Preparation method of photocatalytic composite material based on Ta3N5-MoSx heterojunction
By preparing Ta3N5/MoSx heterojunction, the problems of insufficient absorbance and photoelectric performance of existing photocatalytic materials are solved, and efficient photocatalytic performance improvement is achieved.
Patent Information
- Application Number
- CN202410984265.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The absorbance and photoelectric properties of existing Ta3N5/MoS2 heterojunction photocatalytic materials have not yet reached the ideal level, and there is a lack of a controllable method for compounding MoSx and Ta3N5 into heterojunction.
A step-by-step preparation method is adopted: first prepare Ta3N5 nanoparticles and MoSx, and then form Ta3N5/MoSx heterojunction through ultrasound and high-temperature reaction to improve the absorbance and photoelectric properties of the material. The specific steps include preparing MoSx at room temperature, preparing Ta3N5 nanoparticles using a vacuum tube furnace, and forming Ta3N5/MoSx powder by ultrasonic and oven heating.
The absorbance and photoelectric properties of the photocatalytic composite material are significantly improved, so that it can show excellent performance in photocatalytic reactions.
Smart Images

Figure CN119016069A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photocatalytic composite material preparation, in particular to a photocatalytic composite material based on Ta3N5-MoS x A method for preparing a heterojunction photocatalytic composite material. Background Art
[0002] Photocatalytic composite materials can convert solar energy into chemical energy for the production of hydrogen, and are a clean energy source. Ta3N5 is a potential solar photocatalytic degradation material, with a band gap of about 2.1eV, which can effectively absorb visible light and cover most areas of the sunlight spectrum. Ta3N5 is also an environmentally friendly material. When Ta3N5 absorbs photons, the electrons in the valence band are excited to the conduction band to form electron-hole pairs. The generated photogenerated carriers are active intermediates of the photocatalytic reaction, which can participate in redox reactions, degrade organic pollutants or decompose water, which is in line with the concept of green development.
[0003] Prior art, such as the patent application number CN201910711970.5, discloses a embroidery ball-shaped Ta3N5 / MoS2 heterojunction photocatalytic material and its preparation method. Ta3N5 / MoS2 presents an embroidery ball shape, Ta3N5 nanorods are evenly wrapped between two-dimensional MoS2 layers, and a close contact heterojunction is formed between Ta3N5 and MoS2. The heterojunction photocatalyst constructed by Ta3N5 and MoS2 can accelerate the transfer of photogenerated charges from Ta3N5 to MoS2 and reduce the recombination of photogenerated charges in the bulk phase of Ta3N5. However, the above scheme does not mention MoS with adjustable physical and chemical properties. x The method of combining with Ta3N5 to form a heterojunction, the material's absorbance and photoelectric properties also need to be improved. Summary of the invention
[0004] In order to solve the above-mentioned problems in the background technology, the present invention provides a Ta3N5-MoS x The invention discloses a method for preparing a heterojunction photocatalytic composite material. The photocatalytic composite material prepared by the method has high light absorption rate and excellent photoelectric performance.
[0005] The solution adopted by the present invention to solve the technical problem is: a method based on Ta3N5-MoS x A method for preparing a heterojunction photocatalytic composite material comprises the following steps:
[0006] Step 1, preparation of Ta3N5 nanoparticles;
[0007] Step 2: MoS x Preparation of
[0008] Step 3, preparation of Ta3N5 / MoSx;
[0009] In step 2, MoS x The preparation method is as follows:
[0010] 1) adding ammonium molybdate and thiourea to deionized water, and then stirring at room temperature at a stirring speed of 300 r / min to obtain a mixed solution B, wherein the ratio of the volume (mL) of the deionized water, the mass (g) of the ammonium molybdate, and the mass (g) of the thiourea is 60:1.75:3.8;
[0011] 2) Add 1.25 g of polyvinyl pyrrolidone to the mixed solution B and stir evenly to obtain a homogeneous solution;
[0012] 3) The homogeneous solution was transferred to an 80 mL polytetrafluoroethylene-lined reactor for sealed reaction at a temperature of 200° C. for 24 h to obtain reactant 1;
[0013] 4) The reactant 1 is centrifuged to obtain a precipitate B, which is then rinsed in anhydrous ethanol and deionized water, respectively, and then dried and collected to obtain MoS x .
