.

[0006] CN 109201066A discloses a palladium-cerium-zirconium composite metal oxide catalyst for electrostatic field synergistic removal of methane. The palladium-cerium-zirconium composite metal oxide catalyst is synthesized by a self-propagating high-temperature combustion synthesis method. After synergistic coupling with an electrostatic field, the catalyst has a high catalytic oxidation efficiency for low-concentration methane of 0.2% within 200-500°C. However, the removal of pollutants requires electrostatic field synergistic catalytic oxidation, which is inconvenient to operate.

[0007] At present, the specificity of this type of catalyst is generally relatively single, but the VOCs environment in which it is used is usually not single. For example, for hydrocarbon VOCs, they usually contain not only alkanes such as methane, but also some alkenes such as a small amount of ethylene. Therefore, it is necessary to design a catalyst with wider applicability, especially with wider applicability to hydrocarbon VOCs, to meet the needs of different VOCs catalytic reactions. Summary of the invention

[0008] To remedy the deficiencies of the prior art, the present invention aims to provide a volatile organic compound catalytic oxidation catalyst, a preparation method and its application, which has high catalytic efficiency and meets the needs of different VOCs catalytic reactions.

[0009] To achieve the first aspect of the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0010] A method for preparing a volatile organic compound catalytic oxidation catalyst comprises the following steps:

[0011] 1) preparing an alumina combustion liquid: taking an aluminum salt and a modified salt as soluble salts and a sufficient amount of a combustion agent, dissolving them in deionized water and stirring them evenly to obtain an alumina combustion liquid; wherein the modified salt is a soluble salt of cerium and zirconium; the mass of the soluble salt is calculated as oxide, and the ratio of the sum of the mass of cerium and zirconium oxides to the mass of alumina is 1:(4-9);

[0012] 2) Preparation of alumina coating by self-propagating combustion coating: immersing a cordierite substrate in the alumina combustion liquid so that the alumina combustion liquid is evenly adsorbed and distributed on the wall surface of the substrate, drying the cordierite substrate, and then placing it in a muffle furnace and calcining it at 400-700° C. for 2-6 hours to obtain a cordierite substrate coated with alumina coating;

[0013] 3) Impregnation of precious metals: The cordierite substrate coated with an alumina coating is immersed in a precious metal precursor solution to adsorb the corresponding precious metal salt, and then taken out, dried, and further calcined to obtain a catalyst.

[0014] Step 1) of the present invention is to prepare a combustion liquid for a self-propagating combustion method. The self-propagating combustion method is well known in the art. The combustion agent can be one or more of urea, citric acid or glycine. The amount of the combustion agent used may vary depending on the type of the combustion agent, and it is preferred that the amount of the combustion agent be sufficient to meet the preparation requirements of the self-propagating combustion method.

[0015] In a preferred embodiment, the molar ratio of the combustion agent to the soluble salt is (2-3):1.

[0016] In some embodiments, the aluminum salt is aluminum chloride or aluminum nitrate; and the soluble salts of cerium and zirconium may be cerium nitrate and zirconium nitrate.

[0017] Preferably, in step 1), the modified salt and aluminum salt used are calculated as their oxides, and the mass ratio of the oxide of the modified salt to aluminum oxide is 1-5:8, such as 1:6 or 1:7.

[0018] Preferably, in step 1), the molar ratio of cerium element to zirconium element in the modified salt is 1:3 to 3:1, such as 1:1, 1:2 or 2:1.

[0019] Step 2 of the present invention is to prepare an alumina coating on a cordierite substrate by a self-propagating combustion method; during impregnation, the cordierite substrate is immersed in the configured alumina combustion liquid, and the specific immersion time can be appropriately adjusted according to the solution concentration and the target impregnation amount; in some embodiments, the immersion time can be 20 to 40 minutes, and after taking out, the air in the substrate pores is exhausted with a super air knife to make the combustion liquid fully and evenly distributed on the substrate wall.

[0020] In step 2), the substrate taken out needs to be dried and dehydrated before calcination, for example, by drying in a drying oven or using a hot air gun at 60-120°C.

[0021] Preferably, during the calcination in step 2), the calcination temperature is 500-700° C., such as 550, 650 or 700° C., and the calcination time is 2-3 h.

