Preparation method of heat conduction and radiation composite shielding multilayer structure thermal protection coating material
The multi-layer structure thermal protection coating with reflective layer, absorbing layer and low thermal conductivity layer was prepared by spraying method, which solved the problem of thermal radiation penetration at high temperatures, achieved efficient thermal protection effect and low thermal conductivity, and was suitable for thermal protection in high temperature environments. need.
Patent Information
- Application Number
- CN202411137576.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing thermal protection coating technology has failed to effectively solve the impact of thermal radiation penetration on the substrate at high temperatures, resulting in thermal damage to the hot end components at extreme temperatures. The low thermal conductivity alone is not enough to meet the thermal protection needs of high-temperature environments.
The multi-layer structure thermal protection coating with reflective layer/absorbing layer/low-thermal conductivity layer was prepared by spraying method. The high-reflection layer was used to realize the full-band reflection of high-temperature thermal radiation in the 0.5-10μm band, and the high-absorbing layer was at wavelength and reflective layer wavelength. Interleaved with complementary reflection and absorption, low thermal conductivity hinders phonon heat transfer and reduces overall thermal conductivity.
It realizes the reduction of thermal radiation penetration at high temperatures and reduces thermal shock while maintaining low thermal conductivity and high temperature thermal stability, moderate cost and simple processes are suitable for large-scale production.
Smart Images

Figure CN119016314A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of high-temperature thermal protection and radiation thermal control, and specifically relates to a method for preparing a multi-layered thermal protection coating material with heat conduction and radiation composite shielding. Background Art
[0002] With the development of high-temperature combustion technology, the high-temperature requirements of hot-end components are constantly increasing. The research on thermal protection coatings with low thermal conductivity has always been the focus of domestic and foreign scholars. So far, for the research and development of thermal protection coatings, scholars have paid more attention to the low thermal conductivity of coating materials, but have not focused on the impact of radiation penetration on the substrate at high temperatures. At present, the extreme temperature of hot-end components can reach more than 1500℃. According to Planck's blackbody radiation law, the thermal radiation energy is mainly distributed in the wavelength range of 0.5-10μm, and as the temperature rises, the thermal radiation energy will be concentrated in the shorter wavelength range. Short-wavelength electromagnetic waves are usually less scattered and absorbed, and have stronger penetration ability. Under extreme temperatures, the thermal shock caused by high-temperature thermal radiation penetration is also one of the main causes of thermal damage to hot-end components. Therefore, thermal protection coatings with only low thermal conductivity can no longer meet the thermal protection needs of hot-end components at this stage and in the future. It is extremely important to study a thermal protection coating with thermal conductive radiation composite shielding for multiple high-temperature environments.
[0003] On March 28, 2023, China Patent (CN115849958A) disclosed a thermal protective coating of a ceramic-based composite material, its preparation method and application. The coating uses a ceramic-based material as a substrate, Yb2O3 and CaO co-doped HfO2 as a thermal insulation layer material, and an atmospheric plasma spraying method is used to prepare a multilayer composite thermal protective coating with a sealing layer, an anti-oxidation bonding layer, and a thermal insulation and refractory layer structure. The coating is characterized by improving the temperature resistance of the coating, but does not consider the influence of high-temperature (above 1000°C) thermal radiation penetration. On December 30, 2022, China Patent (CN115537812A) disclosed a high-temperature anti-oxidation coating for thermal protection of composite materials. The coating uses SiC / C as a matrix, silicon carbide, iridium boride, metallic iridium, and hafnium boride as materials to form a multi-layer alternating thermal protective coating for high-temperature oxidation resistance. The coating does not consider the influence of high-temperature (above 1000°C) thermal radiation penetration. On February 15, 2022, a Chinese patent (CN114045456A) disclosed a high-temperature resistant composite coating containing rare earth aluminates and a preparation method. A composite coating with an oxide film layer, a metal bonding layer, and a rare earth aluminate ceramic layer structure was prepared by atmospheric plasma spraying. Although the coating can withstand a high temperature of 1800°C, the influence of thermal radiation penetration is not considered. In summary, the multi-layer thermal protection coating proposed by scholars ignores the combined effects of thermal radiation penetration and heat conduction. Based on this, the research and development of thermal conductive radiation composite shielding coatings is extremely important. Summary of the invention
[0004] The purpose of the present invention is to solve the problem that the existing thermal protection coating technology cannot meet the requirements of thermal conductivity and radiation penetration composite shielding, and to provide a method for preparing a multi-layer thermal protection coating material with thermal conductivity and radiation composite shielding.
