Preparation method and application of MSA / TiO2-x photocatalyst constructed based on M-Ti bimetal MOFs
By using coordination reaction and hydrothermal reaction to prepare MSA/TiO2-x single-atom material in single-atom photocatalyst synthesis, the problems of cumbersome steps and low catalyst activity in the prior art are solved, and the CO2 efficiency and selectivity are achieved Reduction reaction simplifies the preparation process and improves catalytic activity and selectivity.
Patent Information
- Application Number
- CN202411110304.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing single-atom photocatalyst synthesis methods are complicated and the catalyst activity is low, making it difficult to meet the demand for efficient and highly selective reduction of CO2.
By coordinating the metal salt, titanium source, surfactant and ethylene glycol, a bimetallic organic frame structure material is obtained, and combined with the chelating agent through hydrothermal reaction, chelating reaction and lattice rearrangement are performed, and a chelating reaction and lattice rearrangement are prepared. MSA/TiO2-x single atomic material containing oxygen vacancies and metal monoatoms regulates the molar ratio of chelating agents to bimetallic organic frame structure materials to improve catalytic activity and selectivity.
The preparation process is simplified, the catalytic activity and selectivity of MSA/TiO2-x single-atom material is improved, and high catalytic activity and selectivity are shown in CO2 reduction reaction.
Smart Images

Figure CN119016051A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of material synthesis and catalytic reaction, and in particular to a SA / TiO 2-x Single-atom materials, their preparation methods and applications. Background Art
[0002] As fossil fuel resources are becoming increasingly depleted and environmental pollution becomes increasingly serious, it is of great research significance to develop clean energy to replace traditional non-renewable energy. At present, photocatalytic technology can use solar energy to convert CO2 resources into fuels or chemicals, providing a very promising and ideal way to deal with carbon emissions, achieve dual carbon goals and alleviate the energy crisis.
[0003] The design of single-atom active sites has become a frontier research area in heterogeneous catalysis. Single-atom catalysts (SACs) have unique physicochemical properties, such as high active site exposure, strong metal-support interaction, unique electronic structure, and unsaturated coordination environment. These properties are conducive to the efficient separation of photogenerated carriers in the catalyst and the adsorption and activation of CO2 molecules, providing strong support for the exploration of efficient and highly selective reduction of CO2.
[0004] At present, the synthesis methods of single-atom photocatalysts are mainly divided into bottom-up synthesis methods and top-down synthesis methods. Among them, the classic top-down method, such as the "wrap-bake-peel" preparation process, has precise synthesis and preparation, but the steps are cumbersome and the catalyst activity is low. Summary of the invention
[0005] The present invention provides a SA / TiO 2-x Single atom material and its preparation method and application. The MSA / TiO 2-x The preparation process of single-atom materials is simple and the obtained M SA / TiO 2-x Single-atom materials are highly active.
[0006] The present invention provides a kind of M SA / TiO 2-x The method for preparing a single-atom material comprises the following steps:
[0007] The metal salt, titanium source, surfactant and ethylene glycol are mixed to carry out coordination reaction to obtain a bimetallic organic framework structure material;
[0008] The bimetallic organic framework material, the chelating agent and the solvent are mixed and subjected to a hydrothermal reaction to cause a chelating reaction and a lattice rearrangement to obtain the M SA / TiO 2-x Single-atom material; the MSA / TiO 2-x Single-atom materials contain oxygen vacancies and single metal atoms;
[0009] The molar ratio of the chelating agent to the bimetallic organic framework material is 0.5 to 1:1.
[0010] Preferably, the metal salt includes one or more of acetate, hydrochloride, nitrate and carbonate;
[0011] The metal elements in the metal salt include one or more of Co, Ni, Cu, Zn, Mn, Fe, Mg, Ca, Sr and Ba.
[0012] Preferably, the titanium source includes isopropyl titanate and / or tetrabutyl titanate.
[0013] Preferably, it is characterized in that the molar ratio of the titanium source to the metal salt is 1:0.2-5.
