Heavy oil hydrogenation catalyst and preparation method and application thereof
By using silicon-aluminum materials and nonionic surfactants in heavy oil hydrogenation catalyst support to form high acidity and step-by-step pore structures and introducing active metals in step, the problems of insufficient acidity and mechanical properties of existing catalysts are solved, and suitable for heavy oil is achieved High-efficiency catalytic effect of hydrogenation process.
Patent Information
- Application Number
- CN202310579850.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-23
AI Technical Summary
The existing heavy oil hydrogenation catalyst support has weak acidity, low gumification index and poor adhesion, resulting in low hydrogenation activity and low mechanical strength, making it difficult to meet the needs of the boiling bed heavy oil hydrogenation process.
Using silicon-aluminum material as a carrier, excessive crystallization is regulated by adding nonionic surfactant during the preparation of the carrier precursor, forming a high-surface acidic and mesoporous-macropore cascade structure, and introducing active metal components in two steps to enhance The binding force of the catalyst and the metal dispersion.
It improves the acidity, pore structure and mechanical properties of the catalyst, enhances hydrogenation activity and side pressure strength, is suitable for heavy oil hydrogenation process, and is simple in preparation method and low in energy consumption, which is suitable for large-scale production.
Smart Images

Figure BDA0004241352450000151 
Figure BDA0004241352450000161 
Figure BDA0004241352450000162
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petrochemical industry and relates to a catalytic material and a preparation method thereof, in particular to a heavy oil hydrogenation catalyst and a preparation method thereof. Background Art
[0002] Faced with the increasing demand for clean fuels and chemical raw materials, and the situation that crude oil properties are becoming heavier and worse, heavy oil hydrogenation technology has received increasing attention from researchers. In residue oil hydrocracking, the catalyst usually requires appropriate acidity for mild cracking, medium pores for diffusing macromolecules such as asphaltene to active sites, and high hydrogenation activity to avoid coking. Macroporous pseudo-boehmite is usually used as the raw material for residue oil hydrogenation catalyst carriers, but the macroporous pseudo-boehmite prepared by the current pseudo-boehmite production process has weak acidity, low peptization index, and poor adhesion. When used as a hydroprocessing catalyst material, the catalyst has low hydrogenation activity and low mechanical strength.
[0003] CN104646070A discloses a method for preparing a supported hydroprocessing catalyst carrier, which uses a high-concentration organic acid as a binder to enhance the bonding force between catalyst carriers, thereby enhancing the strength of the catalyst carrier. This method uses a high-concentration organic acid instead of traditional nitric acid to reduce NOx emissions during the roasting process, but still requires the addition of a high-concentration acid during the preparation of the carrier.
[0004] CN104096584A discloses a residual oil hydrogenation catalyst and a preparation method thereof. A small amount of activated carbon is introduced into alumina to reduce the reaction of Ni2P active component with alumina during the generation process, while improving its dispersibility, so as to give full play to the high activity of Ni2P and the carrier advantage of alumina-activated carbon mixture, thereby improving the catalyst's ability to remove impurities such as sulfur and residual carbon.
[0005] CN113578337A discloses a residual oil hydrogenation catalyst and its preparation method and application. The method obtains a catalyst carrier with a directional pore structure by molding and crushing magnesium oxide and aluminum oxide, thereby improving the demetallization and anti-carbon deposition capabilities of the catalyst, and increasing the acid center of the catalyst carrier by acid treatment. Summary of the invention
[0006] In view of the deficiencies of the prior art, the present invention provides a heavy oil hydrogenation catalyst and a preparation method and application thereof. The heavy oil hydrogenation catalyst provided by the present invention has suitable acidity, pore structure, hydrogenation activity and mechanical properties, and is particularly suitable for a fluidized bed heavy oil hydrogenation process. The preparation method of the hydrogenation catalyst is simple in process, low in energy consumption, and suitable for large-scale production.
[0007] (I) The present invention provides a method for preparing a heavy oil hydrogenation catalyst, the preparation method comprising the following steps:
[0008] S1: preparing carrier precursor;
[0009] S2: mixing the support precursor obtained in step S1 with an auxiliary agent, then adding a solution containing an active metal, kneading, and then performing a first drying and a first calcination to obtain a catalyst precursor;
[0010] S3: After introducing active metal components into the catalyst precursor obtained in step S2, a heavy oil hydrogenation catalyst is obtained after a second drying and a second calcination.
[0011] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the preparation method of the carrier precursor comprises the following steps:
[0012] (1) preparing sol: mixing silicon source A, template and water to obtain sol;
[0013] (2) mixing the sol obtained in step (1) with alcohol and performing heat treatment to obtain a material stream A;
[0014] (3) adding a silicon source B, an acidic aluminum source and a basic aluminum source into a reactor containing bottom water, obtaining a stream B after reaction, and then mixing the stream B with a nonionic surfactant to obtain a stream C;
[0015] (4) The material stream C is subjected to hydrothermal treatment under hydrothermal treatment conditions, and then washed and dried to obtain a carrier precursor.
[0016] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the silicon source A in step (1) is one or more of ethyl orthosilicate, methyl orthosilicate, and silica sol, preferably ethyl orthosilicate.
[0017] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the template agent in step (1) is tetrapropylammonium hydroxide and / or tetrapropylammonium bromide; preferably tetrapropylammonium hydroxide.
[0018] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the alcohol in step (2) is a C1-C3 alcohol, which can be one or more of a monohydric alcohol, a dihydric alcohol, or a polyhydric alcohol; the specific alcohol can be one or more of ethanol, ethylene glycol, and glycerol, preferably glycerol.