[0005] The present invention solves the shortcomings of current research on thermal protective coatings and the urgent needs in the field of thermal protection, and proposes a method for preparing a thermally conductive radiation composite shielding thermal protective coating with a reflective layer / absorption layer / low thermal conductivity layer structure (i.e., a multi-layer structure thermal protective coating material with thermal conductivity and radiation composite shielding).
[0006] A method for preparing a multi-layer structure thermal protection coating material with heat conduction and radiation composite shielding is specifically completed in the following steps:
[0007] 1. Substrate surface pretreatment:
[0008] Removing dust, grease and impurities from the surface of the substrate, and then activating the surface of the substrate to obtain a pretreated substrate;
[0009] 2. Preparation of low thermal conductivity layer:
[0010] A thermal insulation layer with low thermal conductivity is prepared on the surface of the substrate by a spraying method;
[0011] The thermal conductivity of the thermal insulation layer with low thermal conductivity described in step 2 is less than 2 W / (m·K);
[0012] The functional component of the heat insulation layer in step 2 is one or a combination of ZrO2, Si3N4 and rare earth acid ceramics;
[0013] 3. Preparation of high absorption layer:
[0014] A middle layer with high infrared absorption is prepared on the thermal insulation layer by spraying;
[0015] The functional component of the intermediate layer with high infrared absorption in step 3 has high infrared absorption in the 0.5 μm to 10 μm band and is one or a combination of transition metal oxides, carbon-based materials and narrow bandgap semiconductor materials;
[0016] 4. Preparation of high reflective layer:
[0017] A high-reflection layer is prepared on the middle layer with high infrared absorption by spraying, and a multi-layer structure thermal protection coating material with heat conduction and radiation composite shielding is finally obtained after polishing.
[0018] The functional component of the high reflective layer described in step 4 has high infrared reflectivity in the 0.5 μm to 10 μm band and is any one of metal oxides, two-dimensional materials and noble metals;
[0019] The effective thermal conductivity of the multi-layer thermal protective coating material with thermal conductivity and radiation composite shielding described in step 4 is less than 1W / (m·K), the infrared transmittance in the 0.5μm to 10μm band is less than 0.12, and the infrared reflectivity is greater than 0.4.
[0020] Principle of the present invention:
[0021] The present invention prepares a high-reflection / high-absorption / low-thermal-conductivity multilayer structure of a thermal radiation composite shielding coating (i.e., a multilayer structure thermal protection coating material with thermal conductivity and radiation composite shielding) by a spraying method; the multilayer structure has low thermal conductivity and is resistant to radiation penetration, thereby realizing composite shielding of thermal radiation; the first high-reflection layer (outermost layer) uses a material with a large complex refractive index modulus to realize full-band reflection of high-temperature thermal radiation; the second layer (middle layer) is a high-absorption layer, and the material used is required to have a high absorption coefficient. At the same time, it is necessary to try to meet the high absorption coefficient wavelength and the high refractive index wavelength of the reflection layer to interlace with each other, so that the reflection band and the absorption band have good complementarity, which is more conducive to thermal radiation shielding; the third layer is a low-thermal-conductivity layer (innermost layer), and the material used has low thermal conductivity and is required to have high thermal stability and low thermal expansion coefficient. Based on the first and second layers, photon heat transfer is hindered, and based on the third layer, phonon heat transfer is hindered. According to the blackbody radiation law, at high temperatures (above 1000°C), the radiation energy is mainly distributed in the 0.5-10μm band. The thermal protection coating reduces the transmittance in this band, thereby reducing the thermal shock of radiation on the substrate. At the same time, the overall thermal conductivity of the coating is reduced through the low thermal conductivity layer. The composite structure makes the overall thermal conductivity of the coating less than 1W / (m·K).