[0014] Preferably, the surfactant includes one or more of polyvinyl pyrrolidone, N-methyl pyrrolidone, vinyl pyrrolidone and 2-pyrrolidone.
[0015] Preferably, the mass ratio of the metal salt to the surfactant is 1:0.1-10.
[0016] Preferably, the chelating agent includes one or more of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate and dipotassium ethylenediaminetetraacetate.
[0017] Preferably, the temperature of the hydrothermal reaction is 150-220° C., and the time is 10-30 hours.
[0018] The present invention also provides M prepared by the preparation method described in the above technical solution SA / TiO 2-x Single-atom materials contain oxygen vacancies and single metal atoms.
[0019] The present invention also provides the M described in the above technical solution SA / TiO 2-x Application of single-atom materials as photocatalysts in CO2 reduction reaction.
[0020] The present invention provides a SA / TiO 2-x The method for preparing a single-atom material comprises the following steps:
[0021] The metal salt, titanium source, surfactant and ethylene glycol are mixed to carry out coordination reaction to obtain a bimetallic organic framework structure material;
[0022] The bimetallic organic framework material, the chelating agent and the solvent are mixed and subjected to a hydrothermal reaction to cause a chelating reaction and a lattice rearrangement to obtain the M SA / TiO 2-x Single-atom materials;
[0023] The M SA / TiO 2-x Single-atom materials contain oxygen vacancies and single metal atoms;
[0024] The molar ratio of the chelating agent to the bimetallic organic framework material is 0.5 to 1:1.
[0025] The present invention uses an in-situ topological conversion method to convert the bimetallic organic framework material (M-Ti-EG BMOFs) synthesized by the top-down synthesis strategy into MSA / TiO 2-x The single-atom material was prepared by adjusting the molar ratio of the chelating agent to the M-Ti-EG BMOFs, so that some metal ions in the M-Ti BMOFs were removed by chelation reaction, and the M-Ti-EG BMOFs were rearranged during the hydrothermal process to obtain MSA / TiO containing oxygen vacancies and M single atoms. 2-x photocatalyst, which makes MSA / TiO 2-x The single-atom material has high catalytic activity and selectivity in the photocatalytic CO2 reduction reaction. That is, the present invention prepares MSA / TiO with high catalytic activity and selectivity only by the molar ratio of chelating agent to M-Ti-EG BMOFs. 2-x Single-atom material with simple preparation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the SEM image of Ni-Ti-EG BMOFs precursor;
[0027] Figure 2 is the XRD pattern of Ni-Ti-EG BMOFs precursor;
[0028] Figure 3 FTIR spectrum of Ni-Ti-EG BMOFs precursor;
[0029] Figure 4 For you SA / TiO 2-x HAADF-STEM image of the photocatalyst material;
[0030] Figure 5 For you SA / TiO 2-x XRD patterns of photocatalyst materials;
[0031] Figure 6For you SA / TiO 2-x FTIR spectra of photocatalyst materials;
[0032] Figure 7 The photocatalytic results of the photocatalysts of Example 1 and Comparative Examples 1 to 3 are shown. DETAILED DESCRIPTION
[0033] The present invention provides a SA / TiO 2-x The method for preparing a single-atom material comprises the following steps:
[0034] The metal salt, titanium source, surfactant and ethylene glycol are mixed to carry out coordination reaction to obtain a bimetallic organic framework structure material;
[0035] The bimetallic organic framework material, the chelating agent and the solvent are mixed and subjected to a hydrothermal reaction to cause a chelating reaction and a lattice rearrangement to obtain the M SA / TiO 2-x Single-atom materials;
[0036] The M SA / TiO 2-x Single-atom materials contain oxygen vacancies and single metal atoms;
[0037] The molar ratio of the chelating agent to the bimetallic organic framework material is 0.5-1:1.
[0038] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0039] The present invention mixes metal salt, titanium source, surfactant and ethylene glycol for coordination reaction to obtain a bimetallic organic framework structure material.