[0019] In the above-mentioned preparation method of heavy oil hydrogenation catalyst, in some specific embodiments, the usage ratio of silicon source A, template, water and alcohol is (3-6):(5-8):(2-4):(0.5-5) by weight.
[0020] In the above-mentioned preparation method of heavy oil hydrogenation catalyst, in some specific embodiments, the heat treatment operating conditions in step (2) are as follows: the treatment temperature is 60-100°C, and the treatment time is not more than 24 hours; preferably, the treatment temperature is 80-100°C, and the preferred treatment time is 8-12 hours.
[0021] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the silicon source B in step (3) is water glass and / or alkaline silica sol, preferably alkaline silica sol.
[0022] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the acidic aluminum source in step (3) is a water-soluble acidic aluminum-containing compound, preferably a water-soluble acidic inorganic aluminum-containing compound, especially a water-soluble inorganic strong acid aluminum salt, more preferably one or more selected from aluminum sulfate, aluminum nitrate, and aluminum chloride, preferably aluminum sulfate.
[0023] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the alkaline aluminum source in step (3) is an alkali metal aluminate solution; specifically selected from one or more of sodium aluminate and potassium aluminate, preferably sodium aluminate.
[0024] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the pH value of the feed stream B in step (3) is 4-7, preferably 5-6; the pH value of the feed stream B is regulated by the amount of the acidic aluminum source.
[0025] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the reaction temperature in step (3) is 50°C to 90°C, preferably 50°C to 80°C.
[0026] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the aluminum content of the acidic aluminum source in step (3) is 10 to 70 gAl2O3 / L in terms of Al2O3, the aluminum content of the alkaline aluminum source is 70 to 170 gAl2O3 / L in terms of Al2O3, and the silicon content of the second silicon source is 20 to 80 gSiO2 / L in terms of SiO2.
[0027] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the amount of water used in step (3) is 10% to 20% of the total volume of the reaction system, preferably 13% to 20%.
[0028] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the nonionic surfactant in step (3) is one or more of polyethylene glycol, alkyl alcohol amide, and polyether; preferably polyethylene glycol; the alkyl alcohol amide is one or more of lauryl diethanolamide and coconut oil fatty acid diethanolamide; the polyether is one or more of AEO-6 and AEO-9; the molecular weight of the polyethylene glycol is 200 to 1000, preferably 200 to 700.
[0029] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the weight ratio of the material stream A obtained in step (2) to the material stream C in step (3) is 1:80-100.
[0030] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the hydrothermal treatment conditions in step (4) are as follows: the treatment temperature is 100°C to 180°C, preferably 110°C to 160°C, and more preferably 120°C to 150°C; the treatment pressure is 0.1 to 0.5 MPa, preferably 0.1 to 0.3 MPa, and the treatment time is 0.5h to 10h, preferably 0.5h to 6h.
[0031] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the washing in step (4) is washing with water, the washing temperature is 70-90° C., and the washing is repeated several times, generally until the liquid is neutral.
[0032] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the drying conditions in step (4) are as follows: the drying temperature is 100 to 150° C., and the drying time is 6 to 10 hours.
[0033] In the above-mentioned preparation method of heavy oil hydrogenation catalyst, in some specific embodiments, the auxiliary agent in step S2 is one or more of methyl cellulose, hydroxymethyl cellulose, hydroxypropyl methyl cellulose, etc., and the content of the auxiliary agent is 0.5-5wt% based on the mass of the carrier precursor.
[0034] In the above-mentioned preparation method of heavy oil hydrogenation catalyst, in some specific embodiments, after mixing in step S2, the mixture can be first molded and then dried and calcined. The molding can be carried out by existing molding methods in the art, and can be cylindrical strip, spherical, toothed ball, multi-leaf clover, etc.
[0035] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the first drying conditions in step S2 are as follows: the first drying temperature is 90 to 120° C., and the first drying time is 2 to 10 hours.
[0036] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the first calcination conditions in step S2 are as follows: the first calcination temperature is 500-800° C., and the first calcination time is 4-10 hours.
[0037] In the above-mentioned preparation method of heavy oil hydrogenation catalyst, in some specific embodiments, the active metal in step S2 is one or more of the VIB group metal and / or the VIII group metal, and the concentration and amount of the solution containing the active metal are such that the content of the VIII group metal in the final catalyst precursor is 0.5-5wt%, preferably 1.0-3.0wt%, and the content of the VIB group metal is 1.0-10.0wt%, preferably 2.0-5.0wt%, based on the weight of the catalyst precursor and calculated as oxide. The VIII group metal is one or more of Ni and Co, and the VIB group metal is one or more of Mo and W. The precursor containing the active metal component, water, and an optional phosphorus-containing compound are uniformly mixed to obtain a solution containing the active metal.
[0038] In the preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the method for introducing the active metal component in step S3 can be one of the existing methods such as impregnation method and kneading method, preferably impregnation method. When the active metal component is loaded by impregnation method, the existing impregnation method in the art can be adopted, and the spray method, saturation impregnation method or supersaturation impregnation method can be adopted. When the impregnation method is adopted, the precursor containing the active metal component, water, and the optional phosphorus-containing compound are first mixed uniformly to obtain a solution containing the active metal, and then the solution is mixed uniformly with the carrier, and then the catalyst is obtained after standing, drying, and roasting.
[0039] In the preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the precursor containing the active metal component is a compound containing a metal of Group VIB and / or a metal of Group VIII, the compound containing a metal of Group VIB may be one or more of a molybdenum-containing compound and a tungsten-containing compound, and the compound containing a metal of Group VIII may be one or more of a nickel-containing compound and a cobalt-containing compound. The molybdenum-containing compound may be molybdenum oxide and / or ammonium heptamolybdate; the nickel-containing compound may be basic nickel carbonate and / or nickel nitrate; the cobalt-containing compound may be basic cobalt carbonate and / or cobalt nitrate. The phosphorus-containing compound may be one or more of phosphoric acid, ammonium dihydrogen phosphate, and ammonium monohydrogen phosphate.