[0014] Furthermore, in step 1, the preparation method of Ta3N5 nanoparticles is as follows:
[0015] 1) Tantalum chloride and methanol are mixed together and stirred evenly to obtain a mixed solution A, and then the mixed solution A is added to 50 ml of 19% ammonia water by mass, and then stirred at a stirring speed of 400 r / min for 1 hour to obtain a precipitate A, wherein the ratio of the mass (g) of the tantalum chloride to the volume (ml) of the methanol is 1:10;
[0016] 2) washing the precipitate A with water, filtering it, and then heating the filtered precipitate A in the presence of air at a temperature of 800° C. for 6 hours to obtain tantalum pentoxide nanoparticles;
[0017] 3) Weigh 500 mg of tantalum pentoxide nanoparticles, put them into a vacuum tube furnace, and calcine them in a sealed state under the condition of N2. The vacuum degree in the vacuum tube furnace before calcination is less than 100 Pa, the flow rate of N2 is 10 L / min, and it is calcined at a constant temperature of 800°C for 6 hours. After natural cooling, solid powder Ta3N5 nanoparticles are obtained.
[0018] Furthermore, the calcination heating rate of the vacuum tube furnace is 5 to 10° C. / min.
[0019] Furthermore, the ammonium molybdate includes anhydrous ammonium molybdate and hydrated ammonium molybdate.
[0020] Furthermore, in step 3, the preparation method of Ta3N5 / MoSx is as follows:
[0021] 1) MoSx is placed in deionized water and subjected to ultrasound at a frequency of 40 MHz and a time of 30 to 60 min to obtain a mixed solution C, wherein the ratio of the mass (g) of MoSx to the volume (ml) of deionized water is 0.04:20;
[0022] 2) Dispersing Ta3N5 in deionized water, stirring at a stirring speed of 400 r / min for 20 min, to obtain a mixed solution D, wherein the ratio of the mass (g) of Ta3N5 to the volume (ml) of deionized water is 0.15:30;
[0023] 3) Transfer the mixed solution C and the mixed solution D to an 80 mL Teflon reactor, and then heat them in an oven at a temperature of 160 to 240° C. for 16 to 24 hours. After the reaction is completed, reactant 2 is obtained;
[0024] 4) The reactant 2 was centrifuged to obtain a precipitate C, which was then rinsed in anhydrous ethanol and deionized water, respectively, and then dried at 60°C for 6 hours to obtain Ta3N5 / MoS x powder.
[0025] In summary, the beneficial effects of the present invention are as follows: the Ta3N5-MoS x The heterojunction photocatalytic composite material has high light absorption and excellent photoelectric performance.
[0026] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following specifically cites a preferred embodiment and describes it in detail with the accompanying drawings as follows. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 For this example, Ta3N5 / MoS x Ultraviolet diffuse reflectance spectrum of
[0028] Figure 2 For this example, Ta3N5 / MoS x XRD pattern of
[0029] Figure 3 For this example, Ta3N5 / MoS x XPS spectrum of
[0030] Figure 4 For this example, Ta3N5 / MoS xN2 adsorption isotherm and pore size distribution diagram;
[0031] Figure 5 For this example, Ta3N5 / MoS x The test results of the photoelectric performance. DETAILED DESCRIPTION
[0032] In order to make the content of the present invention more clearly understood, the present invention is further described below based on specific embodiments in conjunction with the accompanying drawings.
