Flotation dispersing agent and flotation method for arsenopyrite type gold ore
By using sodium phytate or a combination of sodium lignosulfonate and calcium lignosulfonate as a dispersant in arsenopyrite-type gold deposits, combined with a specific flotation process, the problem of insufficient enrichment ratio in arsenopyrite-type gold deposits was solved, achieving efficient gold recovery and improved concentrate quality.
Patent Information
- Application Number
- CN202411174403.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-26
AI Technical Summary
In existing technologies, common dispersants have insufficient enrichment ratios in the flotation of arsenopyrite-type gold deposits, making it difficult to effectively improve gold recovery and concentrate quality.
By using sodium phytate as a single dispersant or in combination with calcium lignosulfonate as a dispersant, and in conjunction with a specific flotation process, including grinding, pH adjustment, addition of activators and collectors, the gold enrichment ratio can be significantly improved.
With a recovery rate of over 80%, the enrichment ratio reaches over 13, with a maximum of 18.26, significantly improving the flotation effect.
Smart Images

Figure BDA0005010313200000061 
Figure BDA0005010313200000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing, and in particular relates to a flotation dispersant and a flotation method for arsenopyrite-type gold ore. Background Art
[0002] Gold has stable physical and chemical properties, strong antioxidant capacity, is not easy to change color, does not dissolve at room temperature, and is not easy to lose. Gold has excellent electrical and thermal conductivity, ductility and toughness, and is easy to process. It is widely used in aerospace, communications, new materials, chemistry and other fields. As the demand for gold increases, easy-to-select gold resources are gradually exhausted. Sulfide-associated low-grade arsenopyrite gold mines have become a development resource that cannot be ignored in the gold selection industry.
[0003] Among the proven gold reserves in my country, associated gold accounts for 30% of the total gold reserves, but the gold production of associated gold only accounts for about 12% of the total gold production in my country. Arsenopyrite-type gold deposits are mainly distributed in the northwest region and play an extremely important role in my country's associated gold resources. Arsenopyrite-type gold deposits are fine-grained gold-bearing ores. The main gold-bearing mineral in the ore is arsenopyrite. The gold grade of the original ore is low. The gold mainly exists in the form of encapsulated gold. It is a typical refractory gold ore and often coexists with sericite, chlorite, etc. In flotation operations, fine-grained gangue minerals are prone to mudification and enter the flotation concentrate through "entrainment", thus affecting the quality of the concentrate.
[0004] At present, in view of the covering behavior of easily muddy minerals on gold-bearing sulfides in gold mines, commonly used dispersants include sodium hexametaphosphate, water glass, sodium carbonate, etc. For example, Qin Guanglin et al. [1] The effects of different dispersants on flotation were studied, but the enrichment ratios obtained were very low; for example, Qi Zhongxu et al. used water glass as a dispersant in Chinese invention patent CN 114618685 A; Wei Zongwu et al. used sodium hexametaphosphate as a dispersant in CN 105080728A. It was found that mixed dispersants have better flotation effects than single dispersants, such as Yi Zhengming. [2] It was found that the flotation effect was better when sodium carbonate: sodium silicate: sodium hexametaphosphate (3:2:1) was used as a mixed dispersant. However, whether these common dispersants are used alone or in combination, the enrichment ratio is usually no more than 5, and the flotation effect is not satisfactory.
[0005] In order to obtain better flotation effects, new combined dispersants have been developed, such as Xing Qingqing et al. [3] Using T9 and sodium carbonate as dispersants, the obtained enrichment ratio is more than 12, but the dispersant in this study is not easy to obtain and is difficult to promote. At present, there are few studies on composite dispersants for gold flotation. In addition to combining common dispersants, there are only a few composite dispersants including those developed by Xing Qingqing et al.
[0006] Therefore, whether it is possible to develop a new type of single dispersant to solve the shortcomings of common dispersants in terms of enrichment ratio, and based on this, further develop a composite dispersant with excellent enrichment ratio is urgently needed in this field.
