CuO-Ag2O mesoporous composite material as well as preparation method and application thereof

Through CuO-Ag2O mesoporous composite material as a catalyst, the problem of insufficient catalyst activity and stability in the preparation of 3-hydroxy-3-methyl-1-butyraldehyde is solved, and high efficiency, low energy consumption and continuous production are achieved, reducing The cost of the three waste treatment meets the requirements of green and environmental protection.

CN119016066APending Publication Date: 2024-11-26WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411126138.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the preparation method of 3-hydroxy-3-methyl-1-butyraldehyde has problems such as low yield, complex reaction process, large safety hazards, and difficulty in achieving continuous industrial production, especially the lack of activity and stability of the catalyst. , resulting in high process energy consumption and high cost of three waste treatment.

Method used

CuO-Ag2O mesoporous composite material is used as a catalyst to form a CuO-Ag2O mesoporous composite material with a honeycomb porous structure through the preparation method, which is used to catalyze the preparation of 3-hydroxy-3-methyl-1-butyraldehyde and improve catalysis. Activity and stability, and reduce reaction temperature and energy consumption.

Benefits of technology

It realizes high yield and high selectivity preparation of 3-hydroxy-3-methyl-1-butyraldehyde, reduces process energy consumption and three waste generation, improves the service life of the catalyst and process continuous production capacity, and complies with green environmental protection. idea.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016066A_ABST
    Figure CN119016066A_ABST
Patent Text Reader

Abstract

The invention provides a CuO-Ag2O mesoporous composite material, the total pore volume of the CuO-Ag2O mesoporous composite material is 0.4-1.6 cm < 3 > / g, the BET surface area is 400-900 m < 2 > / g, and the molar ratio of Cu to Ag is 1: (0.1-1). The invention also provides a preparation method and application of the mesoporous composite material. The invention further provides a preparation method of the 3-hydroxyl-3-methyl-1-butyraldehyde, and the 3-hydroxyl-3-methyl-1-butyraldehyde is prepared by the method. The CuO-Ag2O mesoporous composite material provided by the invention has abundant honeycomb mesoporous channels, and active sites are uniformly dispersed, so that the CuO-Ag2O mesoporous composite material has very high catalytic activity and stability. The preparation method of 3-hydroxy-3-methyl-1-butyraldehyde provided by the invention can realize continuous production, has the advantages of mild process conditions, strong operability and low yield of three wastes, and accords with the idea of green environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalysts, in particular to a CuO-Ag2O mesoporous composite material, and also to a preparation method of the CuO-Ag2O mesoporous composite material and use of the CuO-Ag2O mesoporous composite material as a dehydrogenation reaction catalyst. The present invention further relates to a preparation method of 3-hydroxy-3-methyl-1-butyraldehyde. Background Art

[0002] 3-Hydroxy-3-methyl-1-butyraldehyde is an important intermediate for the synthesis of β-methyl-β-hydroxybutyric acid. β-methyl-β-hydroxybutyric acid can be obtained after oxidation reaction of the intermediate. β-methyl-β-hydroxybutyric acid can be obtained after salt formation reaction of β-methyl-β-hydroxybutyric acid to obtain calcium β-methyl-β-hydroxybutyrate, which has the effects of promoting bone health and muscle growth, reducing sports injuries, and preventing myosin loss.

[0003] The chemical structure of 3-hydroxy-3-methyl-1-butyraldehyde is as follows:

[0004]