[0022] Preferably, in the obtained cordierite substrate coated with alumina coating, based on the volume of the cordierite substrate, the alumina loading of the catalyst is 80-90 g / L, such as 82, 86 or 88 g / L, the cerium oxide loading is 3-17 g / L, such as 3.2, 8, 14 or 16.2 g / L, and the zirconium oxide loading is 3-7 g / L, such as 3.8, 5, 6 or 6.8 g / L. It will be appreciated by those skilled in the art that the loading of the relevant components can be adjusted by adjusting the number of impregnation and combustion.

[0023] Step 3) of the present invention is to further load the precious metal on the obtained cordierite substrate coated with the alumina coating by impregnating a precursor solution dissolved with a precious metal salt such as a nitrate. The precious metal can be a type of precious metal commonly added to the catalytic oxidation catalyst of volatile organic compounds in the art, such as one or more precious metals selected from Pt, Pd, Rh, Ru, Ag and Au, preferably one or more selected from Pt, Pd and Ru, and more preferably one or more selected from Pt and Pd.

[0024] According to the preparation method of the present invention, the concentration of the precious metal precursor solution can be 0.1-5wt.%, such as 0.5-2wt.%, 1wt.%. Those skilled in the art understand that too concentrated solution may be detrimental to the uniform distribution of precious metals, while too diluted solution may reduce the impregnation efficiency.

[0025] In one embodiment, the calcination temperature in step 3) is 400-600°C, such as 500°C.

[0026] Preferably, in the catalyst obtained in step 3), based on the volume of the cordierite matrix, the precious metal loading in the catalyst is 0.1-1.5 g / L, preferably 0.1-1.2 g / L, such as 0.2, 0.5 or 1 g / L.

[0027] In some embodiments, the preparation method further includes a cordierite substrate pretreatment step: heating and boiling the cordierite substrate in a 20-50wt% oxalic acid solution for 1 hour, soaking it for 8-30 hours after cooling, taking it out, rinsing it, and drying it to obtain a cordierite substrate, thereby obtaining a cordierite with a rough surface and improving the bonding between the coating and the substrate.

[0028] In order to achieve another aspect of the above-mentioned object of the invention, the present invention also provides a catalyst prepared according to the above-mentioned preparation method.

[0029] In order to achieve another aspect of the above-mentioned object of the invention, the present invention also provides the use of the above-mentioned catalyst in the catalytic oxidation of hydrocarbon volatile organic compounds.

[0030] In a preferred embodiment, the hydrocarbon volatile organic matter contains low-carbon alkanes such as methane and ethylene, such as coal chemical tail gas or exhaust gas.

[0031] Compared with the prior art, the present invention has the following advantages:

[0032] 1. Controlling the metal ratio (Al / Ce+Zr) and ignition temperature in the self-propagating combustion liquid to achieve controllable preparation of coating defects, and then inducing the impregnated precious metals to form polyatomic aggregates on the loaded precious metals, which can meet the needs of different VOCs catalytic reactions (such as ethylene and methane);

[0033] 2. The precious metal utilization rate of the coating prepared by this method is high, and the same or better activity can be achieved with a lower amount of precious metal, which reduces the cost;

[0034] 3. This method improves the thermal stability of the coating and the anti-sintering performance of the carrier. At the same time, due to the interaction between the carrier and the active component, the excessive agglomeration of the precious metal on the catalyst is inhibited;

[0035] 4. Using this method, the coating has a strong bonding force with the carrier and the coating shedding rate is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 TEM image of the catalyst coating prepared in Example 1;

[0037] Figure 2 TEM image of the catalyst coating prepared in Example 2;

[0038] Figure 3 TEM image of the catalyst coating prepared in Example 3;

[0039] Figure 4 The catalyst activity comparison diagram of Example 3 and Comparative Example 1;

[0040] Figure 5 TEM image of the catalyst coating prepared in Comparative Example 2

[0041] Figure 6 The catalyst activity comparison diagram of Example 3 and Comparative Example 2 is shown in FIG. DETAILED DESCRIPTION

[0042] The present invention is further described below in conjunction with the embodiments and drawings, but the present invention is not limited to the listed embodiments, but should also include equivalent improvements and modifications of the technical solutions defined in the claims attached to the patent application of the present invention.

[0043] Unless otherwise specified, all relevant reagents in the following examples / comparative examples are of analytical grade.

