Chlorine-resistant catalyst as well as preparation method and application thereof
By preparing an anti-chlorine catalyst, tetrabutyl titanium titanate and HCl solution were used to form a rutile titanium dioxide powder exposed to (110) crystal surface and reacted with palladium salt to form a Pd/TiO2 catalyst, which solved the high energy consumption and chlorine resistance of catalyzed styrene The problem of poor poisoning ability has achieved the improvement of low-temperature and efficient catalysis and anti-chlorine poisoning ability.
Patent Information
- Application Number
- CN202411123706.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
Existing catalysts have high energy consumption and poor chlorine poisoning ability when catalyzing styrene, making it difficult to effectively treat chlorine-containing waste gases in the plastic and rubber industries.
By preparing an anti-chlorine catalyst, tetrabutyl titanium titanate and HCl solution are used to generate rutile titanium dioxide powder exposed (110) crystal surfaces, and react with soluble palladium salt and platinum salt at different temperatures to form a Pd/TiO2 catalyst. Improve the catalyst's anti-chlorine poisoning ability and low-temperature activity.
The energy consumption of styrene catalytic oxidation treatment is significantly reduced. The catalyst can effectively remove styrene at 240°C and maintain high-efficiency activity at 270°C, which significantly improves the catalytic performance and anti-chlorine poisoning ability.
Smart Images

Figure CN119016043A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a chlorine-resistant catalyst and a preparation method and application thereof. Background Art
[0002] Volatile organic compounds refer to organic compounds with a Reed vapor pressure exceeding 10.3 Pa at normal temperature (293.15K) and pressure (101.325kPa). At present, they are one of the main factors of air pollution. They are the precursors of ozone / photochemical smog, which will lead to excessive ozone and photochemical smog, and also have direct harmful effects on the environment and human health.
[0003] The main sources of VOCs are oil refineries, fuel combustion, chemical industry, decomposition of biomass, pharmaceutical plants, automotive industry, textile manufacturers, solvent processing, cleaning products, printing presses, insulation materials, office supplies, printers, etc. The most common VOCs are halogenated compounds, aldehydes, alcohols, ketones, aromatic compounds and ethers. High concentrations of these VOCs can cause allergies, nausea, dizziness and headaches. Some VOCs are also carcinogenic to humans and animals, such as acrylonitrile, styrene, etc.
[0004] Rubber and plastic related industries, such as plastic recycling, plastic product manufacturing, synthetic rubber, rubber recycling, rubber product manufacturing, etc., often produce styrene-containing organic waste gas and chlorine-containing waste gas such as vinyl chloride during the production process. If such styrene-containing waste gas is not properly handled, it will have a great impact on the environment and the health of surrounding personnel. Therefore, the development of low-energy consumption treatment technology for such waste gas can solve the governance problems faced by such enterprises.
[0005] At present, the commonly used waste gas treatment methods for this type of waste gas include physical adsorption, chemical absorption and catalytic oxidation. Physical adsorption technology mainly uses adsorbents such as activated carbon to adsorb styrene in the waste gas, and then regenerates or pyrolyzes it. However, the characteristics of styrene polymerization often cause the adsorption material to be blocked and cannot be used, and the adsorption material becomes hazardous waste, and the cost of replacement and treatment is huge. Chemical absorption uses chemical reagents in a solution (such as sodium hydroxide solution) to react chemically with styrene in styrene waste gas to absorb it, but the absorption liquid will cause secondary pollution, and the treatment cost of the absorption liquid is high. Styrene catalytic oxidation technology is a method of oxidizing organic matter in styrene waste gas into harmless substances. This technology uses a catalyst to convert styrene into carbon dioxide and water under appropriate temperature, pressure and oxygen conditions to purify the waste gas. This technology has no secondary pollution, is the most thorough and efficient in degrading styrene, and is one of the current mainstream technologies.