[0005] 3-Hydroxy-3-methyl-1-butyraldehyde is usually prepared by dehydrogenation or oxidation reaction with 3-methyl-1,3-butanediol as raw material. WO 2009005675A1 reports a method for synthesizing 3-hydroxy-3-methyl-1-butyraldehyde: 3-methyl-1,3-butanediol and Dess-Martin reagent react at room temperature in a DCM solution. Although this traditional oxidation method has a simple process, the maximum yield is only 69%. At the same time, the reaction reagent needs to use Dess-Martin reagent, which decomposes in large quantities when exposed to water, has certain explosiveness, and has harsh storage conditions, thus posing safety risks. In addition, the reaction adopts an intermittent feeding method, which strictly limits the industrial continuous production of 3-hydroxy-3-methyl-1-butyraldehyde. WO 2020251006A1 reports the use of tetramethylpiperidine (Tempo reagent) / sodium hypochlorite as an oxidizing reagent, with a maximum reaction yield of 90.60%. However, the process is a purely intermittent operation with a large number of intermediate unit operations, making it difficult to industrialize continuous production. At the same time, the reaction needs to be carried out at low temperatures, resulting in high process energy consumption, and sodium hypochlorite will produce a large amount of chlorine-containing wastewater, resulting in high costs for treating the three wastes.

[0006] Therefore, it is urgent to develop a 3-methyl-1,3-butanediol dehydrogenation catalyst with high catalytic activity and long service life, so as to reduce the generation of three wastes, improve the yield of dehydrogenation reaction, reduce reaction energy consumption, and realize process continuity. Summary of the invention

[0007] In order to make up for the deficiencies in the prior art, an object of the present invention is to provide a CuO-Ag2O mesoporous composite material, which has unique honeycomb porous characteristics and contains two active metal components uniformly dispersed, and thus has very excellent catalytic performance and stability, and can be used as a catalyst for various types of reactions.

[0008] Another object of the present invention is to provide a preparation method and use of the CuO-Ag2O mesoporous composite material.

[0009] Another object of the present invention is to provide a method for preparing 3-hydroxy-3-methyl-1-butyraldehyde.

[0010] The first aspect of the present invention provides a CuO-Ag2O mesoporous composite material having a total pore volume of 0.4 to 1.6 cm 3 / g, BET surface area is 400~900m 2 / g, wherein the molar ratio of Cu to Ag is 1:0.1~1.

[0011] The CuO-Ag2O mesoporous composite material provided by the present invention is in powder form, has uniform particle size and has abundant honeycomb mesoporous channels (such as Figure 1 As shown in the figure, the total pore volume and the total specific surface area are significantly improved, which can make the two active metal components have a higher dispersion, thereby generating more active sites and exerting the synergistic effect of the two, thereby achieving higher catalytic activity and stability, and can be applied to various reaction types such as dehydrogenation reaction (or "oxidation reaction"), for example, it can be used to catalyze the synthesis of 3-hydroxy-3-methyl-1-butyraldehyde.

[0012] The total pore volume of the mesoporous composite material provided by the present invention can be 0.4 to 1.6 cm 3 / g, for example, about 0.4 cm 3 / g, about 0.5cm 3 / g, about 0.55cm 3 / g, about 0.6cm 3 / g, about 0.65cm 3 / g, about 0.7cm 3 / g, about 0.75cm 3 / g, about 0.8cm 3 / g, about 0.85cm 3 / g, about 0.9cm 3 / g, about 0.95cm 3 / g, about 1cm 3 / g, about 1.1cm 3 / g, about 1.2cm 3 / g, about 1.3cm 3 / g, about 1.4cm 3 / g, about 1.5cm 3 / g, about 1.6cm 3 / g or any numerical range. In some preferred embodiments, the total pore volume of the mesoporous composite material may be 0.5 to 1.2 cm 3 / g, for example, 0.65 to 1.1 cm 3 / g.

[0013] The mesoporous composite material provided by the present invention has a BET surface area of ​​400 to 900 m 2 / g, for example, about 400 m 2 / g, about 450m 2 / g, about 500m 2 / g, about 550m 2 / g, about 580m 2 / g, about 600m 2 / g, about 620m 2 / g, about 650m 2 / g, about 680m 2 / g, about 700m 2 / g, about 720m 2 / g, about 750m 2 / g, about 780m 2 / g, about 800m 2 / g, about 850m 2 / g, about 900m 2 / g or any numerical range. In some preferred embodiments, the BET surface area of ​​the mesoporous composite material may be 500 to 800 m 2 / g, for example, 550 to 750 m 2 / g.

