Method for continuously and integrally preparing reinforced composite diaphragm by spraying and pre-solidifying

Through the continuous integrated preparation method of spray pre-solidation, the mechanical strength and resistance of composite diaphragms in high electrolytic temperature and alkaline environments are solved, and efficient and low-cost diaphragm preparation is achieved, which is suitable for the hydrogen production process of water electrolysis.

CN119016307APending Publication Date: 2024-11-26SUZHOU XIBEIYOU HYDROGEN ENERGY TECH CO LTD

Patent Information

Application Number
CN202410901128.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-30
Publication Date
2024-11-26

Smart Images

  • Figure CN119016307A_ABST
    Figure CN119016307A_ABST
Patent Text Reader

Abstract

The invention discloses a method for continuously and integrally preparing a reinforced composite diaphragm by spraying and pre-solidifying, which comprises the following specific steps of: A, injecting a milk white slurry solution into two sides of a grid support carrier in the middle of a scraper, and obtaining an uncured wet composite film of which two sides are uniformly coated with slurry under the traction and driving of a roller; b, the uncured wet composite wet film is subjected to phase inversion under the action of anti-solvent spray droplets prepared by atomizers on the two sides to form a pre-cured surface, and then the pre-cured surface enters a first-stage coagulating bath to be subjected to full phase inversion to obtain a white cured diaphragm; and C, further introducing the white cured diaphragm into a secondary coagulating bath through a traction roller, rinsing, and rolling to obtain a finished product of the alkaline water electrolysis composite diaphragm. The method has the advantages of simple implementation process, easy satisfaction of required conditions, simple and easy repetition of steps, low process cost and high production speed, and the microstructure on the surface and inside of the diaphragm is regulated and controlled by changing spray components, spray rate and atomization temperature, so that the comprehensive performance of the composite diaphragm is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparing diaphragms for hydrogen production by electrolysis of water, and in particular to a method for preparing a reinforced composite diaphragm by spray pre-solidification and continuous integration. Background Art

[0002] As a green and clean energy, hydrogen has the advantages of light weight, high calorific value, and pollution-free combustion, so it is considered one of the most effective energy carriers to achieve carbon neutrality. In the process of burning and releasing energy, hydrogen does not emit carbon-containing greenhouse gases, but only produces water, which is a zero-carbon emission reaction. Therefore, vigorously developing the hydrogen energy industry is of extraordinary significance to achieving the dual carbon goals. In order to achieve a low-carbon society, the hydrogen energy industry should combine the use of natural renewable energy such as solar energy and wind energy to produce hydrogen.

[0003] The power generation of wind and solar energy systems depends largely on climate conditions, so it fluctuates greatly, resulting in an imbalance between power supply and demand. In recent years, in order to store excess electricity, people have used power-to-gas technology to produce gas fuels such as hydrogen. As the output of renewable energy increases, the demand for storage and transportation of the produced gas fuel energy also increases.

[0004] As an important means of energy production, water electrolysis can convert electrical energy into hydrogen energy. During the electrolysis process of the alkaline electrolyzer, the anode hydroxide is oxidized to produce oxygen, and the cathode water is reduced to produce hydrogen. The function of the diaphragm is to prevent the mixing of hydrogen and oxygen. In addition, the diaphragm should also have the function of allowing hydroxide ions to flow smoothly from the cathode chamber to the anode chamber; at the same time, it should be able to withstand the corrosion of high-concentration alkali solutions, have good mechanical strength, be able to withstand the impact of electrolytes and generated gases for a long time without structural damage, and be able to maintain chemical stability under high electrolysis temperatures and concentrated alkali conditions.

[0005] In the composite membrane preparation method disclosed in EP0232923, the slurry is coated on a glass sheet, and the membrane is solidified by phase inversion, and then peeled off the glass sheet. However, this preparation method will cause the surface and internal structure on both sides of the membrane to be uneven and have large morphological differences. WO2009147084 and WO2009147086 disclose a process for preparing a reinforced composite membrane, that is, coating the slurry on both sides of a porous support net. However, this method is not the best method for preparing thin membranes. When this method enters the phase inversion stage, the fluctuation of the water surface will cause the membrane surface to present a corrugated structure, forming an uneven surface, which will have a certain impact on the performance of the membrane and the subsequent installation of the electrolytic cell.