[0006] The styrene catalysts used in existing catalytic oxidation technologies are mainly precious metal catalysts loaded with precious metals (platinum, palladium, rhodium, etc.). However, most of these waste gases contain chlorine-containing components, and the ability of the catalyst to resist chlorine poisoning is particularly important to ensure the treatment effect. In addition, the operating temperature of existing catalysts generally needs to be above 320°C, and there is still a problem of high energy consumption. Therefore, styrene catalytic oxidation technology needs to further improve the stability and resistance to chlorine poisoning of the catalyst, reduce energy consumption, explore new catalysts and reaction conditions, and achieve more environmentally friendly and economical waste gas treatment technology in the plastics and rubber industries. Summary of the invention
[0007] The purpose of the present invention is to overcome the above technical deficiencies, provide a chlorine-resistant catalyst and a preparation method and application thereof, and solve the technical problems of high energy consumption and poor resistance to chlorine poisoning of the catalyst in the prior art when catalyzing styrene.
[0008] In order to achieve the above technical purpose, the technical solution of the present invention provides a method for preparing a chlorine-resistant catalyst, comprising the following steps:
[0009] S1, adding tetrabutyl titanate dropwise to a stirring HCl solution, and then continuing to stir to obtain a mixed solution, and then transferring the mixed solution to a reaction kettle, and obtaining a rutile titanium dioxide powder with an exposed (110) crystal plane at 160-180° C.;
[0010] S2, mixing the (110) crystal face rutile titanium dioxide powder obtained in step S1 with water, and then sequentially performing ultrasonic treatment and stirring, and then adjusting the pH to 10-11, and then continuing to add soluble palladium salt and / or soluble platinum salt, and maintaining stirring and heat preservation at 70-80° C. to obtain a solid powder;
[0011] S3. Place the solid powder in a heating device, raise the temperature to 300-600° C. at a rate of 2-3° C. / min and keep the temperature to obtain a catalyst.
[0012] In any embodiment, in step S1, the concentration of the HCl solution is 6-9 mol / L.
[0013] In any embodiment, in step S1, the volume ratio of the tetrabutyl titanate to the HCl solution is 1:(5-6).
[0014] In any embodiment, in step S1, the heat preservation time at 160-180°C is 4-6 hours; and / or, in step S1, stirring is continued for 10-30 minutes to obtain the mixed solution.
[0015] In any embodiment, in step S2, the rutile titanium dioxide powder with (110) crystal face and water are mixed in a dosage ratio of (1-2) g:100 mL; and / or, in step S2, the soluble palladium salt is palladium nitrate dihydrate, the soluble platinum salt is platinum nitrate, and the mass ratio of the palladium nitrate dihydrate or the platinum nitrate to the rutile titanium dioxide powder with (110) crystal face is (5-8) mg:1 g.
[0016] In any embodiment, in step S2, the ultrasound and stirring are performed sequentially, the ultrasound time is 10-20 min, and the stirring time is 10-20 min.
[0017] In any embodiment, in step S2, the time of keeping the temperature at 70-80°C is 10-12 hours.
[0018] In any embodiment, in step S3, the holding time at 300-600°C is 2-3 hours.
[0019] The present invention also provides a chlorine-resistant catalyst, which is prepared by the above preparation method.
[0020] In addition, the present invention also proposes the use of the chlorine-resistant catalyst prepared by the above preparation method or the above chlorine-resistant catalyst in catalytic oxidation of styrene.