[0014] In the mesoporous composite material provided by the present invention, the molar ratio of Cu to Ag can be 1:0.1-1, for example, about 1:0.1, about 1:0.15, about 1:0.2, about 1:0.25, about 1:0.3, about 1:0.35, about 1:0.4, about 1:0.45, about 1:0.5, about 1:0.55, about 1:0.6, about 1:0.65, about 1:0.7, about 1:0.75, about 1:0.8, about 1:0.9, about 1:1 or any numerical range. In some preferred embodiments, the molar ratio of Cu to Ag in the mesoporous composite material can be 1:0.2-0.8, for example, 1:0.25-0.55.

[0015] In the mesoporous composite material provided by the present invention, the particle size of the CuO-Ag2O mesoporous composite material can be 1 to 6 mm. In some preferred embodiments, the particle size of the CuO-Ag2O mesoporous composite material can be 2 to 4 mm.

[0016] The second aspect of the present invention provides a method for preparing the CuO-Ag2O mesoporous composite material, which comprises the following steps:

[0017] S1: preparing spherical Cu-Ag-Al alloy powder with a particle size of 1 to 6 mm;

[0018] S2: adding the Cu-Ag-Al alloy powder into an alkaline solution to remove Al therein; and

[0019] S3: drying and calcining the alloy powder after removing Al to obtain the CuO-Ag2O mesoporous composite material.

[0020] In the preparation method provided by the present invention, Cu-Ag-Al alloy powder is first formed, and then dissolved by alkaline solution to remove Al in the alloy, so that the obtained alloy particles can have a large number of honeycomb mesoporous channels, and the channel size is relatively uniform. After high-temperature calcination, the alloy forms a metal oxide composite, and the thermal stability is greatly improved, and the catalytic activity is also improved.

[0021] In the preparation method provided by the present invention, the step S1 may further include the following process: heating and melting the metal elements Cu, Ag and Al under an inert atmosphere (e.g., a nitrogen atmosphere) to form a Cu-Ag-Al alloy and crushing it into debris, and then heating the obtained debris in a plasma torch to form a spherical Cu-Ag-Al alloy powder (i.e., a thermal spray method); wherein the molar ratio of the metal elements Cu, Ag and Al may be 1:0.1 to 1.5:0.6 to 2. In some preferred embodiments, the molar ratio of the metal elements Cu, Ag and Al may be 1:0.2 to 1:1 to 1.6, for example, 1:0.2 to 0.65:1.2 to 1.55.

[0022] In the preparation method provided by the present invention, the particle size of the spherical Cu-Ag-Al alloy powder can be further 2 to 4 mm.

[0023] In the preparation method provided by the present invention, the step S2 may further include the following process: adding the Cu-Ag-Al alloy powder to an alkaline solution at 20 to 60° C. and stirring to remove Al therein. In some preferred embodiments, the temperature during stirring may be 30 to 45° C. Further, the stirring time may be 1 to 10 hours, for example, 2 to 5 hours.

[0024] In the preparation method provided by the present invention, the alkaline solution can be any kind of alkaline solution that can remove Al but does not react with Cu and Ag, and can include solutions of organic bases and inorganic bases. In some preferred embodiments, the alkaline solution can be an aqueous solution formed by one or more of sodium hydroxide, potassium hydroxide, and calcium hydroxide at a concentration of 5 to 25 wt.% (for example, 10 to 15 wt.%). In other preferred embodiments, the amount of the alkaline solution can be 3 to 10 times, for example, 3 to 6 times, of the Cu-Ag-Al alloy powder by mass.

[0025] In the preparation method provided by the present invention, in the step S3, the drying temperature can be 90-150° C., for example, 100-130° C.; the drying time can be 2-15 hours, for example, 5-10 hours.