[0040] In the present invention, the mixing preferably includes: first mixing the metal salt, the surfactant and ethylene glycol to obtain a first mixture; and second mixing the first mixture with a titanium source.
[0041] In the present invention, the first mixing and the second mixing are preferably performed under stirring conditions.
[0042] In the present invention, the mass ratio of the metal salt to the surfactant is preferably 1:0.1-10, more preferably 1:2-8, more preferably 1:4-6; the surfactant preferably includes one or more of polyvinyl pyrrolidone, N-methyl pyrrolidone, vinyl pyrrolidone and 2-pyrrolidone.
[0043] In the present invention, the volume ratio of the amount of the metal salt to ethylene glycol is preferably 1 mol: 0.2 to 120 L, more preferably 1 mol: 20 to 100 L, and further preferably 1 mol: 40 to 60 L;
[0044] In the present invention, the temperature of the coordination reaction is preferably 20° C., and the time is preferably 12 hours. During the coordination reaction, the metal ions in the metal salt, the titanium in the titanium source and the ethylene glycol undergo a coordination reaction.
[0045] In the present invention, the molar ratio of the titanium source to the metal salt is preferably 1:0.2-5, more preferably 1:1-4, and further preferably 1:2-3; the metal salt preferably includes one or more of acetate, hydrochloride, nitrate and carbonate; the metal element in the metal salt preferably includes one or more of Co, Ni, Cu, Zn, Mn, Fe, Mg, Ca, Sr and Ba; the titanium source preferably includes isopropyl titanate and / or tetrabutyl titanate.
[0046] After the coordination reaction, the method preferably further comprises: separating the product obtained from the coordination reaction, and then washing the separated solid to obtain the bimetallic organic framework material (denoted as M-Ti-EG BMOFs).
[0047] In the present invention, the shape of the M-Ti-EG BMOFs is preferably rod-shaped.
[0048] After obtaining the M-Ti-EG BMOFs, the present invention mixes the bimetallic organic framework material, the chelating agent and the solvent for hydrothermal reaction, so that a chelating reaction and lattice rearrangement occur to obtain the M SA / TiO 2-x Single-atom materials.
[0049] The solvent preferably includes water and ethylene glycol; the volume ratio of the ethylene glycol to water is 1:0.001-100, preferably 1:3-60, and more preferably 1:10-30.
[0050] In the present invention, the molar ratio of the chelating agent to M-Ti-EG BMOFs is preferably 0.5-1:1, more preferably 0.6-0.9:1, and further preferably 0.7-0.8:1; the chelating agent preferably includes one or more of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, and dipotassium ethylenediaminetetraacetate. The present application controls the molar ratio of the chelating agent to M-Ti-EG BMOFs to partially chelate and remove the metal ions in the M-Ti-EG BMOFs, so that the crystal undergoes lattice rearrangement during the hydrothermal process to obtain M containing oxygen vacancies and M single atoms. SA / TiO 2-x Photocatalyst.
[0051] In the present invention, the ratio of the amount of the M-Ti-EG BMOFs to the volume of the solvent is preferably 1 mol: 0.1-600L, more preferably 1 mol: 100-500L, and further preferably 1 mol: 200-300L.
[0052] In the present invention, the temperature of the hydrothermal reaction is preferably 150-220°C, more preferably 160-200°C, and further preferably 170-180°C; the time is preferably 10-30h, more preferably 15-25h, and further preferably 18-20h.
[0053] In the present invention, after the hydrothermal reaction, the method preferably further comprises: separating the product obtained from the hydrothermal reaction, washing and drying the separated solid to obtain the M SA / TiO 2-x Single-atom materials.
[0054] The washing removes the chelate obtained by the chelation reaction.
[0055] The present invention also provides M prepared by the preparation method described in the above technical solution SA / TiO 2-x Single-atom materials contain oxygen vacancies and single metal atoms.