[0021] Compared with the prior art, the beneficial effects of the present invention include: the chlorine-resistant catalyst prepared by the preparation method proposed in the present invention, the active metal oxide as the precious metal Pd carrier in the material will greatly affect the catalytic performance of the catalyst, by controlling the TiO 2 Exposing different crystal faces can significantly improve the catalytic performance and chlorine poisoning resistance of the catalyst. The present invention controls the synthesis process to expose more TiO 2 The high-activity crystal face of the catalyst can further improve the low-temperature activity of the catalyst. The prepared catalyst can achieve catalytic oxidation removal of styrene at 240°C, which can greatly reduce the energy consumption of styrene catalytic oxidation treatment technology. And after chlorination treatment, the catalyst can still achieve catalytic oxidation removal of styrene at 270°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The TiO prepared in Example 1 of the present invention 2 -R and catalyst Pd / TiO 2 TEM, HRTEM and HAADF images of the material; among them, Figure 1 a is the prepared TiO 2 TEM image of -R sample, Figure 1 b is the prepared TiO 2HRTEM image of -R sample, Figure 1 c and Figure 1 d is the Pd / TiO prepared in Example 1 2 TEM image of -R sample, Figure 1 e is the Pd / TiO prepared in Example 1 2 HRTEM image of the -R sample.
[0023] Figure 2 This is the catalytic performance test result of Application Example 1 of the present invention.
[0024] Figure 3 This is the test result of the stability of the catalyst in Application Example 1 of the present invention in treating chlorine-containing VOCs.
[0025] Figure 4 These are the test results of the catalytic performance of the catalyst in Application Example 1 of the present invention before and after chlorination treatment. DETAILED DESCRIPTION
[0026] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0027] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0028] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0029] This specific embodiment provides a method for preparing a chlorine-resistant catalyst, comprising the following steps:
[0030] S1. Tetrabutyl titanate is added dropwise to a stirring HCl solution, and then stirring is continued for 10-30 minutes to obtain a mixed solution, and then the mixed solution is transferred to a reaction kettle, and the mixture is kept at 160-180° C. for 4-6 hours to obtain a rutile titanium dioxide powder with an exposed (110) crystal face; the concentration of the HCl solution is 6-9 mol / L; and the volume ratio of the tetrabutyl titanate to the HCl solution is 1:(5-6);
[0031] S2, the rutile titanium dioxide powder with a (110) crystal face obtained in step S1 and water are mixed in a dosage ratio of (1-2) g:100 mL, and then ultrasonically treated for 10-20 min and stirred for 10-20 min in sequence, and then the pH is adjusted to 10-11, and then a soluble palladium salt and / or a soluble platinum salt are continuously added, stirring is maintained, and the mixture is kept warm at 70-80° C. for 10-12 hours to obtain a solid powder; the soluble palladium salt is palladium nitrate dihydrate, and the soluble platinum salt is platinum nitrate, and the mass ratio of the palladium nitrate dihydrate or the platinum nitrate to the rutile titanium dioxide powder with a (110) crystal face is (5-8) mg:1 g;
[0032] S3. Place the solid powder in a heating device, heat it to 300-600° C. at a rate of 2-3° C. / min and keep it warm for 2-3 hours to obtain a catalyst; in some embodiments, the heating device is a muffle furnace.
[0033] This specific embodiment also provides a catalyst, which is prepared by the above-mentioned preparation method.
[0034] This specific embodiment also proposes the use of the catalyst prepared by the above preparation method or the above catalyst in catalytic oxidation of styrene.
[0035] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0036] In the present invention, reference is made to “some embodiments”, “this embodiment”, examples, etc., which describe a subset of all possible embodiments, but it can be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.
[0037] If similar descriptions of "first / second" appear in the application documents, the following instructions are added. In the following description, the terms "first\second\third" involved are merely used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged in a specific order or sequence where permitted, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein.
[0038] In this embodiment, the term "and / or" is merely a description of the association relationship between associated objects, indicating that three relationships may exist. For example, object A and / or object B may represent three situations: object A exists alone, object A and object B exist at the same time, and object B exists alone.