[0022] Advantages of the present invention:
[0023] 1. The present invention proposes a method for preparing a multi-layer structure thermal protection coating material with heat conduction and radiation composite shielding. Compared with the existing multi-layer composite structure thermal protection coating, the multi-layer structure coating reduces the penetration of thermal radiation and the direct impact of thermal radiation on the substrate, and at the same time has lower thermal conductivity and high temperature thermal stability;
[0024] 2. The material used for the thermal protection coating proposed in the present invention is moderately priced, and the preparation process is simple. It can be prepared by spraying, and the process parameters are adjustable, which is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a schematic diagram of a multi-layer structure thermal protection coating material with heat conduction and radiation composite shielding according to the present invention, in which 1 is a substrate, 2 is a low thermal conductivity layer, 3 is a high absorption layer, and 4 is a high reflection layer;
[0026] Figure 2This is a cross-sectional morphology image of the TiO2 / Fe2O3 / ZrO2 thermal conductive and radiation composite shielding multilayer structure thermal protection coating material prepared in Example 1, obtained by SEM electron microscope scanning;
[0027] Figure 3 The infrared reflectivity spectrum and infrared transmittance spectrum are shown in FIG. (a) is the infrared reflectivity spectrum of the TiO2 / Fe2O3 / ZrO2 thermal conductive and radiation composite shielding multilayer structure thermal protective coating material prepared in Example 1; (b) is the infrared transmittance spectrum of the TiO2 / Fe2O3 / ZrO2 thermal conductive and radiation composite shielding multilayer structure thermal protective coating material prepared in Example 1;
[0028] Figure 4 The infrared transmittance spectrum of the TiO2 / ZrO2 double-layer thermal protection coating prepared in Comparative Example 1;
[0029] Figure 5 The infrared transmittance spectrum of the Fe2O3 / ZrO2 double-layer thermal protection coating prepared in Comparative Example 2;
[0030] Figure 6 The infrared transmittance spectrum of the ZrO2 single-layer thermal protection coating prepared in Comparative Example 3. DETAILED DESCRIPTION
[0031] Specific implementation method 1: This implementation method is a method for preparing a multi-layer structure thermal protection coating material with heat conduction and radiation composite shielding, which is specifically completed according to the following steps:
[0032] 1. Substrate surface pretreatment:
[0033] Removing dust, grease and impurities from the surface of the substrate, and then activating the surface of the substrate to obtain a pretreated substrate;
[0034] 2. Preparation of low thermal conductivity layer:
[0035] A thermal insulation layer with low thermal conductivity is prepared on the surface of the substrate by a spraying method;
[0036] The thermal conductivity of the thermal insulation layer with low thermal conductivity described in step 2 is less than 2 W / (m·K);
[0037] The functional component of the heat insulation layer in step 2 is one or a combination of ZrO2, Si3N4 and rare earth acid ceramics;
[0038] 3. Preparation of high absorption layer:
[0039] A middle layer with high infrared absorption is prepared on the thermal insulation layer by spraying;
[0040] The functional component of the intermediate layer with high infrared absorption in step 3 has high infrared absorption in the 0.5 μm to 10 μm band and is one or a combination of transition metal oxides, carbon-based materials and narrow bandgap semiconductor materials;
[0041] 4. Preparation of high reflective layer:
[0042] A high-reflection layer is prepared on the middle layer with high infrared absorption by spraying, and a multi-layer structure thermal protection coating material with heat conduction and radiation composite shielding is finally obtained after polishing.