[0056] The present invention also provides the M described in the above technical solution SA / TiO 2-x Application of single-atom materials as photocatalysts in CO2 reduction reaction.
[0057] In the present invention, the application preferably includes: SA / TiO 2-x The single-atom material is mixed with water to obtain a mixture; the mixture is placed in a CO2 environment and the CO2 is irradiated with light to cause a reduction reaction.
[0058] In the present invention, the M SA / TiO 2-x The mass ratio of the monatomic material to water is preferably 1:100 to 5000, more preferably 1:1000 to 4000, and even more preferably 1:2000 to 3000.
[0059] The light source for illumination preferably includes one of an LED lamp in the ultraviolet light band, an LED lamp in the visible light band, a xenon lamp in the ultraviolet light band, and a xenon lamp in the visible light band.
[0060] In the present invention, the reduction reaction is preferably carried out under closed conditions.
[0061] The MSA / TiO provided by the present invention is described below in conjunction with the embodiments.2-x The single-atom material and its preparation method and application are described in detail, but they should not be understood as limiting the scope of protection of the present invention.
[0062] The total volume of the mixed solution added in the embodiment does not exceed 4 / 5 of the total volume of the reaction kettle used, that is, the total volume of the reactants added to the reaction system does not exceed 4 / 5 of the total volume of the reaction system.
[0063] Example 1
[0064] 5mmol Ni(CH3COO)2 and 0.5g polyvinyl pyrrolidone were dissolved in 60mL ethylene glycol, and the solution was stirred evenly. Then 5mmol n-butyl titanate was added to the above solution, stirred evenly, and then the coordination reaction was carried out at room temperature for 12h, and then the Ni-Ti-EG BMOFs precursor was prepared by centrifugal washing.
[0065] Weigh 1 mmol of the prepared M-Ti-EG BMOFs precursor and add it to 60 mL of a mixed solution of water and ethylene glycol (the volume ratio of water to ethylene glycol is 1:3), then add 0.75 mmol of EDTA-2Na, stir the solution evenly, put it into a reactor and react in an oven at 180 °C for 12 h, centrifuge and wash to obtain Ni SA / TiO 2-x Photocatalyst materials.
[0066] Figure 1 It is the SEM image of Ni-Ti-EG BMOFs precursor;
[0067] Figure 2 is the XRD pattern of Ni-Ti-EG BMOFs precursor;
[0068] Figure 3 This is the FTIR spectrum of Ni-Ti-EG BMOFs precursor.
[0069] Depend on Figures 1 to 3 It can be seen that Ni-Ti-EG BMOFs with specific morphology and high crystallinity were successfully prepared.
[0070] Figure 4 For you SA / TiO 2-x HAADF-STEM image of the photocatalyst material;
[0071] Figure 5 For you SA / TiO 2-x XRD patterns of photocatalyst materials;
[0072] Figure 6 For you SA / TiO2-x FTIR spectra of photocatalyst materials.
[0073] Depend on Figures 4 to 6 It can be seen that Ni-Ti-EG BMOFs were used as reaction precursors and Ni containing Ni single atoms and oxygen vacancies was successfully obtained through chelation reaction. SA / TiO 2-x Material.
[0074] Example 2
[0075] 5mmol Co(CH3COO)2 and 0.5g polyvinyl pyrrolidone were dissolved in 60mL ethylene glycol, and the solution was stirred evenly. Then 5mmol n-butyl titanate was added to the above solution, stirred evenly, and then the coordination reaction was carried out at room temperature for 12h, and then the Co-Ti-EG BMOFs precursor was prepared by centrifugal washing.
[0076] Weigh 1 mmol of the Co-Ti-EG BMOFs precursor prepared above and add it to 60 mL of a mixed solution of water and ethylene glycol (the volume ratio of water to ethylene glycol is 1:3), then add 0.75 mmol of EDTA-2Na, stir the solution evenly, put it into a reactor and react in an oven at 180 °C for 12 h, centrifuge and wash to obtain Co SA / TiO 2-x Photocatalyst materials.