[0039] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0040] Example 1
[0041] This embodiment proposes a catalyst Pd / TiO 2 The material is prepared by the following steps:
[0042] S1. Add 4 mL of tetrabutyl titanate to a 20 mL HCl solution with a concentration of 8 mol / L, and continue stirring for 10 min to obtain a mixed solution. Then transfer the mixed solution to a polytetrafluoroethylene autoclave, seal it well, and keep it at 180°C for 4 hours to obtain a light yellow powder. The obtained light yellow powder is washed with ethanol and water for 3 times respectively until no precipitation is generated when the supernatant is titrated with silver nitrate. The obtained solid powder is placed in a drying oven at 80°C and dried overnight to obtain a rutile titanium dioxide powder with an exposed (110) crystal face. The sample is marked as TiO 2 -R;
[0043] S2, dispersing 1 g of the rutile titanium dioxide powder with the (110) crystal plane obtained in step S1 into 100 mL of deionized water for mixing, then performing ultrasonic treatment for 10 min and stirring for 10 min in sequence, then adjusting the pH to 10, and then continuing to add 5 mg of palladium nitrate dihydrate, keeping stirring and keeping warm at 70° C. for 12 hours to obtain a solid powder;
[0044] S3, the solid powder was placed in a muffle furnace, the temperature was raised to 400°C at a rate of 2°C / min and kept at this temperature for 2 hours to obtain Pd / TiO 2 Material. Figure 1 Figures a and b show the prepared TiO 2 -R sample TEM and HRTEM images show that the prepared rutile titanium dioxide presents a nanoribbon morphology with a width ranging from 10-45nm and a length of different lengths. Further measurements revealed that Figure 1 The lattice fringes shown in (b) correspond to the (110) crystal plane of rutile titania, demonstrating the successful preparation of rutile titania nanoribbons with exposed (110) crystal planes. Figure 1 c. Figure 1 d and Figure 1 e is Pd / TiO 2 -R sample TEM and HRTEM images. Comparison of TiO 2 -R TEM image, showing the successful loading of precious metal Pd particles.
[0045] Example 2
[0046] This embodiment proposes a catalyst Pd / TiO 2 The material is prepared by the following steps:
[0047] S1. Add 4 mL of tetrabutyl titanate to a 22 mL HCl solution with a concentration of 6 mol / L, and continue stirring for 20 min to obtain a mixed solution. Then transfer the mixed solution to a polytetrafluoroethylene autoclave, seal it well, and keep it at 160°C for 5 hours to obtain a light yellow powder. Wash the obtained light yellow powder with ethanol and water for 3 times, respectively, until no precipitation is generated when the supernatant is titrated with silver nitrate. Place the obtained solid powder in a drying oven at 80°C and dry it overnight to obtain a rutile titanium dioxide powder with an exposed (110) crystal face;
[0048] S2, dispersing 1 g of the rutile titanium dioxide powder with the (110) crystal plane obtained in step S1 into 100 mL of deionized water for mixing, then performing ultrasonication for 15 min and stirring for 15 min in sequence, then adjusting the pH to 10, and then continuing to add 8 mg of palladium nitrate dihydrate, keeping stirring and keeping warm at 75° C. for 11 hours to obtain a solid powder;
[0049] S3, the solid powder was placed in a muffle furnace, the temperature was raised to 400°C at a rate of 2°C / min and kept at this temperature for 2 hours to obtain Pd / TiO 2 Material.
[0050] Example 3
[0051] This embodiment proposes a catalyst Pd / TiO 2 The material is prepared by the following steps:
[0052] S1. Add 4 mL of tetrabutyl titanate to a 24 mL HCl solution with a concentration of 7 mol / L, and continue stirring for 20 min to obtain a mixed solution. Then transfer the mixed solution to a polytetrafluoroethylene autoclave, seal it well, and keep it at 160°C for 5 hours. Wash the obtained light yellow powder with ethanol and water for 3 times, respectively, until no precipitation is generated when the supernatant is titrated with silver nitrate. The obtained solid powder is placed in a drying oven at 80°C and dried overnight to obtain rutile titanium dioxide powder with exposed (110) crystal plane;
[0053] S2, dispersing 1 g of the rutile titanium dioxide powder with the (110) crystal plane obtained in step S1 into 100 mL of deionized water for mixing, then performing ultrasonication for 15 min and stirring for 15 min in sequence, then adjusting the pH to 11, and then continuing to add 6 mg of palladium nitrate dihydrate, keeping stirring and keeping warm at 75° C. for 11 hours to obtain a solid powder;
[0054] S3, the solid powder was placed in a muffle furnace, the temperature was raised to 300°C at a rate of 3°C / min and kept at this temperature for 2.5 hours to obtain Pd / TiO 2 Material.