[0007] References:
[0008] [1] Qin Guanglin, Li Guangsheng, Zhu Xingfu, et al. Experimental study on selectivity of ore washing mud in a gold mine [J]. China Mining,
[0009] 2022,31(S01):5.DOI:10.12075 / j.issn.1004-4051.2022.S1.045.
[0010] [2] Yi Zhengming. Experimental study on the beneficiation of a refractory gold ore[J]. Mining Express, 2008, (07): 31-33.
[0011] [3] Xing Qingqing, Ming Pingtian, Xiong Zhaohua, et al. Experimental study on ore dressing of a low-grade fine disseminated, easily muddy and difficult to process gold ore in Qinghai[J]. Gold, 2016, 37(11): 5. DOI: 10.11792 / hj20161112. Summary of the invention
[0012] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a flotation dispersant and a flotation method for arsenopyrite-type gold ore.
[0013] The objective of the present invention is achieved through the following technical solutions:
[0014] Sodium phytate is used as a dispersant in the flotation of arsenopyrite-type gold ore, in which the metal sulfide minerals include arsenopyrite, and gold particles are contained in the arsenopyrite in a microscopic or ultramicroscopic dispersed state.
[0015] A flotation dispersant for arsenopyrite-type gold ore, comprising sodium phytate and calcium lignin sulfonate; in the arsenopyrite-type gold ore, the metal sulfide minerals comprise arsenopyrite, and gold particles are contained in the arsenopyrite in a microscopic or ultramicroscopic dispersed state.
[0016] Preferably, the weight ratio of the sodium phytate to calcium lignin sulfonate is 10:1-3.
[0017] A flotation method for arsenopyrite gold ore, the flotation method comprising the following steps:
[0018] (1) grinding the arsenopyrite gold ore to obtain slurry, adjusting the pH to 9-10, then sequentially adding a dispersant, an activator, a collector and a frother and fully mixing the slurry, and obtaining a gold rough concentrate and a gold roughing tailings through roughing;
[0019] (2) adding a dispersant to the gold rough concentrate for concentrating to obtain a flotation gold concentrate;
[0020] (3) adding a dispersant to the gold rougher tailings at least once;
[0021] The dispersant is sodium phytate or a composition comprising sodium phytate and calcium lignin sulfonate;
[0022] In the arsenopyrite-type gold ore, the metal sulfide minerals include arsenopyrite, and gold particles are contained in the arsenopyrite in a microscopic or ultramicroscopic dispersed state.
[0023] Preferably, in step (1), the weight fraction of the slurry is 30-35%.
[0024] Preferably, the collector is amyl xanthate and butyl ammonium xanthate.
[0025] Preferably, the activator is copper sulfate; and / or the foaming agent is 2# oil; and / or the agent used to adjust the pH is sodium carbonate.
[0026] Preferably, in step (1), the flotation time of the roughing is 6 to 8 minutes; the amount of sodium carbonate is 1000 to 1500 g / t of raw ore, the amount of dispersant is 100 to 150 g / t of raw ore, the amount of copper sulfate is 150 to 200 g / t of raw ore, the amount of amyl xanthate is 100 to 200 g / t of raw ore, the amount of butyl ammonium black medicine is 20 to 80 g / t of raw ore, and the amount of 2# oil is 10 to 20 g / t of raw ore.
[0027] Preferably, in step (2), the number of times of the selection is 1 to 3 times, and the amount of the dispersant added in each selection is 10 to 30 g / t of raw ore; in step (3), the number of times of the scavenging is 1 to 3 times, and the dispersant is added in the first scavenging, and the amount of the dispersant is 20 to 30 g / t of raw ore. When the number of scavenging exceeds 1 time, the dispersant is not added in the remaining scavenging except the first scavenging.
[0028] Preferably, the dispersant is a combination of sodium phytate and calcium lignin sulfonate, and the weight ratio of sodium phytate to calcium lignin sulfonate is 10:2.