[0006] Therefore, in the development trend of alkaline water electrolysis to produce hydrogen, a method is needed that can continuously and integratedly prepare high-quality reinforced composite diaphragms with excellent comprehensive performance. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration, which has a simple and easy operation process, low equipment cost and high production efficiency.

[0008] In order to solve the above technical problems, the present invention provides a method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration, wherein a roller is used to pull a grid support carrier, and a scraper, an atomizer, a primary coagulation bath and a secondary coagulation bath are sequentially arranged along the pulling direction, comprising the following steps:

[0009] A. Inject the coating slurry solution into both sides of the grid support carrier between the two scrapers through a pump, so that the slurry solution fully infiltrates the grid support carrier, and obtain an uncured wet diaphragm with the slurry solution evenly coated on both sides under the downward traction of the roller;

[0010] B. The uncured wet diaphragm is pulled by the roller and moves to the area between the bottom of the scraper and the surface of the primary coagulation bath. The atomizers on both sides of the uncured wet diaphragm spray to form anti-solvent spray droplets, which undergo local phase transformation under the action of the anti-solvent spray droplets to form a pre-cured diaphragm;

[0011] Among them, in the anti-solvent spray droplets, the spray droplets with a particle size of 1-5 μm need to account for 60%-100% of the spray droplets, the temperature is 20-60°C, the spray rate is 1-10 ml / min, the membrane surface is exposed to the spray for 5-60 seconds, and the thickness formed by the spray on both sides of the uncured membrane is 5-70 μm;

[0012] C. Then the pre-cured diaphragm enters the primary coagulation bath under the traction of the roller, undergoes a full phase conversion, and obtains a fully cured diaphragm;

[0013] The full phase inversion time is 2-30min, and the primary coagulation bath temperature is 5-90°C;

[0014] D. The fully solidified membrane is pulled into the secondary coagulation bath under the traction of rollers for rinsing;

[0015] The rinsing time is 2-30min, and the secondary coagulation bath temperature is 5-90°C;

[0016] E. Finally, the rinsed and fully cured diaphragm is rolled up to obtain a finished film.

[0017] Furthermore, in step A, the slurry solution is composed of an alkali-resistant polymer solution and inorganic nanoparticles.

[0018] Furthermore, in the atomizer anti-solvent spray droplets described in step B, the percentage of anti-solvent spray droplets with a particle size range of 1-5 μm in the total droplet amount is 80%-100%, and the spray temperature of the atomizer is preferably 25°C.

[0019] Furthermore, the spray rate of the atomizer in step B is preferably 5 ml / min, the atomization time is preferably 30 s, and the thickness formed by the spray on both sides of the uncured wet diaphragm is 3-5 μm.

[0020] Furthermore, the atomizer anti-solvent spray in step B is one or more of nitrogen methyl pyrrolidone aqueous solution, pure water, ethanol aqueous solution, and isopropanol aqueous solution, wherein the concentration of nitrogen methyl pyrrolidone aqueous solution is 10%-90%, preferably 40%-50%; the concentration of ethanol aqueous solution is 40%-100%, preferably 50%-60%; the concentration of isopropanol aqueous solution is 40%-100%, preferably 50%-60%.

[0021] Furthermore, the primary coagulation bath in step C is composed of pure water, the time is preferably 5 minutes, the temperature is preferably 20°C-40°C, more preferably 25°C.

[0022] Furthermore, the secondary coagulation bath in step D is composed of pure water, the time is preferably 5 minutes, the temperature is preferably 20°C-40°C, more preferably 25°C.