[0044] Example 1

[0045] (1) Pretreatment of cordierite substrate: a 2 cm×2 cm×5 cm cordierite honeycomb ceramic was heated and boiled in a 20 wt % oxalic acid solution for 1 h, cooled and soaked for 30 h, taken out and rinsed with deionized water, and then placed in a drying oven at 120° C. until completely dried.

[0046] (2) Preparation of alumina combustion liquid: 9.0856 g of cerium nitrate, 2.9944 g of zirconium nitrate, and 131.2955 g of aluminum nitrate were weighed and dissolved in 500 ml of deionized water. After complete dissolution, the mixture was mixed and heated, and 85.1065 g of glycine was added. The mixture was stirred for 1 hour to obtain a combustion liquid.

[0047] (3) Preparation of alumina coating by self-propagating combustion coating: The pre-treated cordierite substrate was immersed in the above-mentioned combustion liquid for 30 minutes, and the air in the pores was exhausted with a super air knife to make the solution fully and evenly distributed on the substrate wall. The substrate was dried with a hot air gun at 60-120°C (60°C for 2 minutes, 90°C for 2 minutes, and 120°C for 2 minutes), and then placed in a muffle furnace and calcined at 700°C for 2 hours to obtain a cordierite substrate coated with alumina coating.

[0048] (4) Impregnation of precious metals: The cordierite substrate coated with an alumina coating was immersed in a nitrate solution with a concentration of 1 wt.% of Pt metal for 30 minutes, then taken out and dried at 120°C for 2 hours, and calcined in a muffle furnace at 550°C for 5 hours to obtain a catalyst with a Pt loading of 0.5 g / L. The catalyst has an alumina loading of 80.00 g / L, a cerium oxide loading of 16.15 g / L, and a zirconium oxide loading of 3.85 g / L (based on the volume of the cordierite substrate). Figure 1 This is a TEM image of the coating removed from the surface of the catalyst prepared in Example 1. It can be seen that the noble metal atoms are spherical or elliptical, and in addition to being in a single atomic state, they also form multi-atom aggregates.

[0049] The catalyst was used to catalyze the oxidation of ethylene (C2H4) waste gas (waste gas: 10 vol.% O2, 0.07 vol.% C2H4, 5 vol.% H2O, and the rest were mainly inert components in the air that did not participate in the reaction). The reaction space velocity was 20,000 h -1 The catalytic performance of the catalyst at 150-500°C was investigated by continuous online monitoring. The results showed that the conversion rate of C2H4 reached 100% at 150°C.

[0050] Example 2

[0051] (1) Pretreatment of cordierite substrate: a 2 cm×2 cm×5 cm cordierite honeycomb ceramic was heated and boiled in a 20 wt % oxalic acid solution for 1 h, cooled and soaked for 30 h, taken out and rinsed with deionized water, and then placed in a drying oven at 120° C. until completely dried.

[0052] (2) Preparation of alumina combustion liquid: 4.3723 g of cerium nitrate, 4.3230 g of zirconium nitrate, and 131.2955 g of aluminum nitrate were weighed and dissolved in 500 ml of deionized water. After complete dissolution, the mixture was mixed and heated. 61.1284 g of urea was added and stirred for 1 hour to obtain a combustion liquid.

[0053] (3) Preparation of alumina coating by self-propagating combustion coating: The pre-treated cordierite substrate was immersed in the above combustion liquid for 40 minutes, and the air in the pores was exhausted with a super air knife to make the solution fully and evenly distributed on the substrate wall. It was dried with a hot air gun at 60-120℃ (60℃ for 2 minutes, 90℃ for 2 minutes, and 120℃ for 2 minutes), and then placed in a muffle furnace and calcined at 600℃ for 3 hours.

[0054] (4) Impregnation of precious metals: The cordierite substrate coated with an alumina coating was immersed in a nitrate solution with a concentration of 1 wt.% of Pd metal for 120 min, then taken out and dried at 120°C for 6 h. The catalyst was calcined in a muffle furnace at 550°C for 6 h to obtain a catalyst with a Pd loading of 1 g / L, an alumina loading of 85.71 g / L, a cerium oxide loading of 8.32 g / L, and a zirconium oxide loading of 5.96 g / L (based on the volume of the cordierite substrate). Figure 2 This is a TEM image of the coating removed from the surface of the catalyst prepared in Example 2. It can be seen that the noble metal atoms are spherical or elliptical, and in addition to being in a single atomic state, they also form multi-atom aggregates.