[0029] As shown in the corresponding embodiments of the present invention, the present invention uses sodium phytate as a dispersant for flotation of arsenopyrite-type gold ore, which has obvious advantages over common dispersants in the art (such as sodium hexametaphosphate or sodium silicate), and can significantly improve the enrichment ratio and the flotation effect. The chemical formula of sodium phytate is C6H6Na 12 O 24P6 is generally used as an antioxidant and color preservative for fruit and vegetable juice drinks, meat products, and seafood. The present invention uses it for the first time as a dispersant for the flotation of arsenopyrite-type gold ore, and achieves excellent results.
[0030] As shown in the corresponding embodiments of the present invention, when the sodium phytate and calcium lignin sulfonate combination is used as a dispersant, the enrichment ratio can be further improved. Combined with Comparative Example 3, it can be seen that sodium phytate and calcium lignin sulfonate have a synergistic effect in the present invention. Beneficial effects of the present invention:
[0031] The present invention uses sodium phytate as a dispersant for flotation of arsenopyrite gold ore, and on this basis develops a flotation dispersant for arsenopyrite gold ore and a corresponding flotation method for arsenopyrite gold ore. The present invention overcomes the difficulty of the prior art in taking both recovery rate and enrichment ratio into consideration, and on the basis of a recovery rate of more than 80%, the enrichment ratio reaches more than 13, and can reach up to 18.26 at the highest. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described in detail below, but the protection scope of the present invention is not limited to the following.
[0033] Example 1
[0034] A certain arsenopyrite gold mine in Northwest my country is a high-temperature hydrothermal altered rock-type gold ore in the compressive structural fracture zone in mylonite. The main precious metal minerals in the ore are gold minerals, mainly fine-grained gold, with an Au grade of 2.26g / t. Most of the gold particles are contained in arsenopyrite in a microscopic and ultramicroscopic dispersed state, followed by gangue minerals such as sericite, chlorite and quartz, and a few are associated or encapsulated with pyrite and pyrrhotite. The metal sulfide minerals in the ore are mainly pyrite, arsenopyrite, rhombohedral arsenic iron ore and pyrrhotite, accounting for about 5% of the total mineral content. The main gangue minerals are quartz, sericite, chlorite, feldspar, kaolin, etc. The hardness of the gangue minerals varies greatly. In the grinding process, in order to fully dissociate the minerals, it is easy to produce ore mud, which causes a cover behavior on the surface of the gold-bearing sulfide, deteriorating the flotation index.
[0035] The specific plan for flotation of the above-mentioned arsenopyrite gold ore is as follows:
[0036] (1) The gold ore was ground, and the content of the floating sample with a particle size of 0.074 mm accounted for 70.09%. After grinding, the ore pulp was prepared, and the mass fraction of the ore pulp was 33%.
[0037] (2) Based on each ton of raw ore, 1500 g / t of sodium carbonate was added to the pulp, the pH value of the pulp was adjusted to 9.0, and the mixture was stirred for 3 min; then 100 g / t of sodium phytate as a dispersant was added, and after stirring for 3 min, 170 g / t of copper sulfate as an activator was added; after stirring for 4 min, a collector (100 g / t of amyl xanthate and 80 g / t of butyl ammonium black powder) was added, and the mixture was stirred for 3 min; finally, 10 g / t of frother 2# oil was added, and the mixture was stirred for 1 min; the flotation time was controlled to be 8 min, and a rough gold concentrate and a rough tailing were obtained.
[0038] (3) The rough gold concentrate is subjected to three rounds of concentrating. The dispersant sodium phytate added in the first, second and third rounds is 30 g / t, 20 g / t and 10 g / t respectively. Each round of concentrating obtains its own concentrating middlings. The last round of concentrating obtains gold concentrate in addition to the concentrating middlings. The first, second and third rounds of concentrating middlings are middlings I, II and III respectively. The middlings are returned in sequence.