[0043] The functional component of the high reflective layer described in step 4 has high infrared reflectivity in the 0.5 μm to 10 μm band and is any one of metal oxides, two-dimensional materials and noble metals;
[0044] The effective thermal conductivity of the multi-layer thermal protective coating material with thermal conductivity and radiation composite shielding described in step 4 is less than 1W / (m·K), the infrared transmittance in the 0.5μm to 10μm band is less than 0.12, and the infrared reflectivity is greater than 0.4.
[0045] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that: the substrate described in step 1 is any one of a metal-based material and a ceramic-based composite material; the metal-based material is carbon steel, aluminum alloy, titanium alloy or nickel-based alloy; the ceramic-based composite material is C / C, C / SiC, SiC / SiC; in step 1, water, methanol, ethanol, ammonia water, potassium hydroxide solution, nitric acid or hydrochloric acid is used to clean the substrate to remove dust, grease and impurities on the surface of the substrate. The other steps are the same as those in specific implementation method 1.
[0046] Specific implementation method three: This implementation method is different from specific implementation method one or two in that the mass fraction of the ammonia water is 1% to 5%, the mass fraction of the potassium hydroxide solution is 5% to 10%, the mass fraction of nitric acid is 10% to 30%, and the mass fraction of hydrochloric acid is 10% to 20%. The other steps are the same as those of specific implementation method one or two.
[0047] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: in step 1, a mechanical sandblasting process is used to activate the surface of the substrate; the sandblasting material selected for the mechanical sandblasting process is silica sand, quartz sand or ceramic beads, the sandblasting pressure is 0.2MPa to 0.6MPa, the sandblasting distance is 100mm to 300mm, and the sandblasting angle is 45 to 90°. The other steps are the same as those of specific embodiments 1 to 3.
[0048] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the rare earth acid salt ceramic described in step 2 is type, type, A is one or a combination of Sc, Yb, Lu, Er, Tm, Dy, Ho, La, Y, Gd, Ti, Sm, Nd and Eu; B is Zr, Ce or Hf; C is Ta or Nb. The other steps are the same as those in the first to fourth embodiments.
[0049] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: the powder particle size of the functional component of the heat insulation layer described in step 2 is 1 μm to 10 μm; the thickness of the heat insulation layer with low thermal conductivity on the substrate in step 2 is 0.01 mm to 1 mm, the density is greater than 70%, and the thermal conductivity is less than 2 W / mK. The other steps are the same as specific embodiments 1 to 5.
[0050] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the transition metal oxide described in step 3 is Fe3O4, Fe2O3, CuO, MnO2, Co2O3 or ZnO; the carbon-based material is nanocarbon black or graphene; the narrow bandgap semiconductor material is cadmium selenide or bismuth selenide. The other steps are the same as specific embodiments 1 to 6.
[0051] Specific embodiment 8: The difference between this embodiment and specific embodiments 1 to 7 is that the thickness of the intermediate layer with high infrared absorption in step 3 is 0.01 mm to 2 mm, the density is greater than 60%, and the absorption coefficient is greater than 10000 cm -1 The other steps are the same as those in Specific Embodiments 1 to 7.
[0052] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: the metal oxide described in step 4 is TiO2 or Al2O3; the two-dimensional material is BN, indium selenide or transition metal disulfide; the noble metal is Pt or Pt alloy; the thickness of the high reflective layer described in step 4 is 0.01 mm to 1 mm, the density is greater than 60%, and the complex refractive index modulus is greater than 2. The other steps are the same as specific embodiments 1 to 8.