[0023] Beneficial effects of the present invention:

[0024] 1. The membrane preparation process of the present invention is simple to implement, the required conditions are easy to meet, the steps are simple and easy to repeat, the process cost is low, the production speed is fast, the application range is wide, and it can be used for the preparation of alkaline water electrolysis composite diaphragms of all systems;

[0025] 2. During the preparation process, spraying is used to pre-solidify the surface of the diaphragm. While increasing the production speed of the diaphragm, the surface and internal microstructure of the diaphragm can be regulated by changing the spray composition, rate and atomization temperature, forming a porous surface and internal sponge-like three-dimensional structure. The diaphragm has excellent properties of high strength and low resistance, ensuring stable and efficient operation of the electrolytic cell;

[0026] 3. The solidified surface layer of the diaphragm formed by the spraying action prevents the interference of the coagulation bath fluctuation on the curing process on both sides of the diaphragm, which can ensure the uniform phase transformation and uniform thickness on the surfaces of both sides of the diaphragm, and finally form a high-performance finished electrolytic water composite diaphragm. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a flow chart of the preparation method of the present invention;

[0028] Figure 2It is a schematic diagram of the preparation process of the pre-cured composite diaphragm of the present invention;

[0029] Figure 3 Scanning electron microscope characterization images of the surface and cross section of the composite diaphragm prepared in Comparative Example 1;

[0030] Figure 4 Scanning electron microscope characterization images of the surface and cross section of the composite diaphragm prepared in Example 1;

[0031] Figure 5 Scanning electron microscope characterization images of the surface and cross section of the composite diaphragm prepared in Example 2;

[0032] Figure 6 Scanning electron microscope characterization images of the surface and cross section of the composite diaphragm prepared in Example 3;

[0033] Figure 7 The surface and cross-section scanning electron microscope characterization images of the composite diaphragm prepared in Example 4;

[0034] Figure 8 Scanning electron microscope characterization images of the surface and cross section of the composite diaphragm prepared in Example 5;

[0035] Fig. 9 The surface and cross-section scanning electron microscope images of the composite diaphragm prepared in Example 6 are shown. DETAILED DESCRIPTION

[0036] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0037] Reference Figure 1 As shown, the present invention uses a roller to pull the grid support carrier, and a scraper, an atomizer, a primary coagulation bath and a secondary coagulation bath are sequentially arranged along the pulling direction, and finally a method for winding up to obtain a finished film is a method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration, wherein the number of scrapers is 2 and they are arranged on both sides of the two surfaces of the grid support carrier, the number of atomizers is 2 and they are also arranged on both sides of the two surfaces of the grid support carrier, pure water is placed in both the primary coagulation bath and the secondary coagulation bath, and the material of the grid support carrier is PPS; specifically, the present application is described in detail through multiple embodiments:

[0038] Comparative Example 1

[0039] First, polysulfone resin was dissolved in N-methylpyrrolidone (NMP) and stirred for 4 hours to obtain a uniformly dispersed NMP-polysulfone solution; then zirconium dioxide was added and stirred for another 4 hours to obtain a milky white coating slurry solution;

[0040] Then, the coating slurry solution prepared in the above manner is injected into both sides of the grid support carrier between the two scrapers by a pump, so that the slurry solution fully infiltrates the grid support carrier, and is coated on the surfaces of both sides of the grid support carrier under the downward traction of the roller, so as to obtain an uncured composite diaphragm with the slurry evenly coated on both sides;

[0041] Then, the uncured composite membrane is directly pulled into the primary coagulation bath by rollers for 5 minutes to fully transform the phase. The primary coagulation bath is pure water at a temperature of 25°C. The fully cured membrane is continuously pulled and introduced into the secondary coagulation bath for rinsing for 5 minutes to completely remove the excess solvent. The secondary coagulation bath is pure water at 25°C.

[0042] Finally, the rinsed and fully cured diaphragm is rolled up to obtain a finished film, i.e., a composite diaphragm.

[0043] The surface and cross-sectional scanning electron microscopy images of the prepared composite diaphragm are shown in Figure 2. Figure 3 As shown in the figure, due to the absence of spray pre-solidification, the surface of the uncured composite diaphragm undergoes a comprehensive and intense phase transformation with pure water, forming a dense and non-porous surface and an internal structure with large finger-like pores. Although an overly dense diaphragm surface is conducive to increasing the bubble point pressure (6.22 bar), it will also hinder the migration of ions during the electrolysis process, increasing the energy consumption of the electrolyzer; and the large finger-like pores in the middle will reduce the mechanical properties of the diaphragm, and may also extend to the surface to cause defects, causing the bubble point pressure to drop, and the diaphragm's gas barrier property will deteriorate, which is very likely to cause the crossover of hydrogen and oxygen in the electrolyzer, resulting in safety accidents.