[0039] (4) The roughing tailings were scavenged three times. In the first scavenging, 700 g / t of sodium carbonate as a pH adjuster, 20 g / t of sodium phytate as a dispersant, 80 g / t of copper sulfate as an activator, 50 g / t of amyl xanthate as a combined collector, 40 g / t of butyl ammonium black powder, and 5 g / t of 2# oil as a foaming agent were added. In the second scavenging, 40 g / t of copper sulfate as an activator, 25 g / t of amyl xanthate as a combined collector, 20 g / t of butyl ammonium black powder, and 3 g / t of 2# oil as a foaming agent were added. In the third scavenging, collectors (25 g / t of amyl xanthate and 20 g / t of butyl ammonium black powder) were added. Each scavenging process obtains its own scavenged ore. The third scavenging process obtains not only the scavenged ore but also the final tailings. The first, second and third scavenging ore are respectively the IV ore, the V ore and the VI ore. The IV ore is combined with the V ore and returned to the gold roughing process for reselection. The VI ore is returned to the first scavenging process for reselection.
[0040] Example 2
[0041] The parameters of the raw ore, mineral processing technology, etc. in this embodiment are the same as those in Example 1, with the only difference being that sodium phytate and calcium lignin sulfonate (weight ratio 1:2) are used as dispersants in this embodiment, and other conditions such as the selection of collectors, dosage of reagents, and subsequent process flow are the same as those in Example 1.
[0042] Example 3
[0043] The parameters of the raw ore, mineral processing technology, etc. in this embodiment are the same as those in Example 1, with the only difference being that sodium phytate and calcium lignin sulfonate (weight ratio 1:1) are used as dispersants in this embodiment, and other conditions such as the selection of collectors, dosage of reagents, and subsequent process flow are the same as those in Example 1.
[0044] Example 4
[0045] The parameters of the raw ore, mineral processing technology, etc. in this embodiment are the same as those in Example 1, with the only difference being that sodium phytate and calcium lignin sulfonate (weight ratio 1:3) are used as dispersants in this embodiment, and other conditions such as the selection of collectors, dosage of reagents, and subsequent process flow are the same as those in Example 1.
[0046] Example 5
[0047] The parameters such as the raw ore and the beneficiation process used in this embodiment are the same as those in Example 1, with the only difference being that Y-89 and butyl ammonium black medicine are used as collectors in this embodiment, and other conditions such as sodium phytate as the dispersant, the dosage of the agent and the subsequent process flow are the same as those in Example 1.
[0048] Example 6
[0049] The parameters such as the raw ore and the beneficiation process used in this embodiment are the same as those in Example 1, with the only difference being that butyl xanthate and butyl ammonium black medicine are used as a combined collector in this embodiment, and other conditions such as sodium phytate as a dispersant, the dosage of the agent and the subsequent process flow are the same as those in Example 1.
[0050] Comparative Example 1
[0051] The parameters of the raw ore, ore dressing process and the like in this comparative example are the same as those in Example 1, with the only difference being that sodium hexametaphosphate is used as the dispersant in Comparative Example 1, and other conditions such as the selection of the collector, the dosage of the reagent and the subsequent process flow are the same as those in Example 1.
[0052] Comparative Example 2
[0053] The parameters of the raw ore, ore dressing process and the like in this comparative example are the same as those in Example 1, with the only difference being that sodium silicate is used as the dispersant in Comparative Example 2, and other conditions such as the selection of the collector, the dosage of the reagent and the subsequent process flow are the same as those in Example 1.
[0054] Comparative Example 3
[0055] The parameters of the raw ore, ore dressing process and the like in this comparative example are the same as those in Example 1, except that calcium lignin sulfonate is used as the dispersant in Comparative Example 3, and other conditions such as the selection of the collector, the dosage of the reagent and the subsequent process flow are the same as those in Example 1.
[0056] Comparative Example 4
[0057] The parameters of the raw ore, ore dressing process and the like in this comparative example are the same as those in Example 1, with the only difference being that no dispersant is added in Comparative Example 4, and other conditions such as the selection of collector, dosage of reagent and subsequent process flow are the same as those in Example 1.
[0058] The flotation conditions of arsenopyrite-type gold ores in the above Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Table 1.