[0040] In the above-mentioned preparation method of heavy oil hydrogenation catalyst, in some specific embodiments, the hydrogenation active metal component described in step S3 is one or more of the metals of group VIB and / or group VIII, and the concentration of the compound containing hydrogenation active metal in the solution and the amount of the solution are such that the content of the metal of group VIII in the final catalyst is 1.5-10.0wt%, preferably 2.0-8.0wt%, and the content of the metal of group VIB is 5.0-25.0wt%, preferably 10.0-20.0wt%. The metal of group VIII is one or more of Ni and Co, and the metal of group VIB is one or more of Mo and W.
[0041] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the second drying conditions in step S3 include: the second drying temperature is 90 to 120° C., and the second drying time is 2 to 10 hours.
[0042] In the above-mentioned preparation method of the heavy oil hydrogenation catalyst, in some specific embodiments, the second calcination conditions in step S3 include: the second calcination temperature is 300-600° C., and the second calcination time is 4-10 hours.
[0043] The second aspect of the present invention provides a heavy oil hydrogenation catalyst obtained by the above preparation method.
[0044] Furthermore, in the above-mentioned heavy oil hydrogenation catalyst, as a specific embodiment, the hydrogenation catalyst includes a carrier and an active metal component, with a silicon-aluminum material as the carrier, and the metal element in the active metal component comes from at least one of a Group VIII metal and a Group VIB metal, the Group VIII metal is one or more of Ni and Co, and the Group VIB metal is one or more of Mo and W.
[0045] Furthermore, in the above-mentioned heavy oil hydrogenation catalyst, as a specific embodiment, based on the total weight of the hydrogenation catalyst, the content of the Group VIII metal in terms of oxide is 1.5-10.0wt%, preferably 2.0-8.0wt%, and the content of the Group VIB metal in terms of oxide is 5.0-25.0wt%, preferably 10.0-20.0wt%.
[0046] Furthermore, in the above-mentioned heavy oil hydrogenation catalyst, as a specific embodiment, the properties of the hydrogenation catalyst are as follows: pore volume of 0.50-0.80 mL / g, specific surface area of 150-280 m 2 / g.
[0047] Furthermore, in the above-mentioned heavy oil hydrogenation catalyst, as a specific embodiment, the pore distribution of the hydrogenation catalyst has the following characteristics: the pore volume of pores with a pore diameter of 8-20nm accounts for 40%-70% of the total pore volume, and the pore volume of pores with a pore diameter of >100nm accounts for more than 10% of the total pore volume.
[0048] Furthermore, in the above-mentioned heavy oil hydrogenation catalyst, as a specific implementation, the catalyst diameter is less than 1.5 mm and the lateral pressure strength is greater than 10 N / mm.
[0049] The present invention also provides an application of the heavy oil hydrogenation catalyst in a heavy oil hydrogenation reaction.
[0050] Furthermore, in the above application, the heavy oil may be at least one or more of atmospheric residue oil, vacuum residue oil, catalytic slurry oil, and coal tar.
[0051] Furthermore, in the above application, the hydrogenation reaction conditions are generally: reaction temperature is 320-520°C, reaction pressure is 8-20 MPa, liquid hourly volume space velocity is 0.1-0.5 h -1 , the volume ratio of hydrogen to oil is 300-1000.
[0052] Furthermore, in the above application, the heavy oil hydrogenation reaction is carried out in a fixed bed reactor, an ebullated bed reactor, or a suspended bed hydrogenation reactor, preferably in an ebullated bed hydrogenation reactor.
[0053] Compared with the existing methods, the heavy oil hydrogenation catalyst and preparation method provided by the present invention have the following technical effects and advantages:
[0054] 1. The heavy oil hydrogenation catalyst of the present invention uses silicon-aluminum material as a carrier, and the carrier has high lateral pressure strength, good wear resistance, and good mechanical properties. At the same time, it can provide strong B acid for the catalyst, which is beneficial to the residual oil hydrogenation reaction.
[0055] 2. In the preparation method of the heavy oil hydrogenation catalyst of the present invention, the introduction of the additive enhances the bonding force between the catalyst carriers and enhances the strength of the catalyst carriers. At the same time, the active metal components are introduced in two steps, which is more conducive to reducing the agglomeration between the metals, improving the dispersion of the metals, and increasing the active centers on the catalyst surface.
[0056] 3. In the preparation method of the heavy oil hydrogenation catalyst of the present invention, the silicon-aluminum material used as the carrier precursor has a large pore volume, and has both mesopore-macropore two-level gradient pores, and has molecular sieve characteristics, and has the characteristics of high B acid content of molecular sieves and low impurity content (especially low sodium content), etc., and is particularly suitable for use as a carrier of heavy oil hydrogenation catalyst.
[0057] 4. In the preparation method of the heavy oil hydrogenation catalyst of the present invention, during the preparation process of the carrier precursor, when preparing the semi-crystallized precursor, the over-crystallization of the precursor is regulated by adding a nonionic surfactant, and then the precursor is added to the silicon-aluminum material, so that the silicon-aluminum material grows on its surface to form a high surface acidity and a mesoporous-macroporous ladder channel structure. At the same time, the precursor provides a crystal nucleus for the subsequent reaction, and the acidified silica gel group and aluminum hydroxide colloid are adsorbed on the crystal nucleus formed by the precursor, which promotes the enlargement of the prepared silicon-aluminum material grains, which is conducive to the formation of a silicon-aluminum material with a large pore volume, a large pore size, and strong acidity.