[0044] Example 1

[0045] First, polysulfone resin was dissolved in N-methylpyrrolidone (NMP) and stirred for 4 hours to obtain a uniformly dispersed NMP-polysulfone solution; then zirconium dioxide was added and stirred for another 4 hours to obtain a milky white coating slurry solution;

[0046] Then, the coating slurry solution prepared in the above manner is injected into both sides of the grid support carrier between the two scrapers by a pump, so that the slurry solution fully infiltrates the grid support carrier, and is coated on the surfaces of both sides of the grid support carrier under the downward traction of the roller, so as to obtain an uncured composite diaphragm with the slurry evenly coated on both sides;

[0047] Then, the uncured composite membrane is pulled into the area between the bottom of the scraper and the surface of the primary coagulation bath by a roller, and the uncured composite membrane undergoes phase transformation under the action of the anti-solvent spray droplets atomized by the atomizers on both sides to form a pre-cured surface. Figure 2As shown, the anti-solvent spray component used in this embodiment is pure water; in the water mist droplets formed by the atomizer, the water mist droplets with a particle size of 1-5μm need to account for 60%-100% of the total water mist droplets, the atomization temperature is 25°C, the spray rate is 1ml / min, and the accumulation degree of droplet particles on the surface of the diaphragm is affected by the spray rate and the roller traction rate. The roller traction rate can determine the time for the diaphragm surface to be exposed to the spray. This time is set to 30s, and then the pre-cured diaphragm is pulled into the primary coagulation bath under the traction of the roller for 5min to fully transform the phase. The primary coagulation bath is pure water with a temperature of 25°C; it is continued to be pulled into the secondary coagulation bath for rinsing for 5min to completely remove the excess solvent. The secondary coagulation bath is pure water at 25°C;

[0048] Finally, the rinsed and fully cured diaphragm is rolled up to obtain a finished film, i.e., a composite diaphragm.

[0049] The surface and cross-sectional scanning electron microscopy images of the prepared composite diaphragm are shown in Figure 2. Figure 4 As shown, due to the low spray rate, the small and uneven number of atomized droplets, and the solidified layer thickness of <1 μm, the surface solidification effect is not obvious, resulting in a relatively violent phase transformation in the primary coagulation bath and the formation of finger-like holes inside the diaphragm.

[0050] Example 2

[0051] First, polysulfone resin was dissolved in N-methylpyrrolidone (NMP) and stirred for 4 hours to obtain a uniformly dispersed NMP-polysulfone solution; then zirconium dioxide was added and stirred for another 4 hours to obtain a milky white coating slurry solution;

[0052] Then, the uncured composite membrane is pulled into the area between the bottom of the scraper and the surface of the primary coagulation bath by rollers. The uncured composite membrane undergoes phase transformation under the action of the anti-solvent spray droplets atomized by the atomizers on both sides to form a pre-cured surface. The anti-solvent spray component used in this embodiment is pure water; in the water mist droplets formed by the atomizer, the water mist droplets with a particle size of 1-5 μm must account for 60%-100% of the total water mist droplets, the atomization temperature is 25°C, the spray rate is 5 ml / min, the accumulation degree of droplet particles on the membrane surface is affected by the spray rate and the roller traction rate, and the roller traction rate can determine the time the membrane surface is exposed to the spray, which is set to 30s. Then, the pre-cured membrane is pulled into the primary coagulation bath under the traction of the roller and fully phase transformed for 5 minutes. The primary coagulation bath is pure water at a temperature of 25°C; it is continued to be pulled into the secondary coagulation bath for rinsing for 5 minutes to completely remove excess solvent. The secondary coagulation bath is pure water at 25°C;

[0053] Finally, the rinsed and fully cured diaphragm is rolled up to obtain a finished film, i.e., a composite diaphragm.