[0026] In the preparation method provided by the present invention, in step S3, the calcination temperature can be 400-700° C., for example, 550-600° C.; the calcination time can be 5-15 hours, for example, 6-10 hours; and the calcination pressure can be normal pressure.

[0027] According to a specific embodiment of the preparation method of the present invention, the preparation process of the CuO-Ag2O mesoporous composite material may include: heating metal elements Cu, Ag and Al to 1100-1300°C under a nitrogen atmosphere, stopping heating after all metals are melted, cooling to room temperature under a nitrogen atmosphere to form a Cu-Ag-Al alloy, crushing it into fragments with a size of 5-12 mm, and then feeding the obtained fragments into a plasma torch through a carrier gas argon (the process parameters are as follows: the powder feeding rate can be 1-5 g / min, the carrier gas flow rate can be 1-7 slpm, and the power can be 5-20 KW), forming spherical Cu-Ag-Al alloy powder therein, screening out alloy powder with a particle size of 2-4 mm, adding 10-15wt.% NaOH solution thereto, stirring and reacting at 35-45°C for 3-5h, then filtering, washing, drying, and finally calcining at 550-600°C for 6-8h to obtain the CuO-Ag2O mesoporous composite material.

[0028] The third aspect of the present invention provides the use of the CuO-Ag2O mesoporous composite material described in the first aspect of the present invention, or the CuO-Ag2O mesoporous composite material prepared by the preparation method described in the second aspect of the present invention as a dehydrogenation catalyst (i.e., a catalyst for dehydrogenation reaction or oxidation reaction).

[0029] In some preferred embodiments, the dehydrogenation catalyst is a catalyst for preparing 3-hydroxy-3-methyl-1-butyraldehyde using 3-methyl-1,3-butanediol as a raw material. The CuO-Ag2O mesoporous composite material provided by the present invention is particularly suitable for catalytic preparation of 3-hydroxy-3-methyl-1-butyraldehyde, the dehydrogenation reaction can be carried out at a relatively low temperature, the conditions are mild and easy to control, the target product yield is high, the selectivity is good, and the composite material used as a catalyst also has the advantages of easy recovery and good stability, and the service life can be greatly increased.

[0030] The fourth aspect of the present invention provides a method for preparing 3-hydroxy-3-methyl-1-butyraldehyde, which uses 3-methyl-1,3-butanediol as a raw material and carries out a dehydrogenation reaction in the presence of a dehydrogenation catalyst to obtain the 3-hydroxy-3-methyl-1-butyraldehyde, wherein the dehydrogenation catalyst is the CuO-Ag2O mesoporous composite material described in the first aspect of the present invention, or the CuO-Ag2O mesoporous composite material obtained by the preparation method described in the second aspect of the present invention.

[0031] In the preparation method of 3-hydroxy-3-methyl-1-butyraldehyde provided by the present invention, the dehydrogenation reaction can be carried out at a relatively low temperature, for example, not exceeding 200° C. In some preferred embodiments, the reaction temperature of the dehydrogenation reaction can be 150 to 200° C. In some more preferred embodiments, the reaction temperature of the dehydrogenation reaction can be 150 to 180° C., for example, 170° C.

[0032] The preparation method of 3-hydroxy-3-methyl-1-butyraldehyde provided by the present invention can be applicable to intermittent production or continuous production. In some preferred embodiments, the preparation method can be a continuous process, that is, applicable to continuous production.

[0033] In the preparation method of 3-hydroxy-3-methyl-1-butyraldehyde provided by the present invention, the dehydrogenation reaction can be carried out in a fixed bed reactor, that is, the CuO-Ag2O mesoporous composite material used as a dehydrogenation catalyst is filled in the fixed bed, and then the preheated 3-methyl-1,3-butanediol raw material is transported to the catalyst bed for reaction. In some preferred embodiments, the diameter of the fixed bed can be 1 to 3 cm, for example, 1.5 to 2 cm, and the bed height can be 1 to 3 m, for example, 1.5 to 2 m.