[0033] This embodiment is a method based on Ta3N5 / MoS x A method for preparing a heterojunction photocatalytic composite material;
[0034] Step 1, preparation of Ta3N5 nanoparticles;
[0035] 1) 1 g of tantalum chloride and 10 ml of methanol were mixed together to obtain a mixed solution A, and then the mixed solution A was added to 50 ml of 19% ammonia water by mass, and then stirred at a stirring speed of 400 r / min for 1 hour to obtain a precipitate A. The tantalum chloride in this embodiment can also be replaced by other tantalum halides;
[0036] 2) washing the precipitate A with water, filtering it, and then heating the filtered precipitate A in the presence of air at a temperature of 800° C. for 6 hours to obtain tantalum pentoxide nanoparticles;
[0037] 3) Weigh 500 mg of tantalum pentoxide nanoparticles, put them into a vacuum tube furnace, and calcine them in a sealed state under the condition of N2. The vacuum degree in the vacuum tube furnace before calcination is less than 100 Pa, the flow rate of N2 is 10 L / min, the calcination heating rate of the vacuum tube furnace is 5-10°C / min, and it is calcined at a constant temperature of 800°C for 6 hours. After natural cooling, solid powder Ta3N5 nanoparticles are obtained.
[0038] Step 2: MoS x Preparation of
[0039] 1) adding 1.75 g of ammonium molybdate and 3.8 g of thiourea to 60 mL of deionized water, and then stirring at room temperature at a stirring speed of 300 r / min to obtain a mixed solution B, wherein the ammonium molybdate includes anhydrous ammonium molybdate and hydrated ammonium molybdate;
[0040] 2) Add 1.25 g of polyvinyl pyrrolidone to the mixed solution B and stir evenly to obtain a homogeneous solution;
[0041] 3) The homogeneous solution was transferred to an 80 mL polytetrafluoroethylene-lined reactor for sealed reaction at a temperature of 200° C. for 24 h to obtain reactant 1;
[0042] 4) The reactant 1 is centrifuged to obtain a precipitate B, which is then rinsed in anhydrous ethanol and deionized water, respectively, and then dried and collected to obtain MoS x .
[0043] Step 3, preparation of Ta3N5 / MoSx;
[0044] 1) 40 mg of MoSx was placed in 20 mL of deionized water and subjected to ultrasound at a frequency of 40 MHz for 30 to 60 min to obtain a mixed solution C;
[0045] 2) Disperse 150 mg Ta3N5 into 30 mL deionized water and stir at a stirring speed of 400 r / min for 20 min to obtain a mixed solution D;
[0046] 3) Transfer the mixed solution C and the mixed solution D to an 80 mL Teflon reactor, and then heat them in an oven at a temperature of 160 to 240° C. for 16 to 24 hours. After the reaction is completed, reactant 2 is obtained;
[0047] 4) The reactant 2 was centrifuged to obtain a precipitate C, which was then rinsed in anhydrous ethanol and deionized water, respectively, and then dried at 60°C for 6 hours to obtain Ta3N5 / MoS x powder.
[0048] Figures 1 to 5 are Ta3N5 / MoS x UV diffuse reflectance spectrum, XRD spectrum, XPS diagram, N2 adsorption isotherm and pore size distribution diagram, and photoelectric performance test results. Figure 5 (a) is Ta3N5 / MoS in this embodiment x Open circuit voltage diagram of photoelectrocatalytic materials, Figure 5 (b) is Ta3N5 / MoS x EIS graph of photoelectrocatalytic materials, Figure 5 (c) is Ta3N5 / MoS x Photocurrent diagram of photoelectrocatalytic materials.
[0049] The embodiments described above are only preferred implementation modes of the present invention and cannot be used to limit the protection scope of the present invention. Any non-substantial changes and modifications made by those skilled in the art on the basis of the invention shall fall within the protection scope of the present invention.