[0054] The surface and cross-sectional scanning electron microscopy images of the prepared composite diaphragm are shown in Figure 2. Figure 5 As shown, this embodiment increases the spray rate to 5 ml / min. Since an appropriate amount of atomized liquid droplets fall on the surface of the wet diaphragm to undergo phase transformation to form a relatively uniform surface microporous structure, and the surface curing degree is sufficient (pre-curing layer thickness 4 μm), the phase transformation rate occurring in the primary coagulation bath is slowed down, so that three-dimensional sponge-like pores are formed inside the diaphragm, which ensures the porosity of the diaphragm while also enhancing the mechanical properties of the diaphragm to a certain extent. The appropriately sized surface pores not only ensure a higher bubble point pressure (3.08 bar) but also further improve the ion migration ability of the diaphragm.

[0055] Example 3

[0056] First, polysulfone resin was dissolved in N-methylpyrrolidone (NMP) and stirred for 4 hours to obtain a uniformly dispersed NMP-polysulfone solution; then zirconium dioxide was added and stirred for another 4 hours to obtain a milky white coating slurry solution;

[0057] Then, the coating slurry solution prepared in the above manner is injected into both sides of the grid support carrier between the two scrapers by a pump, so that the slurry solution fully infiltrates the grid support carrier, and is coated on the surfaces of both sides of the grid support carrier under the downward traction of the roller, so as to obtain an uncured composite diaphragm with the slurry evenly coated on both sides;

[0058] Then, the uncured composite membrane is pulled into the area between the bottom of the scraper and the surface of the primary coagulation bath by a roller, and the uncured composite membrane undergoes phase transformation under the action of the anti-solvent spray droplets atomized by the atomizers on both sides to form a pre-cured surface. Figure 2 As shown, the anti-solvent spray component used in this embodiment is pure water; in the water mist droplets formed by the atomizer, the water mist droplets with a particle size of 1-5μm need to account for 60%-100% of the total water mist droplets, the atomization temperature is 25°C, the spray rate is 8ml / min, and the accumulation degree of the droplet particles on the surface of the diaphragm is affected by the spray rate and the roller traction rate. The roller traction rate can determine the time for the diaphragm surface to be exposed to the spray. This time is set to 30s, and then the pre-cured diaphragm is pulled into the primary coagulation bath under the traction of the roller for 5min to fully transform the phase. The primary coagulation bath is pure water with a temperature of 25°C; it is continued to be pulled into the secondary coagulation bath for rinsing for 5min to completely remove the excess solvent. The secondary coagulation bath is pure water at 25°C;

[0059] Finally, the rinsed and fully cured diaphragm is rolled up to obtain a finished film, i.e., a composite diaphragm.

[0060] The surface and cross-sectional scanning electron microscopy images of the prepared composite diaphragm are shown in Figure 2. Figure 6As shown, this embodiment further increases the spray rate to 8 ml / min. Since excessive atomized droplets will densely fall on the surface of the wet diaphragm and fuse to undergo phase transformation, resulting in excessively large pores, the bubble point pressure of the diaphragm is reduced (0.93 bar), and the thickness of the pre-curing layer is increased to 8 μm, which makes the phase transformation of the diaphragm in the primary coagulation bath too slow, thereby forming more dense three-dimensional sponge-like pores inside, which will reduce the ion migration ability of the diaphragm.

[0061] Example 4

[0062] First, polysulfone resin was dissolved in N-methylpyrrolidone (NMP) and stirred for 4 hours to obtain a uniformly dispersed NMP-polysulfone solution; then zirconium dioxide was added and stirred for another 4 hours to obtain a milky white coating slurry solution;

[0063] Then, the coating slurry solution prepared in the above manner is injected into both sides of the grid support carrier between the two scrapers by a pump, so that the slurry solution fully infiltrates the grid support carrier, and is coated on the surfaces of both sides of the grid support carrier under the downward traction of the roller, so as to obtain an uncured composite diaphragm with the slurry evenly coated on both sides;