[0058] 5. In the preparation method of the heavy oil hydrogenation catalyst of the present invention, a nonionic surfactant is added during the preparation of the carrier precursor, so that the soluble silicon species in the slurry are exchanged with the like ions on the surface of the nonionic surfactant micelles and adsorbed on the micelle surface, and also react with the nonionic surfactant molecules in the liquid phase to form a new inorganic-organic complex. The adsorbed silicon-containing micelles and composite molecules form a mesoporous material with a stable structure at a lower temperature through multiple thermodynamic equilibrium under the action of ionic bonds, hydrogen bonds and intermolecular dispersion forces. DETAILED DESCRIPTION
[0059] The technical scheme of the present invention is further described below by examples and comparative examples, but is not limited to the following examples.
[0060] In the context of this specification, pore volume, specific surface area and pore size distribution are measured by low temperature nitrogen adsorption method. Total acid, B acid and L acid are measured by pyridine infrared adsorption method.
[0061] In the context of this specification, the lateral compression strength is measured using a strength meter using the Q / SH 361 926-2020 method.
[0062] In the context of this specification, metal dispersion is measured by X-ray photoelectron spectroscopy (XPS). X-ray photoelectron spectroscopy (XPS) uses Shimadzu AXIS SPURA+, and all binding energies are corrected for contaminating carbon (C1s284.8eV). Al Ka photoelectron source, E b =1486.6eV.
[0063] Unless otherwise specified, all percentages, parts, ratios, etc. mentioned in this specification are based on weight and pressure is gauge pressure.
[0064] In the context of this specification, any two or more embodiments of the present invention may be arbitrarily combined, and the technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.
[0065] Example 1
[0066] (1) Preparation of silicon-aluminum materials
[0067] Prepare an aluminum sulfate solution with a concentration of 50gAl2O3 / L and a silica sol solution with a concentration of 60gSiO2 / L for standby use. Prepare a sodium aluminate solution with a caustic ratio of 1.20 and a concentration of 150gAl2O3 / L for standby use. Mix 50g of tetraethyl orthosilicate (TEOS), 70g of tetrapropylammonium hydroxide (TPAOH), and 30g of deionized water to form a sol, then mix and stir with 15g of propylene glycol and age at 60°C for 18h to obtain a precursor solution. Add 500mL of deionized water as bottom water to a 5000mL reactor, start stirring and heat, and after the deionized water is heated to 65°C, add the prepared aluminum sulfate solution to the reactor at 16mL / min, and add the prepared sodium aluminate and silica sol in parallel. Control the pH of the reaction to 7.0 by adjusting the flow rate of sodium aluminate and silica sol, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, 1320 ml of aluminum sulfate, 580 ml of sodium aluminate, and 1160 ml of silica sol are added to the reactor under stirring conditions. 20 g of polyethylene glycol 200 is then added to the above solution, and stirred until uniformly mixed. The above slurry is placed in a reactor, and the treatment temperature is 100 ° C, the treatment pressure is 0.2 MPa, and the treatment is carried out for 8 hours under stirring conditions. The treated slurry is washed with hot water at 90 ° C until the liquid is neutral, and dried at 150 ° C for 6 hours to obtain a carrier precursor.
[0068] (2) Catalyst preparation
[0069] Weigh 53.29g of molybdenum oxide (content 99%), 24.42g of basic nickel carbonate (nickel oxide content 54wt%), and 19.62g of phosphoric acid, and heat to prepare 500ml of impregnation liquid. Weigh 400g of carrier precursor (dry basis 70wt%), mix with 2.8g of methyl cellulose, take 100ml of the above impregnation liquid, dilute it ten times, add it into the above mixture and knead it, after extrusion, dry it at 110℃ for 6h, and calcine it at 700℃ for 4h to obtain hydrogenation catalyst carrier; impregnate the carrier by equal volume impregnation method, dry it at 100℃ for 10h, and calcine it at 500℃ for 3h to obtain hydrogenation catalyst A, and the physicochemical properties of the obtained catalyst are listed in Table 1.
[0070] Example 2
[0071] (1) Preparation of silicon-aluminum materials
[0072] Prepare an aluminum chloride solution with a concentration of 30gAl2O3 / L and a water glass solution with a concentration of 30gSiO2 / L and a modulus of 2.5 for standby use. Prepare a sodium aluminate solution with a caustic ratio of 1.20 and a concentration of 100gAl2O3 / L for standby use. Stir 60g methyl orthosilicate, 80g tetrapropylammonium hydroxide (TPAOH), and 40g deionized water to form a sol, then mix with 50g ethanol and age at 80°C for 8h to obtain a precursor solution. Add 700mL deionized water as bottom water to a 5000mL reactor, start stirring and heat, and after the deionized water is heated to 70°C, add the prepared aluminum chloride solution to the reactor at 14mL / min, and add the prepared sodium aluminate and water glass in parallel. Control the pH of the reaction to 6.0 by adjusting the flow rate of sodium aluminate and water glass, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, 1100 ml of aluminum chloride, 500 ml of sodium aluminate, and 950 ml of water glass are added to the reactor under stirring conditions. 10 g of lauryl diethanolamine is then added to the above solution, and stirred until mixed evenly. The above slurry is placed in a reactor, and the treatment temperature is 120 ° C, the treatment pressure is 0.2 MPa, and the treatment is carried out for 4 hours under stirring conditions. The treated slurry is washed with hot water at 70 ° C until the liquid is neutral, and dried at 120 ° C for 8 hours to obtain a carrier precursor.