[0053] Specific embodiment 10: The difference between this embodiment and specific embodiments 1 to 9 is that the specific method of polishing described in step 4 is: remove the debris and dirt on the surface of the metallographic grinding and polishing machine worktable, install the 300-mesh grinding sheet on the turntable for rough grinding, adjust the parameters of the metallographic grinding machine, set the speed to 300r / min, and the grinding time is 3min; replace the 800-mesh grinding sheet for fine grinding, adjust the parameters of the metallographic grinding machine, set the speed to 600r / min, and the grinding time is 2min. The average roughness Ra of the coating surface is less than 2μm; the spraying method described in steps 2, 3, and 4 is: thermal spraying or slurry spraying; the binder in the slurry spraying is one or a combination of potassium silicate, aluminum silicate, silica sol and aluminum phosphate. The other steps are the same as specific embodiments 1 to 9.
[0054] The following examples are used to verify the beneficial effects of the present invention:
[0055] Example 1: A method for preparing a TiO2 / Fe2O3 / ZrO2 thermal conductive and radiation composite shielding multilayer thermal protective coating material is specifically completed in the following steps:
[0056] 1. Substrate surface pretreatment:
[0057] Using anhydrous ethanol as solvent, dust, grease and impurities on the surface of the substrate are removed, and then the surface of the substrate is activated to obtain a pretreated substrate;
[0058] The substrate described in step 1 is an aluminum alloy with a thickness of 3 mm and a model of 6061;
[0059] In step 1, a mechanical sandblasting process is used to activate the surface of the substrate; the sandblasting material selected for the mechanical sandblasting process is quartz sand, the sandblasting pressure is 0.2MPa, the sandblasting distance is 100mm, and the sandblasting angle is 45°;
[0060] 2. Preparation of low thermal conductivity layer:
[0061] The ceramic powder with low thermal conductivity is fully mixed with a binder to obtain a mixed powder; the mixed powder is sprayed onto the pretreated substrate surface by a slurry spraying method, and the coating thickness can be controlled by the spraying time; the prepared coating is dried at room temperature (25°C) for 5 hours, and then cured at 240°C for 1 hour to obtain a substrate covered with a ceramic bottom layer with low thermal conductivity;
[0062] The ceramic powder with low thermal conductivity described in step 2 is ZrO2, and the particle size is 2 μm;
[0063] The binder described in step 2 is sodium silicate;
[0064] The mass ratio of the ceramic powder with low thermal conductivity to the binder described in step 2 is 3:2;
[0065] The process parameters of the slurry spraying method described in step 2 are: air pressure 2MPa, spraying distance 300mm, spraying time 15s;
[0066] In step 2, the thickness of the ceramic bottom layer with low thermal conductivity on the substrate is 0.25 mm and the density is 77%;
[0067] 3. Preparation of high absorption layer:
[0068] The powder with high infrared absorption is fully mixed with a binder to obtain a mixed powder; the mixed powder is sprayed onto the surface of a substrate covered with a ceramic bottom layer with low thermal conductivity by a slurry spraying method, and the coating thickness can be controlled by the spraying time; the prepared coating is dried at room temperature (25°C) for 5 hours, and then cured at 240°C for 1 hour to obtain a substrate covered with an intermediate layer with high infrared absorption;
[0069] The powder with high infrared absorption described in step 3 is Fe2O3;
[0070] The binder described in step 3 is sodium silicate;
[0071] The mass ratio of the powder with high infrared absorption to the binder described in step 3 is 3:2;
[0072] The process parameters of the slurry spraying method in step 3 are: air pressure 2MPa, spraying distance 300mm, and spraying time 50s;
[0073] The thickness of the intermediate layer with high infrared absorption in step 3 is 0.95 mm, the density is 71%, and the absorption coefficient is 46895 cm -1 ;
[0074] 4. Preparation of high reflective layer:
[0075] The powder with high reflection is fully mixed with the binder to obtain the mixed powder; the mixed powder is sprayed onto the surface of the substrate covered with the intermediate layer with high infrared absorption by a slurry spraying method, and the coating thickness can be controlled by the spraying time; the prepared coating is dried at room temperature (25°C) for 5 hours, then cured at 240°C for 1 hour, and then polished to obtain a substrate covered with a high reflection layer, that is, a TiO2 / Fe2O3 / ZrO2 thermal conductive and radiation composite shielding multilayer structure thermal protective coating material;
[0076] The highly reflective powder described in step 4 is TiO2;
[0077] The binder described in step 4 is sodium silicate;
[0078] The mass ratio of the highly reflective powder to the binder described in step 4 is 3:2;
[0079] The process parameters of the slurry spraying method described in step 4 are: air pressure 2MPa, spraying distance 300mm, spraying time 25s;
[0080] The specific method of the polishing treatment described in step 4 is: remove the debris and dirt on the surface of the metallographic grinding and polishing machine workbench, install a 300-mesh grinding sheet on the turntable for rough grinding, adjust the parameters of the metallographic grinding machine, set the speed to 300r / min, and the grinding time to 3min; replace the 800-mesh grinding sheet for fine grinding, adjust the parameters of the metallographic grinding machine, set the speed to 600r / min, and the grinding time to 2min;
[0081] The thickness of the high reflective layer in the TiO2 / Fe2O3 / ZrO2 thermal conductive and radiation composite shielding multilayer thermal protective coating described in step 4 is 0.3 mm, and the density is 73%; the average surface roughness of the coating is 0.8 μm, and the complex refractive index modulus is 2.31.
[0082] The optical properties of the TiO2 / Fe2O3 / ZrO2 thermal conductive, radiation composite shielding multilayer structure thermal protective coating material prepared in Example 1 were tested using a Fourier spectrometer, and the results showed that the transmittance of the coating in the 0.5-10 μm band was 0.044 and the reflectivity was 0.48.
[0083] The thermal conductivity of the TiO2 / Fe2O3 / ZrO2 thermal conductive, radiation composite shielding multilayer structure thermal protective coating material prepared in Example 1 was measured using a laser thermal conductivity meter, and the thermal conductivity of the coating at high temperature (1000°C) was measured to be 0.95 W / (m·K).
[0084] Example 2: A method for preparing a multilayer structure thermal protective coating material with Al2O3 / ZnO / Y3NbO7 heat conduction and radiation composite shielding is specifically completed in the following steps:
[0085] 1. Substrate surface pretreatment:
[0086] Using anhydrous ethanol as solvent, dust, grease and impurities on the surface of the substrate are removed, and then the surface of the substrate is activated to obtain a pretreated substrate;
[0087] The substrate described in step 1 is a nickel-based alloy with a thickness of 3 mm, and the nickel-based alloy model is GH4169;
[0088] In step 1, a mechanical sandblasting process is used to activate the surface of the substrate; the sandblasting material selected for the mechanical sandblasting process is silica sand, the sandblasting pressure is 0.3 MPa, the sandblasting distance is 120 mm, and the sandblasting angle is 45°;
[0089] 2. Preparation of low thermal conductivity layer:
[0090] The powder is sprayed onto the pretreated substrate surface by thermal spraying to obtain a substrate covered with a ceramic bottom layer having low thermal conductivity;
[0091] The ceramic powder with low thermal conductivity described in step 2 is Y3NbO7, with a particle size of 1.5 μm, and the preparation method is as follows: weigh a certain amount of Y2O3 and Nb2O5 in proportion and put them into a ball mill, add zirconium oxide grinding balls, the ball-to-material ratio is 3:1, add an appropriate amount of anhydrous ethanol, and ball mill for 24 hours with the speed set to 200 r / min; put the ball-milled powder into a drying oven, set the temperature to 90°C, and keep it warm for 6 hours; after the powder is sieved through 200 mesh, put it into a box furnace, and calcine at 1600°C for 8 hours to obtain Y3NbO7; the mass ratio of Y2O3 to Nb2O5 is 2.55:1;