[0055] The catalyst was used to catalytically oxidize methane (CH4) waste gas (waste gas: 10 vol.% O2, 0.1 vol.% CH4, 5 vol.% H2O, and the rest were mainly inert components in the air that did not participate in the reaction), with a reaction space velocity of 20,000 h -1 The catalytic performance of the catalyst at 200-500°C was investigated by continuous online monitoring. The results showed that the CH4 conversion rate reached 90% at 450°C.

[0056] Example 3

[0057] (1) Pretreatment of cordierite substrate: a 2 cm×2 cm×5 cm cordierite honeycomb ceramic was heated and boiled in a 20 wt % oxalic acid solution for 1 h, cooled and soaked for 30 h, taken out and rinsed with deionized water, and then placed in a drying oven at 120° C. until completely dried.

[0058] (2) Preparation of alumina combustion liquid: Weigh 2.3799 g of cerium nitrate, 7.0592 g of zirconium nitrate, and 69.9000 g of aluminum chloride and dissolve them in 500 ml of deionized water. After complete dissolution, mix and heat, add 81.9986 g of glycine, and continue stirring for 1 hour to obtain a combustion liquid.

[0059] (3) Preparation of alumina coating by self-propagating combustion coating: The pre-treated cordierite substrate was immersed in the above combustion liquid for 20 minutes, and the air in the pores was exhausted with a super air knife to make the solution fully and evenly distributed on the substrate wall. It was dried with a hot air gun at 60-120℃ (60℃ for 2 minutes, 90℃ for 2 minutes, and 120℃ for 2 minutes), and then placed in a muffle furnace and calcined at 500℃ for 5 hours.

[0060] (4) Impregnation of precious metals: The cordierite substrate coated with an alumina coating was immersed in a nitrate solution with a precious metal concentration of 1 wt.% (Pd / Pt mass ratio of 4) for 120 min, then taken out, dried at 120°C for 6 h, and calcined in a muffle furnace at 550°C for 6 h to obtain a catalyst with a precious metal loading of 1.0 g / L, an alumina loading of 90.00 g / L, a cerium oxide loading of 3.18 g / L, and a zirconium oxide loading of 6.82 g / L (based on the volume of the cordierite substrate). Figure 3 This is a TEM image of the catalyst surface coating of Example 3. It can be seen that the noble metal atomic particles are spherical or elliptical, and also form a large number of multi-atom aggregates.

[0061] Comparative Example 1:

[0062] According to the content of alumina, cerium-zirconium modifier and precious metals in Example 3, a catalyst with a precious metal loading of 1.0 g / L was prepared by a traditional coating method. The loading of alumina was 90.00 g / L, the loading of cerium oxide was 3.18 g / L, and the loading of zirconium oxide was 6.82 g / L (based on the volume of the cordierite matrix).

[0063] The catalyst of Example 3 and the comparative catalyst were tested for shedding rate. The catalyst end face was evenly and slowly purged with 0.55 MPa compressed air for 60 seconds. The shedding rate of the catalyst of the present invention was 0.13% based on the mass difference before and after, while the shedding rate of the comparative catalyst was 0.21%.

[0064] The monolithic catalysts of Example 3 and the comparative example were used to catalytically oxidize a CH4 / C2H4 mixed gas, wherein the mixed gas contained 10 vol.% O2, 0.07 vol.% C2H4, 0.1 vol.% CH4, and 5 vol.% H2O, and the remainder was mainly inert components in the air that did not participate in the reaction. The reaction space velocity was 20000 h -1 The catalytic performance of the catalyst at 200-500°C was investigated by continuous online monitoring. Figure 4 .

[0065] from Figure 4 It can be clearly seen that the integral catalyst prepared in Example 3 has significantly higher activity for the CH4 / C2H4 mixed gas than the comparative catalyst. The catalyst in Example 3 achieves more than 90% conversion of C2H4 and CH4 at 300°C and 450°C, respectively, while the comparative catalyst is significantly lower accordingly.