[0073] (2) Catalyst preparation
[0074] Weigh 38.86g of molybdenum oxide (content 99%), 17.81g of basic nickel carbonate (nickel oxide content 54wt%), and 17.88g of phosphoric acid, and heat to prepare 500ml of impregnation solution. Weigh 400g of carrier precursor (dry basis 70wt%), mix with 11.2g of hydroxymethyl cellulose, take 100ml of the above impregnation solution, dilute it ten times, add it into the above mixture and knead it, after extrusion, dry it at 100℃ for 6h, and calcine it at 600℃ for 6h to obtain hydrogenation catalyst carrier; impregnate the carrier by equal volume impregnation method, dry it at 110℃ for 8h, and calcine it at 600℃ for 3h to obtain hydrogenation catalyst B, and the physicochemical properties of the obtained catalyst are listed in Table 1.
[0075] Example 3
[0076] (1) Preparation of silicon-aluminum materials
[0077] Prepare aluminum nitrate solution with a concentration of 70gAl2O3 / L and silica sol solution with a concentration of 80gSiO2 / L for standby use. Prepare potassium aluminate solution with a caustic ratio of 1.20 and a concentration of 170gAl2O3 / L for standby use. Stir 30g silica sol, 50g tetrapropylammonium hydroxide (TPAOH), and 20g deionized water to form a sol, then mix with 15g ethylene glycol and age at 80°C for 8h to obtain a precursor solution. Add 1000mL deionized water as bottom water to a 5000mL reactor, start stirring and heat, and after the deionized water is heated to 70°C, add the prepared aluminum nitrate solution to the reactor at 18mL / min, and add the prepared potassium aluminate and silica sol in parallel. Control the pH of the reaction to 6.0 by adjusting the flow rate of potassium aluminate and silica sol, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, 1500ml of aluminum nitrate, 700ml of potassium aluminate, and 1300ml of silica sol are added to the reactor under stirring conditions. 10g of AEO-9 is then added to the above solution with 50g of the precursor solution, and stirred until the mixture is uniform. The above slurry is placed in a reactor, and the treatment temperature is 180°C, the treatment pressure is 0.5MPa, and the treatment is carried out for 0.5h under stirring conditions. The treated slurry is washed with hot water at 80°C until the liquid is neutral, and dried at 100°C for 10h to obtain a carrier precursor.
[0078] (2) Catalyst preparation
[0079] Weigh 186.98g of molybdenum oxide (content 99%), 68.56g of basic nickel carbonate (nickel oxide content 54wt%), and 45.90g of phosphoric acid, and heat to prepare 500ml of impregnation liquid. Weigh 400g of carrier precursor (dry basis 70wt%), mix 5.6g of hydroxypropyl methylcellulose, take 100ml of the above impregnation liquid, dilute it ten times, add the above mixture and knead, extrusion molding, dry at 110℃ for 6h, and roast at 500℃ for 5h to obtain hydrogenation catalyst carrier; impregnate the carrier by equal volume impregnation method, dry at 90℃ for 10h, and roast at 400℃ for 4h to obtain hydrogenation catalyst C, and the physicochemical properties of the obtained catalyst are listed in Table 1.
[0080] Comparative Example 1
[0081] Weigh 53.29 g of molybdenum oxide (content: 99%), 24.42 g of basic nickel carbonate (nickel oxide content: 54 wt%), and 19.62 g of phosphoric acid, and heat to prepare 500 ml of impregnation solution.
[0082] Weigh 400g of industrial pseudo-boehmite raw material (70wt% on a dry basis) and mix with 2.8g of methyl cellulose, take 100ml of the above impregnation solution, dilute it ten times, add it into the above mixture and knead it, extrude it into strips, dry it at 110℃ for 6h, and calcine it at 700℃ for 4h to obtain a hydrogenation catalyst carrier;
[0083] The carrier was impregnated by the equal volume impregnation method, and the hydrogenation catalyst D1 was obtained after drying at 100°C for 10 h and calcining at 500°C for 3 h. The physicochemical properties of the obtained catalyst are listed in Table 2.
[0084] Comparative Example 2
[0085] The preparation of the carrier precursor is the same as in Example 1.
[0086] Weigh 53.29 g of molybdenum oxide (content: 99%), 24.42 g of basic nickel carbonate (nickel oxide content: 54 wt%), and 19.62 g of phosphoric acid, and heat to prepare 500 ml of impregnation solution.
[0087] Weigh 400 g of the carrier precursor (70 wt% on a dry basis) and 2.8 g of methyl cellulose, add water and knead, extrude into strips, dry at 110° C. for 6 h, and calcine at 700° C. for 4 h to obtain a hydrogenation catalyst carrier;
[0088] The carrier was impregnated by the equal volume impregnation method, and the hydrogenation catalyst D2 was obtained after drying at 100°C for 10 h and calcining at 500°C for 3 h. The physicochemical properties of the obtained catalyst are listed in Table 2.
[0089] Comparative Example 3
[0090] The preparation of the carrier precursor is the same as in Example 1.
[0091] Weigh 53.29 g of molybdenum oxide (content: 99%), 24.42 g of basic nickel carbonate (nickel oxide content: 54 wt%), and 19.62 g of phosphoric acid, and heat to prepare 500 ml of impregnation solution.
[0092] Weigh 400 g of the carrier precursor (70 wt% on a dry basis), add 2.0 wt% of sesbania powder and mix, take 100 ml of the above impregnation solution, dilute it ten times, add it into the above mixture and knead, extrude it into strips, dry it at 110° C. for 6 h, and calcine it at 700° C. for 4 h to obtain a hydrogenation catalyst carrier;
[0093] The carrier was impregnated by the equal volume impregnation method, and the hydrogenation catalyst D3 was obtained after drying at 100°C for 10 h and calcining at 500°C for 3 h. The physicochemical properties of the obtained catalyst are listed in Table 2.