[0055] Example 4
[0056] This embodiment proposes a catalyst Pd / TiO 2 The material is prepared by the following steps:
[0057] S1. Add 4 mL of tetrabutyl titanate to a 22 mL HCl solution with a concentration of 9 mol / L, and continue stirring for 20 min to obtain a mixed solution. Then transfer the mixed solution to a polytetrafluoroethylene autoclave, seal it well, and keep it at 160°C for 5 hours. Wash the obtained light yellow powder with ethanol and water three times respectively until no precipitation is generated when the supernatant is titrated with silver nitrate. Place the obtained solid powder in a drying oven at 80°C and dry it overnight to obtain rutile titanium dioxide powder with exposed (110) crystal plane;
[0058] S2, dispersing 1 g of the (110) crystal face rutile titanium dioxide powder obtained in step S1 into 100 mL of deionized water for mixing, then performing ultrasonic treatment for 20 min and stirring for 20 min in sequence, then adjusting the pH to 11, and then continuing to add 7 mg of palladium nitrate dihydrate, maintaining stirring and keeping warm at 80° C. for 10 hours to obtain a solid powder;
[0059] S3, the solid powder was placed in a muffle furnace, the temperature was raised to 600°C at a rate of 3°C / min and kept at this temperature for 3 hours to obtain Pd / TiO 2 Material.
[0060] Example 5
[0061] This embodiment provides a catalyst, which is prepared by the following steps:
[0062] S1. Add 4 mL of tetrabutyl titanate to a 20 mL HCl solution with a concentration of 8 mol / L, and continue stirring for 10 min to obtain a mixed solution. Then transfer the mixed solution to a polytetrafluoroethylene autoclave, seal it well, and keep it at 180°C for 4 hours to obtain a light yellow powder. The obtained light yellow powder is washed with ethanol and water for 3 times respectively until no precipitation is generated when the supernatant is titrated with silver nitrate. The obtained solid powder is placed in a drying oven at 80°C and dried overnight to obtain a rutile titanium dioxide powder with an exposed (110) crystal face. The sample is marked as TiO 2 -R;
[0063] S2, dispersing 1 g of the rutile titanium dioxide powder with the (110) crystal plane obtained in step S1 into 100 mL of deionized water for mixing, then performing ultrasonication for 10 min and stirring for 10 min in sequence, then adjusting the pH to 10, and then continuing to add 5 mg of platinum nitrate, keeping stirring and keeping warm at 70° C. for 12 hours to obtain a solid powder;
[0064] S3. Place the solid powder in a muffle furnace, heat it to 400° C. at a rate of 2° C. / min and keep it at that temperature for 2 hours to obtain a catalyst.