[0077] Example 3
[0078] 5mmol Cu(CH3COO)2 and 1g polyvinyl pyrrolidone were dissolved in 60mL ethylene glycol, and the solution was stirred evenly. Then, 1mmol isopropyl titanate was added to the above solution, stirred evenly, and then the coordination reaction was carried out at room temperature for 12h, and then the Cu-Ti-EG BMOFs precursor was prepared by centrifugal washing.
[0079] (2) Weigh 1 mmol of the Cu-Ti-EG BMOFs precursor prepared above and add it to 60 mL of a mixed solution of water and ethylene glycol (the volume ratio of water to ethylene glycol is 1:5), then add 0.75 mmol of EDTA-2Na, stir the solution evenly, put it into a reactor and react in an oven at 180 °C for 12 h, centrifuge and wash to obtain Cu SA / TiO 2-x Photocatalyst materials.
[0080] Example 4
[0081] 5mmol Zn(CH3COO)2 and 0.25g polyvinyl pyrrolidone were dissolved in 60mL ethylene glycol, the solution was stirred evenly, and then 5mmol isopropyl titanate was added to the above solution, stirred evenly and then coordinated at room temperature for 12h, and then centrifuged and washed to prepare the Zn-Ti-EG BMOFs precursor.
[0082] (2) Weigh 1 mmol of the Zn-Ti-EG BMOFs precursor prepared above and add it to a mixed solution of 60 mL of water and ethylene glycol (the volume ratio of water to ethylene glycol is 10:1), then add 0.75 mmol of EDTA-2Na, and after the solution is stirred evenly, put it into a reactor and react in an oven at 180°C for 12 h, and centrifuge and wash to obtain Zn SA / TiO 2-x Photocatalyst materials.
[0083] Comparative Example 1
[0084] (1) 5 mmol Ni(CH3COO)2 and 0.5 g polyvinyl pyrrolidone were dissolved in 60 mL ethylene glycol, and the solution was stirred evenly. Then, 5 mmol n-butyl titanate was added to the above solution, stirred evenly, and the coordination reaction was carried out at room temperature for 12 h. Then, the Ni-Ti-EG BMOFs precursor was prepared by centrifugal washing.
[0085] (2) Weigh 1 mmol of the Ni-Ti-EG BMOFs precursor prepared above and add it to 60 mL of a mixed solution of water and ethylene glycol (the volume ratio of water to ethylene glycol is 1:3) without adding any chelating agent. After the solution is stirred evenly, put it into a reactor and react in an oven at 180°C for 12 h. Centrifuge and wash to obtain a NiTiO3 photocatalyst material.
[0086] Comparative Example 2
[0087] (1) 5 mmol Ni(CH3COO)2 and 0.5 g polyvinyl pyrrolidone were dissolved in 60 mL ethylene glycol, and the solution was stirred evenly. Then, 5 mmol n-butyl titanate was added to the above solution, stirred evenly, and the coordination reaction was carried out at room temperature for 12 h. Then, the Ni-Ti-EG BMOFs precursor was prepared by centrifugal washing.
[0088] (2) Weigh 1 mmol of the Ni-Ti-EG BMOFs precursor prepared above and add it to a mixed solution of 60 mL of water and ethylene glycol (the volume ratio of water to ethylene glycol is 1:3), then add 0.25 mmol of EDTA-2Na, stir the solution evenly, put it into a reactor and react in an oven at 180 °C for 12 h, centrifuge and wash to obtain Ni NP / TiO 2-x Photocatalyst materials.
[0089] Comparative Example 3
[0090] (1) 5 mmol Ni(CH3COO)2 and 0.5 g polyvinyl pyrrolidone were dissolved in 60 mL ethylene glycol, and the solution was stirred evenly. Then, 5 mmol n-butyl titanate was added to the above solution, stirred evenly, and the coordination reaction was carried out at room temperature for 12 h. Then, the Ni-Ti-EG BMOFs precursor was prepared by centrifugal washing.