[0094] Comparative Example 4
[0095] Prepare an aluminum sulfate solution with a concentration of 50gAl2O3 / L and a silica sol solution with a concentration of 60gSiO2 / L for standby use. Prepare a sodium aluminate solution with a caustic ratio of 1.20 and a concentration of 150gAl2O3 / L for standby use. Mix 50g tetraethyl orthosilicate (TEOS) and 30g deionized water to form a sol, then mix and stir with 15g propylene glycol and age at 60°C for 18h to obtain a precursor solution. Add 500mL deionized water as bottom water to a 5000mL reactor, start stirring and heat, and after the deionized water is heated to 65°C, add the prepared aluminum sulfate solution to the reactor at 16mL / min, and add the prepared sodium aluminate and silica sol in parallel. Control the pH of the reaction to 7.0 by adjusting the flow rate of sodium aluminate and silica sol, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, 1320 ml of aluminum sulfate, 580 ml of sodium aluminate, and 1160 ml of silica sol are added to the reactor under stirring conditions. 20 g of polyethylene glycol 200 is then added to the above solution, and then 40 g of the precursor solution is added and stirred until uniformly mixed. The above slurry is placed in a reactor, and the treatment temperature is 100 ° C, the treatment pressure is 0.2 MPa, and the treatment is carried out for 8 hours under stirring conditions. The treated slurry is washed with hot water at 90 ° C until the liquid is neutral, and dried at 150 ° C for 6 hours to obtain carrier precursor B-1.
[0096] (2) Catalyst preparation
[0097] Weigh 53.29g of molybdenum oxide (content 99%), 24.42g of basic nickel carbonate (nickel oxide content 54wt%), and 19.62g of phosphoric acid, and heat to prepare 500ml of impregnation solution. Weigh 400g of carrier precursor B-1 (dry basis 70wt%), mix with 2.8g of methyl cellulose, take 100ml of the above impregnation solution, dilute it ten times, add it into the above mixture and knead it, after extrusion, dry it at 110℃ for 6h, and calcine it at 700℃ for 4h to obtain the hydrogenation catalyst carrier; impregnate the carrier by equal volume impregnation method, dry it at 100℃ for 10h, and calcine it at 500℃ for 3h to obtain hydrogenation catalyst D4, and the physicochemical properties of the obtained catalyst are listed in Table 2.
[0098] Comparative Example 5
[0099] Prepare an aluminum chloride solution with a concentration of 30gAl2O3 / L and a water glass solution with a concentration of 30gSiO2 / L and a modulus of 2.5 for later use. Prepare a sodium aluminate solution with a caustic ratio of 1.20 and a concentration of 100gAl2O3 / L for later use. Stir 60g methyl orthosilicate, 80g tetrapropylammonium hydroxide (TPAOH), and 40g deionized water to form a sol, then mix with 50g ethanol and age at 80°C for 8h to obtain a precursor solution.
[0100] Add 700mL of deionized water as bottom water to a 5000mL reactor, start stirring and heating, after the deionized water is heated to 70°C, add the prepared aluminum chloride solution to the reactor at 14mL / min, and add the prepared sodium aluminate and water glass in parallel, and control the pH of the reaction to 6.0 by adjusting the flow rate of sodium aluminate and water glass, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, the amount of aluminum chloride is 1100ml, the amount of sodium aluminate is 500mL, and the amount of water glass is 950ml, and then 45g of the precursor solution is added to the above solution and stirred until mixed evenly.
[0101] The slurry was placed in a reactor and treated at a temperature of 120°C and a pressure of 0.2 MPa for 4 hours under stirring. The treated slurry was washed with hot water at 70°C until the liquid was neutral, and dried at 120°C for 8 hours to obtain carrier precursor B-2.
[0102] (2) Catalyst preparation
[0103] Weigh 38.86g of molybdenum oxide (content 99%), 17.81g of basic nickel carbonate (nickel oxide content 54wt%), and 17.88g of phosphoric acid, and heat to prepare 500ml of impregnation liquid. Weigh 400g of carrier precursor B-2 (dry basis 70wt%), mix 11.2g of hydroxymethyl cellulose, take 100ml of the above impregnation liquid, dilute it ten times, add the above mixture to knead, extrusion molding, dry at 100℃ for 6h, and calcine at 600℃ for 6h to obtain hydrogenation catalyst carrier; impregnate the carrier by equal volume impregnation method, dry at 110℃ for 8h, and calcine at 600℃ for 3h to obtain hydrogenation catalyst D5, the physicochemical properties of the obtained catalyst are listed in Table 2.
[0104] Comparative Example 6
[0105] Prepare aluminum nitrate solution with a concentration of 70gAl2O3 / L and silica sol solution with a concentration of 80gSiO2 / L and a modulus of 2.8 for standby use. Prepare potassium aluminate solution with a caustic ratio of 1.20 and a concentration of 170gAl2O3 / L for standby use. Stir 30g silica sol and 20g deionized water to make a sol, then mix with 15g ethylene glycol and age at 80°C for 8h to obtain a precursor solution. Add 1000mL deionized water as bottom water to a 5000mL reactor, start stirring and heat, and after the deionized water is heated to 70°C, add the prepared aluminum nitrate solution to the reactor at 18mL / min, and add the prepared potassium aluminate and silica sol in parallel. Control the pH of the reaction to 6.0 by adjusting the flow rate of potassium aluminate and silica sol, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, the amount of aluminum nitrate is 1500ml, the amount of potassium aluminate is 700mL, and the amount of silica sol is 1300ml. Then 50g of the precursor solution is added to the above solution and stirred until mixed evenly. The above slurry is placed in a reactor, and under stirring conditions, the treatment temperature is 180°C, the treatment pressure is 0.5MPa, and the treatment is 0.5h. The treated slurry is washed with hot water at 80°C until the liquid is neutral, and dried at 100°C for 10h, carrier precursor B-3.