Claims
1. A method based on Ta3N5-MoS x A method for preparing a heterojunction photocatalytic composite material, characterized in that: Includes steps: Step 1, preparation of Ta3N5 nanoparticles; Step 2: MoS x Preparation of Step 3, preparation of Ta3N5 / MoSx; In step 2, MoS x The preparation method is as follows: 1) adding ammonium molybdate and thiourea to deionized water, and then stirring at room temperature at a stirring speed of 300 r / min to obtain a mixed solution B, wherein the ratio of the volume (mL) of the deionized water, the mass (g) of the ammonium molybdate, and the mass (g) of the thiourea is 60:1.75:3.8; 2) Add 1.25 g of polyvinyl pyrrolidone to the mixed solution B and stir evenly to obtain a homogeneous solution; 3) The homogeneous solution was transferred to an 80 mL polytetrafluoroethylene-lined reactor for sealed reaction at a temperature of 200° C. for 24 h to obtain reactant 1; 4) The reactant 1 is centrifuged to obtain a precipitate B, which is then rinsed in anhydrous ethanol and deionized water, respectively, and then dried and collected to obtain MoS x .
2. A Ta3N5-MoS based on claim 1 x A method for preparing a heterojunction photocatalytic composite material, characterized in that: In the step 1, the preparation method of Ta3N5 nanoparticles is as follows: 1) Tantalum chloride and methanol are mixed together and stirred evenly to obtain a mixed solution A, and then the mixed solution A is added to 50 ml of 19% ammonia water by mass, and then stirred at a stirring speed of 400 r / min for 1 hour to obtain a precipitate A, wherein the ratio of the mass (g) of the tantalum chloride to the volume (ml) of the methanol is 1:10; 2) washing the precipitate A with water, filtering it, and then heating the filtered precipitate A in the presence of air at a temperature of 800° C. for 6 hours to obtain tantalum pentoxide nanoparticles; 3) Weigh 500 mg of tantalum pentoxide nanoparticles, put them into a vacuum tube furnace, and calcine them in a sealed state under the condition of N2. The vacuum degree in the vacuum tube furnace before calcination is less than 100 Pa, the flow rate of N2 is 10 L / min, and it is calcined at a constant temperature of 800°C for 6 hours. After natural cooling, solid powder Ta3N5 nanoparticles are obtained.
3. A Ta3N5-MoS based on claim 2 x A method for preparing a heterojunction photocatalytic composite material, characterized in that: The calcination heating rate of the vacuum tube furnace is 5-10°C / min.
4. A Ta3N5-MoS based on claim 1 x A method for preparing a heterojunction photocatalytic composite material, characterized in that: The ammonium molybdate includes anhydrous ammonium molybdate and hydrated ammonium molybdate.
5. A Ta3N5-MoS based on claim 2 x A method for preparing a heterojunction photocatalytic composite material, characterized in that: Step 3, Ta3N5 / MoS x The preparation method is as follows: 1) MoSx is placed in deionized water and subjected to ultrasound at a frequency of 40 MHz and a time of 30 to 60 min to obtain a mixed solution C, wherein the ratio of the mass (g) of MoSx to the volume (ml) of deionized water is 0.04:20; 2) Dispersing Ta3N5 in deionized water, stirring at a stirring speed of 400 r / min for 20 min, to obtain a mixed solution D, wherein the ratio of the mass (g) of Ta3N5 to the volume (ml) of deionized water is 0.15:30; 3) Transfer the mixed solution C and the mixed solution D to an 80 mL Teflon reactor, and then heat them in an oven at a temperature of 160 to 240° C. for 16 to 24 hours. After the reaction is completed, reactant 2 is obtained; 4) The reactant 2 was centrifuged to obtain a precipitate C, which was then rinsed in anhydrous ethanol and deionized water, respectively, and then dried at 60°C for 6 hours to obtain Ta3N5 / MoS x powder.
Citation Information
Patent Citations
Hydrangea-like Ta3N5 / MoS2 heterojunction photocatalytic material and preparation method thereof
CN110560118A
Cation-doped Ta3N5-MoS2 heterojunction photocatalytic hydrogen production material and preparation method thereof
CN111905792A
Composite photocatalytic nano-material for degrading micro-plastic under driving of visible light and preparation method of composite photocatalytic nano-material
CN117205954A
Capacitor having tantalum oxynitride film and method for making same