[0064] Then, the uncured composite membrane is pulled into the area between the bottom of the scraper and the surface of the primary coagulation bath by a roller, and the uncured composite membrane undergoes phase transformation under the action of the anti-solvent spray droplets atomized by the atomizers on both sides to form a pre-cured surface. Figure 2 As shown, the anti-solvent spray component used in this embodiment is a 50% NMP aqueous solution; in the water mist droplets formed by the atomizer, the water mist droplets with a particle size of 1-5μm need to account for 60%-100% of the total water mist droplets, the atomization temperature is 25°C, the spray rate is 5ml / min, the accumulation degree of droplet particles on the surface of the diaphragm is affected by the spray rate and the roller traction rate, and the roller traction rate can determine the time the diaphragm surface is exposed to the spray, and this time is set to 30s, and then the pre-cured diaphragm is pulled into the primary coagulation bath under the traction of the roller, and a full phase conversion is carried out for 5min. The primary coagulation bath is pure water with a temperature of 25°C; it is continued to be pulled into the secondary coagulation bath for rinsing for 5min to completely remove the excess solvent. The secondary coagulation bath is pure water at 25°C;

[0065] Finally, the rinsed and fully cured diaphragm is rolled up to obtain a finished film, i.e., a composite diaphragm.

[0066] The surface and cross-sectional scanning electron microscopy images of the prepared composite diaphragm are shown in Figure 2. Figure 7As shown, this embodiment uses a 50% NMP aqueous solution as the anti-solvent spray component, and the spray rate is set to 5 ml / min, so that an appropriate amount of atomized droplets fall on the surface of the wet diaphragm to undergo phase transformation and form a uniform surface microporous structure, and the thickness of the surface solidified layer is appropriately 5 μm (the addition of NMP reduces the water content of the droplets and slows down the surface solidification rate), so that the phase transformation rate of the pre-cured wet diaphragm in the primary coagulation bath is slowed down, thereby forming loose three-dimensional sponge-like pores inside. This structure not only ensures the porosity of the diaphragm, but also enhances the mechanical properties of the diaphragm to a certain extent. The surface pores of appropriate size (pore size ≤ 100 nm) and uniform distribution can not only improve the ion migration ability of the diaphragm during the operation of the electrolytic cell, but also maintain a high air tightness (bubble point pressure = 5.06 bar).

[0067] Example 5

[0068] First, polysulfone resin was dissolved in N-methylpyrrolidone (NMP) and stirred for 4 hours to obtain a uniformly dispersed NMP-polysulfone solution; then zirconium dioxide was added and stirred for another 4 hours to obtain a milky white coating slurry solution;

[0069] Then, the coating slurry solution prepared in the above manner is injected into both sides of the grid support carrier between the two scrapers by a pump, so that the slurry solution fully infiltrates the grid support carrier, and is coated on the surfaces of both sides of the grid support carrier under the downward traction of the roller, so as to obtain an uncured composite diaphragm with the slurry evenly coated on both sides;

[0070] Then, the uncured composite membrane is pulled into the area between the bottom of the scraper and the surface of the primary coagulation bath by a roller, and the uncured composite membrane undergoes phase transformation under the action of the anti-solvent spray droplets atomized by the atomizers on both sides to form a pre-cured surface. Figure 2 As shown, the anti-solvent spray component used in this embodiment is a 90% NMP aqueous solution; in the water mist droplets formed by the atomizer, the water mist droplets with a particle size of 1-5μm need to account for 60%-100% of the total water mist droplets, the atomization temperature is 25°C, the spray rate is 5ml / min, the accumulation degree of droplet particles on the surface of the diaphragm is affected by the spray rate and the roller traction rate, and the roller traction rate can determine the time the diaphragm surface is exposed to the spray, and this time is set to 30s, and then the pre-cured diaphragm is pulled into the primary coagulation bath under the traction of the roller, and a full phase conversion is carried out for 5min. The primary coagulation bath is pure water with a temperature of 25°C; it is continued to be pulled into the secondary coagulation bath for rinsing for 5min to completely remove the excess solvent. The secondary coagulation bath is pure water at 25°C;

[0071] Finally, the rinsed and fully cured diaphragm is rolled up to obtain a finished film, i.e., a composite diaphragm.