[0106] (2) Catalyst preparation
[0107] Weigh 186.98g of molybdenum oxide (content 99%), 68.56g of basic nickel carbonate (nickel oxide content 54wt%), and 45.90g of phosphoric acid, and heat to prepare 500ml of impregnation liquid. Weigh 400g of carrier precursor B-3 (dry basis 70wt%), mix with 5.6g of hydroxypropyl methylcellulose, take 100ml of the above impregnation liquid, dilute it ten times, add it into the above mixture and knead it, after extrusion, dry it at 110℃ for 6h, and calcine it at 500℃ for 5h to obtain the hydrogenation catalyst carrier; impregnate the carrier by equal volume impregnation method, dry it at 90℃ for 10h, and calcine it at 400℃ for 4h to obtain hydrogenation catalyst D6, and the physicochemical properties of the obtained catalyst are listed in Table 2.
[0108] Table 1 Physicochemical properties of catalysts in the examples
[0109] serial number A B C <![CDATA[Specific surface area, m 2 / g]]> 191 225 182 Pore volume, mL / g 0.63 0.67 0.51 Pore size distribution >100nm 18 15 11 8-20nm 60 51 46 Catalyst composition, wt% <![CDATA[MoO3]]> 7.32 5.92 22.02 NiO 2.21 1.38 4.51 P 0.82 0.71 1.52 Lateral compressive strength, N / mm 12.7 11.9 12.9 Metal dispersion IMo / IAl 0.068 0.06 0.151 INi / IAl 0.035 0.022 0.067 B acid, mmol / g 0.119 0.122 0.131
[0110] Table 2 Comparative Example Catalyst Physicochemical Properties
[0111]
[0112]
[0113] From the comparison of the data in Table 1 and Table 2, it can be seen that the hydrogenation catalyst prepared by the method of the present invention has higher lateral pressure strength, good metal dispersion, higher B acid content, and is more suitable for use as a heavy oil hydrogenation catalyst.
[0114] The above catalyst was evaluated for activity on a continuous stirred autoclave (CSTR), with a catalyst loading of 100 mL. The ebullated bed reactor is similar to the continuous stirred tank reactor (CSTR), both of which have good full back mixing performance and comparable reaction kinetics. Therefore, a CSTR can be used instead of an ebullated bed reactor to evaluate the catalyst performance. The properties of the evaluated feedstock oil are shown in Table 3. The evaluation conditions are a reaction temperature of 420°C, a reaction pressure of 15 MPa, a hydrogen-to-oil volume ratio of 500:1, and a volume space velocity of 0.4 h -1 The data of comparative example 1 is taken as 100 as a benchmark, and the evaluation results of other samples after comparing the activities with those of comparative example 1 are shown in Table 4, and the values are rounded off.
[0115] Table 3 Raw oil properties
[0116]
[0117]
[0118] Table 4 Catalyst evaluation results
[0119]
Claims
1. A method for preparing a heavy oil hydrogenation catalyst, the preparation method comprising the following steps: S1: preparing a carrier precursor; the carrier precursor preparation method comprises the following steps: (1) Preparing sol: mixing silicon source A, template and water to obtain sol; (2) mixing the sol obtained in step (1) with alcohol and performing heat treatment to obtain a material stream A; (3) adding silicon source B, acidic aluminum source and alkaline aluminum source into a reactor containing bottom water, obtaining a stream B after reaction, and then mixing with a nonionic surfactant to obtain a stream C; (4) hydrothermally treating the material stream C under hydrothermal treatment conditions, and then washing and drying to obtain a carrier precursor; S2: mixing the support precursor obtained in step S1 with an auxiliary agent, then adding a solution containing an active metal, kneading, and then performing a first drying and a first calcination to obtain a catalyst precursor; S3: After introducing active metal components into the catalyst precursor obtained in step S2, a heavy oil hydrogenation catalyst is obtained after a second drying and a second calcination.
2. The method for preparing the heavy oil hydrogenation catalyst according to claim 1, characterized in that: The silicon source A in step (1) is one or more of ethyl orthosilicate, methyl orthosilicate, and silica sol, preferably ethyl orthosilicate.
3. The method for preparing the heavy oil hydrogenation catalyst according to claim 1, characterized in that: The template agent in step (1) is tetrapropylammonium hydroxide and / or tetrapropylammonium bromide; preferably tetrapropylammonium hydroxide.
4. The method for preparing the heavy oil hydrogenation catalyst according to claim 1, characterized in that: The alcohol in step (2) is a C1-C3 alcohol, which is one or more of a monohydric alcohol, a dihydric alcohol, or a polyhydric alcohol.
5. The method for preparing the heavy oil hydrogenation catalyst according to claim 1 or 4, characterized in that: The alcohol in step (2) is one or more of ethanol, ethylene glycol, and glycerol, preferably glycerol.
6. The method for preparing the heavy oil hydrogenation catalyst according to claim 1, characterized in that: In terms of weight ratio, the usage ratio of silicon source A, template, water and alcohol is (3-6): (5-8): (2-4): (0.5-5).
7. The method for preparing the heavy oil hydrogenation catalyst according to claim 1, characterized in that: The heat treatment operating conditions in step (2) are as follows: the treatment temperature is 60-100° C., and the treatment time is not more than 24 hours; preferably, the treatment temperature is 80-100° C., and the preferred treatment time is 8-12 hours.