[0034] In the preparation method of 3-hydroxy-3-methyl-1-butyraldehyde provided by the present invention, the mass space velocity of the 3-methyl-1,3-butanediol can be determined according to the actual production scale. In some preferred embodiments, the mass space velocity of the 3-methyl-1,3-butanediol can be 1 to 20 h -1 , for example, 4 to 8 hours-1 .

[0035] The preparation method of 3-hydroxy-3-methyl-1-butyraldehyde provided by the present invention may also include the following post-treatment process: the reaction liquid obtained by the dehydrogenation reaction is subjected to reduced pressure distillation, and the fraction at 138-140°C / 2Kpa is collected, which is 3-hydroxy-3-methyl-1-butyraldehyde.

[0036] In the above-mentioned preparation method provided by the present invention, the desired material can be obtained through a separation step, and the separation equipment or method can be a common equipment or method in the art, including but not limited to natural sedimentation, (normal pressure or vacuum) filtration, centrifugation and the like and their common equipment.

[0037] In the above-mentioned preparation method provided by the present invention, the washing step refers to washing the material with distilled water or deionized water until the surface of the material is close to or neutral, and the number of washing times can be adjusted according to actual conditions, for example, it can be 2 to 5 times, usually 3 times.

[0038] The technical solution provided by the present invention has the following advantages:

[0039] (1) The CuO-Ag2O mesoporous composite material provided by the present invention has abundant honeycomb-like mesoporous channels, and the two metal active components act synergistically and have high dispersibility. Therefore, the composite material has high catalytic activity and stability and is very suitable for use as an industrial catalyst.

[0040] (2) The CuO-Ag2O mesoporous composite material provided by the present invention can be used as a dehydrogenation catalyst in the preparation of 3-hydroxy-3-methyl-1-butyraldehyde. The reaction temperature can be reduced to 150°C, the selectivity of the target product can be as high as 95%, and the yield can reach about 80%, or even higher.

[0041] (3) The preparation method of 3-hydroxy-3-methyl-1-butyraldehyde provided by the present invention can achieve long-term, continuous production, mild process conditions, strong operability, low output of three wastes, long catalyst service life, and conforms to the concept of green environmental protection. Therefore, it has very important economic and social value. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is the SEM image of the CuO-Ag2O composite material prepared in Example 1. DETAILED DESCRIPTION

[0043] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments.

[0044] The sources of the raw materials or reagents used in the embodiments and comparative examples of the present invention are as follows:

[0045] The purity of copper powder, silver powder and aluminum rod were all >99.9%, and they were all purchased from Beijing Inokai Technology Co., Ltd.; 3-methyl-1,3-butanediol was analytical grade and purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; the purity of sodium hydroxide was >99%, and it was purchased from Beijing Inokai Technology Co., Ltd.

[0046] Unless otherwise specified, other raw materials or reagents were commercially available and of analytical or chemical purity.

[0047] The following test methods were used in the embodiments and comparative examples of the present invention:

[0048] 3-Hydroxy-3-methyl-1-butyraldehyde was analyzed by GC-9800 chromatograph, and the chromatographic conditions were as follows: initial temperature was 80°C, maintained for 2 min, programmed to 280°C at a rate of 10°C / min, and retained for 5 min; vaporization chamber temperature was 300°C, detection chamber temperature was 300°C; FID detection; injection volume was 0.2 μL.

[0049] The percentages used in the embodiments and comparative examples of the present invention are all mass percentages unless otherwise specified.