[0091] (2) Weigh 1 mmol of the Ni-Ti-EG BMOFs precursor prepared above and add it to a mixed solution of 60 mL of water and ethylene glycol (the volume ratio of water to ethylene glycol is 1:3), then add 1.5 mmol of EDTA-2Na, stir the solution evenly, put it into a reactor and react in an oven at 180 °C for 12 h, centrifuge and wash to obtain TiO 2-x Photocatalyst materials.
[0092] Weigh 20 mg of the photocatalysts of Example 1 and Comparative Examples 1 to 3 respectively and place them in a reaction system of 15 mL of pure water. Then seal the reaction system and use a vacuum pump to evacuate the system, then introduce CO2 gas, and finally fill the entire reaction device with CO2 gas (the pressure in the device is 0.04 MPa). Under room temperature magnetic stirring and illumination, take samples every 1 hour, and use gas chromatography to detect the amount of CO gas generated. The photocatalytic results of the photocatalysts of Example 1 and Comparative Examples 1 to 3 are shown in Figure 1. Figure 7 As shown in Table 1.
[0093] Table 1 Photocatalytic results of the photocatalysts of Example 1 and Comparative Examples 1 to 3
[0094]
[0095] Depend on Figure 7 As shown in Table 1, it is obvious that Ni SA / TiO 2-x It exhibits high yield and selectivity in the photocatalytic reduction of CO2 to produce CO.
[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A M SA / TiO 2-x A method for preparing a single-atom material, characterized in that: The following steps are involved: The metal salt, titanium source, surfactant and ethylene glycol are mixed to carry out coordination reaction to obtain a bimetallic organic framework structure material; The bimetallic organic framework material, the chelating agent and the solvent are mixed and subjected to a hydrothermal reaction to cause a chelating reaction and a lattice rearrangement to obtain the M SA / TiO 2-x Single-atom material; the M SA / TiO 2-x Single-atom materials contain oxygen vacancies and single metal atoms; The molar ratio of the chelating agent to the bimetallic organic framework material is 0.5-1:
1.
2. The preparation method according to claim 1, characterized in that: The metal salt includes one or more of acetate, hydrochloride, nitrate and carbonate; The metal elements in the metal salt include one or more of Co, Ni, Cu, Zn, Mn, Fe, Mg, Ca, Sr and Ba.
3. The preparation method according to claim 1, characterized in that: The titanium source includes isopropyl titanate and / or tetrabutyl titanate.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The molar ratio of the titanium source to the metal salt is 1:0.2-5.
5. The preparation method according to claim 1, characterized in that: The surfactant includes one or more of polyvinyl pyrrolidone, N-methyl pyrrolidone, vinyl pyrrolidone and 2-pyrrolidone.
6. The preparation method according to claim 1 or 5, characterized in that: The mass ratio of the metal salt to the surfactant is 1:0.1-10.
7. The preparation method according to claim 1, characterized in that: The chelating agent includes one or more of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate and dipotassium ethylenediaminetetraacetate.
8. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 150-220° C. and the time is 10-30 hours.
9. M prepared by the preparation method according to any one of claims 1 to 8 SA / TiO 2-x Single-atom materials, characterized in that Contains oxygen vacancies and single metal atoms.
10. The M according to claim 9 SA / TiO 2-x Application of single-atom materials as photocatalysts in CO2 reduction reaction.
Citation Information
Patent Citations
Monatomic catalyst with high catalytic activity and preparation method and application thereof
CN109939718A
TiO2-x-based hindered Lewis acid-base pair photocatalyst as well as preparation method and application thereof
CN112569919A
Monatomic loaded photo-titanium dioxide catalytic material and preparation method thereof
CN112717908A
Method for preparing superfine cerium dioxide supported metal monatomic catalyst from cluster-based framework material
CN114293223A
Preparation method of CO2 photo-reduction catalyst
CN114950561A