[0072] The surface and cross-sectional scanning electron microscopy images of the prepared composite diaphragm are shown in Figure 2. Figure 8 As shown, this embodiment uses 90% NMP aqueous solution as the anti-solvent spray component, and the spray rate is set to 5ml / min, so that an appropriate amount of atomized droplets fall on the surface of the wet membrane to undergo phase transformation. Since the spray component is 90% NMP aqueous solution, the water content in the spray droplets attached to the surface of the wet membrane is further reduced, and a slower phase transformation is carried out in an excessive organic solvent environment, so that replacement pores with larger pore sizes are formed on the surface, which will greatly reduce the air tightness of the membrane (bubble point pressure = 0.85bar). In addition, the thickness of the surface solidification layer is as deep as 10μm, which greatly reduces the phase transformation rate of the pre-cured wet membrane in the next step of the primary coagulation bath, thereby forming a relatively dense three-dimensional sponge-like pore inside. Although the mechanical strength of the membrane is increased, the ion transmission capacity in the electrolyte solution is greatly reduced, resulting in an increase in the membrane surface resistance.

[0073] Example 6

[0074] First, polysulfone resin was dissolved in N-methylpyrrolidone (NMP) and stirred for 4 hours to obtain a uniformly dispersed NMP-polysulfone solution; then zirconium dioxide was added and stirred for another 4 hours to obtain a milky white coating slurry solution;

[0075] Then, the coating slurry solution prepared in the above manner is injected into both sides of the grid support carrier between the two scrapers by a pump, so that the slurry solution fully infiltrates the grid support carrier, and is coated on the surfaces of both sides of the grid support carrier under the downward traction of the roller, so as to obtain an uncured composite diaphragm with the slurry evenly coated on both sides;

[0076] Then, the uncured composite membrane is pulled into the area between the bottom of the scraper and the surface of the primary coagulation bath by a roller, and the uncured composite membrane undergoes phase transformation under the action of the anti-solvent spray droplets atomized by the atomizers on both sides to form a pre-cured surface. Figure 2 As shown, the anti-solvent spray component used in this embodiment is a 50% isopropanol aqueous solution; in the water mist droplets formed by the atomizer, the water mist droplets with a particle size of 1-5μm need to account for 60%-100% of the total water mist droplets, the atomization temperature is 25°C, the spray rate is 5ml / min, the accumulation degree of droplet particles on the surface of the diaphragm is affected by the spray rate and the roller traction rate, and the roller traction rate can determine the time the diaphragm surface is exposed to the spray, and this time is set to 30s, and then the pre-cured diaphragm is pulled into the primary coagulation bath under the traction of the roller, and a full phase conversion is carried out for 5min. The primary coagulation bath is pure water with a temperature of 25°C; it is continued to be pulled into the secondary coagulation bath for rinsing for 5min to completely remove the excess solvent. The secondary coagulation bath is pure water at 25°C;

[0077] Finally, the rinsed and fully cured diaphragm is rolled up to obtain a finished film, i.e., a composite diaphragm.

[0078] The surface and cross-sectional scanning electron microscope images of the prepared composite diaphragm are shown in the attached manual. Fig. 9 As shown, this embodiment uses 50% isopropanol aqueous solution as the anti-solvent spray component, and the spray rate is set to 5ml / min, so that an appropriate amount of atomized liquid drops on the surface of the wet diaphragm to form a uniform surface microporous structure while undergoing phase transformation, and the thickness of the surface solidified layer is preferably 4μm, so that the phase transformation rate of the pre-cured wet diaphragm in the primary coagulation bath is slowed down, so that a relatively loose three-dimensional sponge-like pore can be formed inside the diaphragm. This structure not only ensures the porosity of the diaphragm, but also has a certain mechanical strength, and the surface pores of appropriate size (pore size ≤ 50nm) and uniform distribution are conducive to the uniform and rapid migration of ions in the diaphragm during the working process of the electrolytic cell, and can also maintain a high air tightness (bubble point pressure = 5.92bar). In addition, the effect of using ethanol aqueous solution as the anti-solvent spray component is similar to that of isopropanol aqueous solution, and both can change the surface and internal structure of the diaphragm.

[0079] The comparison of the parameters of the diaphragms prepared in the above examples and the results of the related tests is shown in Table 1:

[0080] Table 1 Comparison of relevant test parameters of composite diaphragms prepared in Example

[0081]

[0082] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.