[0050] Example 1

[0051] (1) Preparation of CuO-Ag2O composites

[0052] Take 128g of single element Cu, 75.6g of single element Ag and 72.85g of single element Al, add them into a crucible, heat to 1200℃ under a nitrogen atmosphere, stop heating after all the metals are melted, cool to room temperature under a nitrogen atmosphere, use a ball mill to crush the obtained alloy to form metal debris, sieve to screen out 5-12mm alloy debris, and send the alloy debris into a plasma torch through carrier gas argon (process parameters are as follows: powder feeding rate is 3g / min, carrier gas flow rate is 2.5slpm, power is 12KW), the alloy debris melts in a very short time and forms a sphere under the action of surface tension. The obtained spherical Cu-Ag-Al alloy powder was cooled and sieved to screen out powder with a particle size of 2-4 mm, and then added to 1500 g of 15wt% NaOH solution and stirred for reaction at 35°C for 3.5 h. The solid was then filtered, washed, and dried at 120°C for 7 h. Finally, the dried solid was placed in a muffle furnace at 580°C and calcined in an air atmosphere for 7.5 h to obtain a porous CuO-Ag2O composite material.

[0053] The characterization data of the composite material obtained above are as follows: 铜 :n 银 =1:0.3 (molar ratio), particle size distribution is 2.2-4 mm, BET surface area is 674 m 2 / g, pore volume 0.85cm 3 / g, the pore size distribution is 3.2~18nm, which shows that it is a mesoporous material. The SEM picture is as follows Figure 1 As shown, it can be seen that the composite material has a honeycomb pore structure.

[0054] (2) Catalytic performance evaluation

[0055] 200g CuO-Ag2O composite material was loaded as catalyst into a fixed bed reaction tube with a diameter of 20mm and a length of 1500mm. The preheater and bed temperature were set to 170℃. The nitrogen valve was opened at the same time and nitrogen was replaced for 10min. After the temperature reached the set value, the raw material 3-methyl-1,3-butanediol was heated for 4h. -1 The raw materials are preheated in a preheater and then enter the catalyst bed to react. After the reaction is completed, the reaction liquid is placed in a vacuum distillation device for vacuum distillation, and the fraction collected at 138-140℃ / 2Kpa is 3-hydroxy-3-methyl-1-butyraldehyde.

[0056] The selectivity of the target product calculated from the analysis of the reaction liquid before distillation and the product obtained by distillation was 95.2%, and the yield was 80.3%.

[0057] The reaction selectivity and product yield data of the catalyst during long-term operation are shown in Table 1.

[0058] Table 1

[0059] Catalyst operation time / h Reaction selectivity / % Product yield / % 0 95.2 80.3 100 94.8 79.9 300 94.5 79.6 500 94.1 79.2

[0060] From the results in Table 1, it can be seen that after the catalyst bed has been running for a long time, the catalyst still has excellent catalytic performance, and the selectivity and product yield of the target product are maintained at a high level, indicating that the catalyst has good stability, and thus the service life can be greatly improved.

[0061] Example 2

[0062] (1) Preparation of CuO-Ag2O composites

[0063] Take 128g of single element Cu, 54g of single element Ag and 70.2g of single element Al, and obtain spherical Cu-Ag-Al alloy powder according to the method of Example 1. After the alloy powder is cooled, it is sieved to screen out powder with a particle size of 2-4mm, and then added to 1500g of 10wt% NaOH solution, stirred and reacted at 40°C for 4h, then the solid was filtered, washed, and dried at 130°C for 8h. Finally, the dried solid was placed in a muffle furnace at 580°C and calcined in an air atmosphere for 8h to obtain a porous CuO-Ag2O composite material.

[0064] The characterization data of the composite material obtained above are as follows: 铜 :n银 =1:0.22 (molar ratio), particle size distribution is 2-4 mm, BET surface area is 580 m 2 / g, pore volume 0.65cm 3 / g, and the pore size distribution is between 3.2 and 18 nm.

[0065] (2) Catalytic performance evaluation

[0066] 200 g of the CuO-Ag2O composite material prepared above was loaded as a catalyst into a fixed bed reaction tube with a diameter of 20 mm and a length of 1500 mm. The preheater and the bed temperature were set to 170 °C. At the same time, the nitrogen valve was opened and nitrogen was replaced for 10 min. After the temperature reached the set value, the raw material 3-methyl-1,3-butanediol was heated for 6 h. -1 The raw materials are preheated in the preheater and then enter the catalyst bed to react. After the reaction is completed, the reaction liquid is placed in a vacuum distillation device for vacuum distillation, and the fraction at 138-140℃ / 2Kpa is collected, which is 3-hydroxy-3-methyl-1-butyraldehyde. The selectivity of the target product is 95.8%, and the product yield is 76.64%.