[0065] Comparative Example 1
[0066] This comparative example proposes a Pd / TiO 2 The material is prepared by the following steps:
[0067] S1. Synthesis of anatase titanium dioxide with exposed (101) crystal plane: Commercial anatase titanium dioxide is used as raw material, and a one-step alkaline hydrothermal reaction is carried out to prepare anatase titanium dioxide with exposed specific crystal planes. The specific experimental steps are as follows: 1g of commercial anatase titanium dioxide powder is ultrasonically dispersed in a 10M NaOH solution. After the powder is evenly dispersed, the suspension is transferred to a polytetrafluoroethylene high-pressure reactor and sealed. It is then placed in a constant temperature oven and kept warm at 200°C for 48 hours. After the reactor is cooled to room temperature, the white precipitate is separated by centrifugation, washed twice with water, and then washed with 0.1M HCl until the supernatant is acidic. Then continue washing with water until the supernatant is neutral and wash with 0.1M AgNO 3 The solution was titrated without precipitation. The obtained white solid precipitate was placed in a forced air drying oven at 80°C and dried overnight. Finally, the obtained solid powder was placed in a muffle furnace and heated to 750°C at a rate of 1°C / min and kept at this temperature for 30 min to obtain the final product, which was labeled as TiO 2 -A;
[0068] S2, dispersing 1 g of the rutile titanium dioxide powder with the (110) crystal plane obtained in step S1 into 100 mL of deionized water for mixing, then performing ultrasonic treatment for 10 min and stirring for 10 min in sequence, then adjusting the pH to 10, and then continuing to add 5 mg of palladium nitrate dihydrate, keeping stirring and keeping warm at 70° C. for 12 hours to obtain a solid powder;
[0069] S3, placing the solid powder in a heating device, heating it to 400°C at a rate of 2°C / min and keeping it at that temperature for 2 hours to obtain Pd / TiO 2 Material.
[0070] Comparative Example 2
[0071] This comparative example proposes a Pd / TiO 2 The material is prepared by the following steps:
[0072] S1. Synthesis of brookite titanium dioxide with exposed (120) crystal face: Using TiCl4 as the titanium source, brookite titanium dioxide with exposed (120) crystal face was prepared by a one-step hydrothermal method. The specific experimental steps are as follows: a 100 ml polytetrafluoroethylene reactor lined with an ice-water bath was placed to keep warm, 60 ml of deionized water was added, and then 1.65 ml of TiCl 4, stirred for 30 minutes, then added 5g of urea, and after it was evenly dissolved, 5ml of sodium lactate solution was added dropwise and stirred for 30 minutes. The above reactor was sealed and placed in a constant temperature oven, kept at 200°C for 12 hours. After the reaction was completed, it was taken out and cooled, and then centrifuged to obtain an off-white powder, which was washed with ethanol and water several times, and placed in a forced air drying oven at 80°C to dry overnight to obtain a brookite titanium dioxide powder with an exposed (120) crystal face. This sample was labeled TiO 2 -B;
[0073] S2, dispersing 1 g of the rutile titanium dioxide powder with the (110) crystal plane obtained in step S1 into 100 mL of deionized water for mixing, then performing ultrasonic treatment for 10 min and stirring for 10 min in sequence, then adjusting the pH to 10, and then continuing to add 5 mg of palladium nitrate dihydrate, keeping stirring and keeping warm at 70° C. for 12 hours to obtain a solid powder;
[0074] S3, placing the solid powder in a heating device, heating it to 400°C at a rate of 2°C / min and keeping it at that temperature for 2 hours to obtain Pd / TiO 2 Material.
[0075] Application Example 1
[0076] The performance test of the prepared samples was carried out to evaluate the catalytic performance with reference to the industrial use. Specifically, the samples of Example 1, Comparative Example 1 and Comparative Example 2 were dispersed in deionized water, and a certain amount of Al 2 O 3 The sol was stirred to prepare a coating slurry, and the cordierite honeycomb ceramics used in engineering were cut into small pieces and immersed in the slurry. After dipping, the pieces were taken out, and the excess slurry was blown out by air flow. Then, the pieces were dried at 120°C for 10 hours, and the temperature was increased to 400°C at 10°C / min and calcined for 2 hours to prepare an industrial monolithic catalyst for subsequent testing. The samples of Example 1, Comparative Example 1 and Comparative Example 2 were marked as Pd / TiO 2 -R, Pd / TiO 2 -A and Pd / TiO 2 -B. Use VOCs solvent and air as test gas, the test air velocity is 12000 / h, and the VOCs concentration is 2000mg / m 3 , catalyst loading amount is 5mL, and the gas temperature at the catalyst inlet is controlled at the test value.