[0059] Table 1
[0060]
[0061]
[0062] As shown in Table 1, after adopting the flotation reagent of the present invention, adding dispersant sodium phytate, and adopting a beneficiation process of one roughing, three cleaning, and three scavenging, a gold concentrate with an Au grade of at least 29.28 g / t is finally obtained, and the enrichment ratio is at least 13. In particular, under the same flotation process, when a combination of sodium phytate and calcium lignin sulfonate is used as a dispersant, the enrichment ratio can reach up to 18.26. When other dispersants or no dispersant are used, the flotation effect is significantly poor.
Claims
1. Application of sodium phytate as a dispersant in flotation of arsenopyrite-type gold ore, in which the metal sulfide minerals include arsenopyrite, and gold particles are contained in the arsenopyrite in a microscopic or ultramicroscopic dispersed state.
2. A flotation dispersant for arsenopyrite-type gold ore, It is characterized in that The flotation dispersant includes sodium phytate and calcium lignin sulfonate; in the arsenopyrite-type gold ore, the metal sulfide minerals include arsenopyrite, and most of the gold particles are contained in the arsenopyrite in a microscopic or ultramicroscopic dispersed state.
3. The flotation dispersant according to claim 2, It is characterized in that The weight ratio of the sodium phytate to the calcium lignin sulfonate is 10:1-3.
4. A flotation method for arsenopyrite-type gold ore, It is characterized in that The flotation method comprises the following steps: (1) grinding the arsenopyrite gold ore to obtain slurry, adjusting the pH to 9-10, then sequentially adding a dispersant, an activator, a collector and a frother and fully mixing the slurry, and obtaining a gold rough concentrate and a gold roughing tailings through roughing; (2) adding a dispersant to the gold rough concentrate for concentrating to obtain a flotation gold concentrate; (3) adding a dispersant to the gold rougher tailings at least once; The dispersant is sodium phytate or a composition comprising sodium phytate and calcium lignin sulfonate; In the arsenopyrite-type gold ore, the metal sulfide minerals include arsenopyrite, and most of the gold particles are contained in the arsenopyrite in a microscopic or ultramicroscopic dispersed state.
5. The flotation method according to claim 4, It is characterized in that In step (1), the weight fraction of the slurry is 30-35%.
6. The flotation method according to claim 4, It is characterized in that The collectors are amyl xanthate and butyl ammonium black medicine.
7. The flotation method according to any one of claims 4 to 6, It is characterized in that The activator is copper sulfate; and / or the foaming agent is 2# oil; and / or the agent used to adjust pH is sodium carbonate.
8. The flotation method according to claim 7, It is characterized in that In step (1), the flotation time of the roughing is 6 to 8 minutes; the amount of sodium carbonate is 1000 to 1500 g / t of the raw ore, the amount of the dispersant is 100 to 150 g / t of the raw ore, the amount of copper sulfate is 150 to 200 g / t of the raw ore, the amount of amyl xanthate is 100 to 200 g / t of the raw ore, the amount of butyl ammonium black medicine is 20 to 80 g / t of the raw ore, and the amount of 2# oil is 10 to 20 g / t of the raw ore.
9. The flotation method according to claim 8, It is characterized in that In step (2), the number of times of selection is 1 to 3 times, and the amount of the dispersant added in each selection is 10 to 30 g / t of raw ore; in step (3), the number of times of scavenging is 1 to 3 times, and the dispersant is added in the first scavenging, and the amount of the dispersant is 20 to 30 g / t of raw ore; when the number of scavenging exceeds 1 time, except for the first scavenging, the dispersant is not added in the remaining scavenging.
10. The flotation method according to claim 9, It is characterized in that The dispersant is a composition of sodium phytate and calcium lignin sulfonate, and the weight ratio of sodium phytate to calcium lignin sulfonate is 10:2.
Citation Information
Patent Citations
Flotation separation method of antimony sulfide and gold-bearing pyrite
CN105080728A
Method for recovering gold from clay type gold ore
CN114618685A