[0067] Example 3

[0068] (1) Preparation of CuO-Ag2O composites

[0069] Take 128g of single element Cu, 118.8g of single element Ag and 81g of single element Al, and obtain spherical Cu-Ag-Al alloy powder according to the method of Example 1. After the alloy powder is cooled, it is sieved to screen out powder with a particle size of 2-4mm, and then added to 1500g of 15wt% NaOH solution, stirred and reacted at 40°C for 4h, then the solid was filtered, washed, and dried at 130°C for 8h. Finally, the dried solid was placed in a muffle furnace at 600°C and calcined in an air atmosphere for 7h to obtain a porous CuO-Ag2O composite material.

[0070] The characterization data of the composite material obtained above are as follows: 铜 :n 银 =1:0.54 (molar ratio), particle size distribution is 2.15-4 mm, BET surface area is 745 m 2 / g, pore volume 1.1cm 3 / g, and the pore size distribution is between 4.3 and 18 nm.

[0071] (2) Catalytic performance evaluation

[0072] 200 g of the CuO-Ag2O composite material prepared above was loaded as a catalyst into a fixed bed reaction tube with a diameter of 20 mm and a length of 1500 mm. The preheater and the bed temperature were set to 150 °C. The nitrogen valve was opened at the same time and nitrogen was replaced for 10 min. After the temperature reached the set value, the raw material 3-methyl-1,3-butanediol was heated for 4 h. -1 The raw materials are preheated in the preheater and then enter the catalyst bed to react. After the reaction is completed, the reaction liquid is placed in a vacuum distillation device for vacuum distillation, and the fraction at 138-140℃ / 2Kpa is collected, which is 3-hydroxy-3-methyl-1-butyraldehyde. The selectivity of the target product is 96.2%, and the product yield is 79.8%.

[0073] Comparative Example 1

[0074] (1) Preparation of CuO-Ag2O composites

[0075] Take 128g of single element Cu, 54g of single element Ag and 23.4g of single element Al, and obtain spherical Cu-Ag-Al alloy powder according to the method of Example 1. After the alloy powder is cooled, it is sieved to screen out powder with a particle size of 2-4mm, and then added to 1500g of 10wt% NaOH solution, stirred and reacted at 40°C for 4h, then the solid was filtered, washed, and dried at 130°C for 8h. Finally, the dried solid was placed in a muffle furnace at 580°C and calcined in an air atmosphere for 8h to obtain a CuO-Ag2O composite material.

[0076] The characterization data of the composite material obtained above are as follows: 铜 :n 银 =1:0.23 (molar ratio), particle size distribution is 2-4 mm, BET surface area is 210 m 2 / g, pore volume 0.21cm 3 / g, and the pore size distribution is between 3.2 and 13 nm.

[0077] (2) Catalytic performance evaluation

[0078] 200 g of the CuO-Ag2O composite material prepared above was loaded as a catalyst into a fixed bed reaction tube with a diameter of 20 mm and a length of 1500 mm. The preheater and the bed temperature were set to 170 ° C. At the same time, the nitrogen valve was opened and nitrogen was replaced for 10 min. After the temperature reached the set value, the raw material 3-methyl-1,3-butanediol was heated for 4 h. -1The raw materials are preheated in the preheater and then enter the catalyst bed to react. After the reaction is completed, the reaction liquid is placed in a vacuum distillation device for vacuum distillation, and the fraction at 138-140℃ / 2Kpa is collected, which is 3-hydroxy-3-methyl-1-butyraldehyde. The selectivity of the target product is 43.2%, and the product yield is 15.12%.