[0077] Combination Figure 2 By comparing the three different catalyst samples, it can be seen that the Pd / TiO 2 -R sample has the highest catalytic activity for styrene, and it can effectively remove styrene at 240°C. 2-A and Pd / TiO 2 -B catalytic performance is basically the same, and effective removal of styrene can only be achieved at 280°C.
[0078] For the above sample Pd / TiO 2 -R was used to test the chlorine resistance. Specifically, the small catalyst sample prepared above was tested with vinyl chloride, styrene and air as test gas, with a test air velocity of 10000 / h and a vinyl chloride concentration of 100 mg / m 3 , styrene concentration is 2000mg / m 3 , the catalyst loading amount is 5mL, the gas temperature at the catalyst inlet is controlled at 240℃, the test is continued for 240 hours, and the change in conversion rate is recorded. Figure 3 It can be seen that after 240 hours of stability testing, the conversion rate of the catalyst decreased by less than 10%. Figure 4 It can be seen that the catalyst after chlorination treatment can still effectively remove styrene at 270°C.
[0079] Pd / TiO prepared in Example 2, Example 3 and Example 4 2 The material has a catalytic performance comparable to that of Example 1 in catalyzing styrene.
[0080] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a chlorine-resistant catalyst, characterized in that: The following steps are involved: S1, adding tetrabutyl titanate dropwise to a stirring HCl solution, and then continuing to stir to obtain a mixed solution, and then transferring the mixed solution to a reaction kettle, and obtaining a rutile titanium dioxide powder with an exposed (110) crystal plane at 160-180° C.; S2, mixing the (110) crystal face rutile titanium dioxide powder obtained in step S1 with water, and then sequentially performing ultrasonic treatment and stirring, and then adjusting the pH to 10-11, and then continuing to add soluble palladium salt and / or soluble platinum salt, and maintaining stirring and heat preservation at 70-80° C. to obtain a solid powder; S3. placing the solid powder in a heating device, heating it to 300-600° C. at a rate of 2-3° C. / min and keeping the temperature to obtain the catalyst.
2. The method for preparing a chlorine-resistant catalyst according to claim 1, characterized in that: In step S1, the concentration of the HCl solution is 6-9 mol / L.
3. The method for preparing a chlorine-resistant catalyst according to claim 2, characterized in that: In step S1, the volume ratio of the tetrabutyl titanate to the HCl solution is 1:(5-6).
4. The method for preparing a chlorine-resistant catalyst according to claim 1, characterized in that: In step S1, the heat preservation time at 160-180°C is 4-6 hours; and / or, in step S1, stirring is continued for 10-30 minutes to obtain the mixed solution.
5. The method for preparing a chlorine-resistant catalyst according to claim 1, characterized in that: In step S2, the rutile titanium dioxide powder with a (110) crystal face and water are mixed in a dosage ratio of (1-2) g:100 mL; and / or, in step S2, the soluble palladium salt is palladium nitrate dihydrate, the soluble platinum salt is platinum nitrate, and the mass ratio of the palladium nitrate dihydrate or the platinum nitrate to the rutile titanium dioxide powder with a (110) crystal face is (5-8) mg:1 g.
6. The method for preparing a chlorine-resistant catalyst according to claim 1, characterized in that: In step S2, the ultrasonic treatment and stirring are performed sequentially, the ultrasonic treatment time is 10-20 minutes, and the stirring time is 10-20 minutes.
7. The method for preparing a chlorine-resistant catalyst according to claim 1, characterized in that: In step S2, the temperature is kept at 70-80°C for 10-12 hours.
8. The method for preparing a chlorine-resistant catalyst according to claim 1, characterized in that: In step S3, the holding time at 300-600°C is 2-3 hours.
9. A chlorine-resistant catalyst, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.