[0066] Comparative Example 2:

[0067] The preparation process is the same as that in Example 3, except that the amount of each raw material of the combustion liquid is changed, that is, 1.7450g of cerium nitrate, 6.9014g of zirconium nitrate, and 69.9000g of aluminum chloride are weighed and dissolved in 500ml of deionized water, mixed and heated after complete dissolution, 143.0170g of glycine is added, and stirring is continued for 1h to obtain a combustion liquid. An alumina coating is prepared by self-propagating combustion coating and impregnated with a noble metal salt solution, and a catalyst with a noble metal loading of 1.0g / L is obtained after drying and roasting, and the loading of alumina is 90.91g / L, the loading of cerium oxide is 2.35g / L, and the loading of zirconium oxide is 6.73g / L (based on the volume of the cordierite matrix).

[0068] Figure 5 This is a TEM image of the surface coating of the integral catalyst prepared in Example 2. It can be seen that the noble metal atomic particles are spherical or elliptical and the particle size is relatively large.

[0069] The catalysts of Example 3 and Comparative Example 2 were used to catalytically oxidize a CH4 / C2H4 mixed gas, and the mixed gas composition and reaction conditions were the same as those in Comparative Example 1 ( Figure 6 ). The activity of the catalyst prepared in Example 3 to the CH4 / C2H4 mixed gas is significantly higher than that of the catalyst prepared in Comparative Example 2.

Claims

1. A method for preparing a volatile organic compound catalytic oxidation catalyst, comprising the following steps: 1) preparing an alumina combustion liquid: taking an aluminum salt and a modified salt as soluble salts and a sufficient amount of a combustion agent, dissolving them in deionized water and stirring them evenly to obtain an alumina combustion liquid; wherein the modified salt is a soluble salt of cerium and zirconium; the mass of the soluble salt is calculated as oxide, and the ratio of the sum of the mass of cerium and zirconium oxides to the mass of alumina is 1:(4-9); 2) Preparation of alumina coating by self-propagating combustion coating: immersing a cordierite substrate in the alumina combustion liquid so that the alumina combustion liquid is evenly adsorbed and distributed on the wall surface of the substrate, drying the cordierite substrate, and then placing it in a muffle furnace and calcining it at 400-700° C. for 2-6 hours to obtain a cordierite substrate coated with alumina coating; 3) Impregnation of precious metals: The cordierite substrate coated with an alumina coating is immersed in a precious metal precursor solution to adsorb the corresponding precious metal salt, and then taken out, dried, and further calcined to obtain a catalyst.

2. The preparation method according to claim 1, characterized in that: The combustion agent is one or more of urea, citric acid or glycine; the molar ratio of the combustion agent to the soluble salt is (2-3):

1.

3. The preparation method according to claim 1, characterized in that: The molar ratio of cerium element to zirconium element in the modified salt is (1-3): (3-1).

4. The preparation method according to claim 1, characterized in that: In the obtained cordierite substrate coated with alumina coating, based on the volume of the cordierite substrate, the catalyst has an alumina loading of 80-90 g / L, a cerium oxide loading of 3-17 g / L, and a zirconium oxide loading of 3-7 g / L.

5. The preparation method according to claim 1, characterized in that: The calcination temperature in step 2) is 500-700°C; the calcination temperature in step 3) is 400-600°C.

6. The preparation method according to claim 1, characterized in that: The concentration of the noble metal precursor solution is 0.1-5wt.%; Preferably, the noble metal is selected from one or more of Pt, Pd, Rh, Ru, Ag and Au, preferably selected from one or more of Pt, Pd and Ru, and more preferably selected from one or more of Pt and Pd.

7. The preparation method according to claim 1, characterized in that: Based on the volume of the cordierite matrix, the loading amount of the noble metal in the catalyst is 0.1-1.5 g / L, preferably 0.2-1 g / L.

8. The preparation method according to claim 1, characterized in that: The preparation method also includes a cordierite matrix pretreatment step: heating and boiling the cordierite matrix in a 20-50wt% oxalic acid solution for 1 hour, cooling and soaking for 8-30 hours, taking out, rinsing and drying to obtain the cordierite matrix.

9. The catalyst prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the catalyst according to claim 9 in catalytic oxidation of hydrocarbon volatile organic compounds; preferably, the hydrocarbon volatile organic compounds contain methane and ethylene.

Citation Information

Patent Citations

  • Integral low-temperature SCR denitration catalyst and preparation method thereof

    CN105709719A

  • Pd-Ce-Zr composite metal oxide catalyst for synergistic removal of methane by electrostatic field

    CN109201066A

Cited By

  • Preparation method, product and application of coating type cordierite catalyst

    CN120285978A