[0079] It can be seen from the results of Comparative Example 1 that when the amount of Al used is too small, abundant honeycomb-like mesoporous channels cannot be formed, and the BET surface area and pore volume of the resulting composite material are greatly reduced, thereby significantly reducing the catalytic performance of the composite material.

[0080] Unless otherwise defined, the terms used in the present invention have the meanings commonly understood by those skilled in the art.

[0081] The embodiments described in the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, changes and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above embodiments, but is only limited by the claims.

Claims

1. A CuO-Ag 2 O mesoporous composite materials, It is characterized in that The CuO-Ag 2 The total pore volume of the mesoporous composite material is 0.4-1.6 cm 3 / g, BET surface area is 400~900m 2 / g, wherein the molar ratio of Cu to Ag is 1:0.1~1.

2. CuO-Ag according to claim 1 2 O mesoporous composite materials, It is characterized in that The CuO-Ag 2 The total pore volume of the mesoporous composite material is 0.5-1.2 cm 3 / g, BET surface area is 500~800m 2 / g, wherein the molar ratio of Cu to Ag is 1:0.2~0.

8.

3. CuO-Ag according to claim 1 or 2 2 O mesoporous composite materials, It is characterized in that The CuO-Ag 2 The particle size of the mesoporous composite material is 1 to 6 mm, preferably 2 to 4 mm; More preferably, the CuO-Ag 2 OThe mesoporous composite material has a honeycomb mesoporous channel structure.

4. The CuO-Ag according to any one of claims 1 to 3 2 O Preparation method of mesoporous composite material, It is characterized in that The following steps are involved: S1: preparing spherical Cu-Ag-Al alloy powder with a particle size of 1 to 6 mm; S2: adding the Cu-Ag-Al alloy powder into an alkaline solution to remove Al therein; and S3: Dry and calcine the alloy powder after removing Al to obtain the CuO-Ag 2 O mesoporous composite materials.

5. The preparation method according to claim 4, It is characterized in that The step S1 comprises the following process: heating and melting metal elements Cu, Ag and Al in an inert atmosphere to form a Cu-Ag-Al alloy and crushing the alloy into fragments, and then heating the obtained fragments in a plasma torch to form spherical Cu-Ag-Al alloy powder; wherein the molar ratio of the metal elements Cu, Ag and Al is 1:0.1-1.5:0.6-2, preferably 1:0.2-1:1-1.

6.

6. The preparation method according to claim 4 or 5, It is characterized in that The alkaline solution is an aqueous solution of one or more of sodium hydroxide, potassium hydroxide and calcium hydroxide at a concentration of 5 to 25 wt.%.

7. The preparation method according to any one of claims 4 to 6, It is characterized in that In step S3, the drying temperature is 90 to 150° C. and the drying time is 2 to 15 hours; and / or The calcination temperature is 400-700°C, and the calcination time is 5-15h.

8. The CuO-Ag according to any one of claims 1 to 3 2 O mesoporous composite material, or CuO-Ag prepared by the preparation method according to any one of claims 4 to 7 2 O Use of mesoporous composite materials as dehydrogenation catalysts; Preferably, the dehydrogenation catalyst is a catalyst for preparing 3-hydroxy-3-methyl-1-butyraldehyde using 3-methyl-1,3-butanediol as a raw material.

9. A method for preparing 3-hydroxy-3-methyl-1-butyraldehyde, It is characterized in that Using 3-methyl-1,3-butanediol as a raw material, a dehydrogenation reaction is carried out in the presence of a dehydrogenation catalyst to obtain the 3-hydroxy-3-methyl-1-butyraldehyde, wherein the dehydrogenation catalyst is the CuO-Ag according to any one of claims 1 to 3. 2 O mesoporous composite material, or CuO-Ag prepared by the preparation method according to any one of claims 4 to 7 2 O mesoporous composite materials.

10. The preparation method according to claim 9, It is characterized in that The reaction temperature of the dehydrogenation reaction is 150-200°C, preferably 150-180°C; Preferably, the preparation method is a continuous process.