8. The method for preparing the heavy oil hydrogenation catalyst according to claim 1, characterized in that: The silicon source B in step (3) is water glass and / or alkaline silica sol, preferably alkaline silica sol.
9. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The acidic aluminum source in step (3) is a water-soluble acidic aluminum-containing compound, preferably a water-soluble acidic inorganic aluminum-containing compound, especially a water-soluble inorganic strong acid aluminum salt, more preferably one or more selected from aluminum sulfate, aluminum nitrate, and aluminum chloride, preferably aluminum sulfate.
10. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The alkaline aluminum source in step (3) is an alkali metal aluminate solution; selected from one or more of sodium aluminate and potassium aluminate, preferably sodium aluminate.
11. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The pH value of the material stream B in step (3) is 4 to 7, preferably 5 to 6; the pH value of the material stream B is regulated by the amount of the acidic aluminum source.
12. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The reaction temperature in step (3) is 50°C to 90°C, preferably 50°C to 80°C.
13. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: In step (3), the aluminum content of the acidic aluminum source is 10-70 gAl2O3 / L in terms of Al2O3, the aluminum content of the alkaline aluminum source is 70-170 gAl2O3 / L in terms of Al2O3, and the silicon content of the second silicon source is 20-80 gSiO2 / L in terms of SiO2.
14. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The nonionic surfactant in step (3) is one or more of polyethylene glycol, alkyl alcohol amide, and polyether; preferably polyethylene glycol; the alkyl alcohol amide is one or more of lauryl diethanolamide and coconut oil fatty acid diethanolamide; the polyether is one or more of AEO-6 and AEO-9; the molecular weight of the polyethylene glycol is 200 to 1000, preferably 200 to 700.
15. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The weight ratio of the material stream A obtained in step (2) to the material stream C in step (3) is 1:80-100.
16. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The hydrothermal treatment conditions in step (4) are as follows: the treatment temperature is 100°C to 180°C, preferably 110°C to 160°C, and more preferably 120°C to 150°C; the treatment pressure is 0.1 to 0.5 MPa, preferably 0.1 to 0.3 MPa; the treatment time is 0.5h to 10h, preferably 0.5h to 6h.
17. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The drying conditions in step (4) are as follows: the drying temperature is 100 to 150° C., and the drying time is 6 to 10 hours.
18. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: In step S2, the auxiliary agent is one or more of methyl cellulose, hydroxymethyl cellulose, hydroxypropyl methyl cellulose, etc., and the content of the auxiliary agent is 0.5-5wt% based on the mass of the carrier precursor.
19. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: In step S2, the first drying conditions are as follows: the first drying temperature is 90-120° C., and the first drying time is 2-10 hours; the first roasting conditions are as follows: the first roasting temperature is 500-800° C., and the first roasting time is 4-10 hours.
20. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: In step S2, the active metal is one or more of the Group VIB metals and / or Group VIII metals. Based on the weight of the catalyst precursor and calculated as oxide, the concentration of the solution containing the active metal and the amount of the solution are such that the content of the Group VIII metal in the final catalyst precursor is 0.5 to 5 wt%, preferably 1.0 to 3.0 wt%, and the content of the Group VIB metal is 1.0 to 10.0 wt%, preferably 2.0 to 5.0 wt%.
21. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The hydrogenation active metal component described in step S3 is one or more of the Group VIB metals and / or Group VIII metals, calculated as oxide and based on the catalyst, the content of the Group VIII metal in the final catalyst is 1.5-10.0wt%, preferably 2.0-8.0wt%, and the content of the Group VIB metal is 5.0-25.0wt%, preferably 10.0-20.0wt%.
22. The method for preparing a heavy oil hydrogenation catalyst according to claim 1, characterized in that: In step S3, the second drying conditions include: the second drying temperature is 90-120° C., and the second drying time is 2-10 hours; the second roasting conditions include: the second roasting temperature is 300-600° C., and the second roasting time is 4-10 hours.
23. A heavy oil hydrogenation catalyst, wherein the catalyst is prepared by the method described in any one of claims 1 to 22.
24. The heavy oil hydrogenation catalyst according to claim 23, characterized in that: The hydrogenation catalyst includes a carrier and an active metal component. The carrier is a silicon-aluminum material. The metal element in the active metal component comes from at least one of the VIII group metal and the VIB group metal. The VIII group metal is one or more of Ni and Co, and the VIB group metal is one or more of Mo and W.
25. The heavy oil hydrogenation catalyst according to claim 23, characterized in that: The properties of the hydrogenation catalyst are as follows: pore volume is 0.50-0.80mL / g, specific surface area is 150-280m 2 / g.
26. The heavy oil hydrogenation catalyst according to claim 23, characterized in that: The pore distribution of the hydrogenation catalyst has the following characteristics: the pore volume of pores with a pore diameter of 8-20 nm accounts for 40%-70% of the total pore volume, and the pore volume of pores with a pore diameter of more than 100 nm accounts for more than 10% of the total pore volume.
27. The heavy oil hydrogenation catalyst according to claim 23, characterized in that: The catalyst diameter is less than 1.5 mm and the lateral pressure strength is greater than 10 N / mm.
28. Use of the heavy oil hydrogenation catalyst according to any one of claims 23 to 27 in a heavy oil hydrogenation reaction.
Citation Information
Patent Citations
Preparation method for hydrotreatment catalyst
CN103801346A
Hydrogenation catalyst for producing low-sulfur ship fuel and preparation method thereof
CN114749193A
Coal tar hydrogenation catalyst and preparation method thereof
CN114749194A
Crude oil hydrocracking catalyst and preparation method thereof
CN114749195A
Residual oil hydrodemetallization catalyst as well as preparation method and application thereof
CN116060056A