Claims

1. A method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration, characterized in that: The grid support carrier is pulled by a roller, and a scraper, an atomizer, a primary coagulation bath and a secondary coagulation bath are sequentially arranged along the pulling direction, including the following steps: A. Inject the coating slurry solution into both sides of the grid support carrier between the two scrapers through a pump, so that the slurry solution fully infiltrates the grid support carrier, and obtain an uncured wet diaphragm with the slurry solution evenly coated on both sides under the downward traction of the roller; B. The uncured wet diaphragm is pulled by the roller and moves to the area between the bottom of the scraper and the surface of the primary coagulation bath. The atomizers on both sides of the uncured wet diaphragm spray to form anti-solvent spray droplets, which undergo local phase transformation under the action of the anti-solvent spray droplets to form a pre-cured diaphragm; Among them, in the anti-solvent spray droplets, the spray droplets with a particle size of 1-5 μm need to account for 60%-100% of the spray droplets, the temperature is 20-60°C, the spray rate is 1-10 ml / min, the membrane surface is exposed to the spray for 5-60 seconds, and the thickness formed by the spray on both sides of the uncured membrane is 5-70 μm; C. Then the pre-cured diaphragm enters the primary coagulation bath under the traction of the roller, undergoes a full phase conversion, and obtains a fully cured diaphragm; The full phase inversion time is 2-30min, and the primary coagulation bath temperature is 5-90°C; D. The fully solidified membrane is pulled into the secondary coagulation bath under the traction of rollers for rinsing; The rinsing time is 2-30min, and the secondary coagulation bath temperature is 5-90°C; E. Finally, the rinsed and fully cured diaphragm is rolled up to obtain a finished film.

2. The method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration according to claim 1, characterized in that: In step A, the slurry solution is composed of an alkali-resistant polymer solution and inorganic nanoparticles.

3. The method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration according to claim 1, characterized in that: In the atomizer anti-solvent spray droplets described in step B, the percentage of anti-solvent spray droplets with a particle size range of 1-5 μm in the total droplet amount is 80%-100%, and the spray temperature of the atomizer is preferably 25°C.

4. The method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration according to claim 1, characterized in that: The spray rate of the atomizer in step B is preferably 5 ml / min, the atomization time is preferably 30 s, and the thickness formed by the spray on both sides of the uncured wet diaphragm is 3-5 μm.

5. The method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration according to claim 1, characterized in that: The atomizer anti-solvent spray in step B is one or more of nitrogen methyl pyrrolidone aqueous solution, pure water, ethanol aqueous solution, and isopropanol aqueous solution, wherein the concentration of nitrogen methyl pyrrolidone aqueous solution is 10%-90%, preferably 40%-50%; the concentration of ethanol aqueous solution is 40%-100%, preferably 50%-60%; the concentration of isopropanol aqueous solution is 40%-100%, preferably 50%-60%.

6. The method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration according to claim 1, characterized in that: The primary coagulation bath described in step C is composed of pure water, the time is preferably 5 minutes, the temperature is preferably 20°C-40°C, more preferably 25°C.

7. The method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration according to claim 1, characterized in that: The secondary coagulation bath described in step D is composed of pure water, the time is preferably 5 minutes, the temperature is preferably 20°C-40°C, more preferably 25°C.

8. The method for preparing a reinforced composite diaphragm by spray pre-solidification continuous integration according to claim 1, characterized in that: The material of the grid support carrier is PPS.

Citation Information

Patent Citations

  • Process for producing an ion-permeable web-reinforced separator

    WO2009147084A1

  • Apparatus and process for producing an ion-permeable web-reinforced separator and separator obtainable therewith

    WO2009147086A1

Cited By

  • Aromatic polyamide porous membrane as well as preparation method and application thereof

    CN119971801A

  • Aromatic polyamide porous membrane, method for producing the same, and use thereof

    CN119971801B

  • Temperature control system and method for preparing polyacrylonitrile-based carbon film

    CN121277261A

  • A temperature control system and method for the production of polyacrylonitrile-based carbon films

    CN121277261B