[0092] The thermal spraying method described in step 2 is atmospheric plasma spraying, and the process parameters are: argon is used as the main gas, hydrogen is used as the auxiliary gas, the main gas flow rate is 40NLPM, the auxiliary gas flow rate is 10NLPM, the carrier gas flow rate is 3NLPM, the plasma spray gun power is 42.5kw, the powder feeder speed is 25rpm, and the nozzle distance is 100mm;
[0093] In step 2, the thickness of the ceramic bottom layer with low thermal conductivity on the substrate is 0.25 mm and the density is 85%;
[0094] 3. Preparation of high absorption layer:
[0095] The powder with high infrared absorption is fully mixed with the binder to obtain a mixed powder; the mixed powder is sprayed onto the surface of the substrate covered with a ceramic bottom layer with low thermal conductivity by a slurry spraying method, and the coating thickness can be controlled by the spraying time. The prepared coating is dried at room temperature (25°C) for 5 hours, and then cured at 240°C for 1 hour to obtain a substrate covered with an intermediate layer with high infrared absorption;
[0096] The powder with high infrared absorption described in step 3 is ZnO;
[0097] The binder described in step 3 is sodium silicate;
[0098] The mass ratio of the powder with high infrared absorption to the binder described in step 3 is 3:2;
[0099] The process parameters of the slurry spraying method in step 3 are: air pressure 2MPa, spraying distance 300mm, spraying time 65s;
[0100] The thickness of the intermediate layer with high infrared absorption in step 3 is 0.95 mm, the density is 78%, and the absorption coefficient is 9896.5 cm-1 ;
[0101] 4. Preparation of high reflective layer:
[0102] The powder with high reflection is fully mixed with the binder to obtain the mixed powder; the mixed powder is sprayed onto the surface of the substrate covered with the intermediate layer with high infrared absorption by the slurry spraying method, and the coating thickness can be controlled by the spraying time. The prepared coating is dried at room temperature (25°C) for 5 hours, then cured at 240°C for 1 hour, and then polished to obtain a substrate covered with a high reflection layer, that is, Al2O3 / ZnO / Y3NbO7 thermal conductive and radiation composite shielding multilayer structure thermal protection coating material;
[0103] The highly reflective powder described in step 4 is Al2O3;
[0104] The binder described in step 4 is sodium silicate;
[0105] The mass ratio of the highly reflective powder to the binder described in step 4 is 3:2;
[0106] The process parameters of the slurry spraying method described in step 4 are: air pressure 2MPa, spraying distance 300mm, spraying time 20s;
[0107] The specific method of the polishing treatment described in step 4 is: remove the debris and dirt on the surface of the metallographic grinding and polishing machine workbench, install a 300-mesh grinding sheet on the turntable for rough grinding, adjust the parameters of the metallographic grinding machine, set the speed to 300r / min, and the grinding time to 3min; replace the 800-mesh grinding sheet for fine grinding, adjust the parameters of the metallographic grinding machine, set the speed to 600r / min, and the grinding time to 2min;
[0108] The thickness of the high reflective layer in the Al2O3 / ZnO / Y3NbO7 thermal conductive and radiation composite shielding multilayer thermal protective coating described in step 4 is 0.3 mm, and the density is 74%; the average surface roughness of the coating is 0.5 μm, and the complex refractive index modulus is 2.07.
[0109] The optical properties of the Al2O3 / ZnO / Y3NbO7 thermal conductive, radiation composite shielding multilayer structure thermal protective coating material prepared in Example 2 were tested using a Fourier spectrometer, and the results showed that the transmittance of the coating in the 0.5-10 μm band was 0.089 and the reflectivity was 0.45.
[0110] The thermal conductivity of the Al2O3 / ZnO / Y3NbO7 thermal conductive, radiation composite shielding multilayer structure thermal protective coating material prepared in Example 2 was measured using a laser thermal conductivity meter, and the thermal conductivity of the coating at high temperature (1000°C) was measured to be 0.89W / (m·K).
[0111] Comparative Example 1: The TiO2 / ZrO2 double-layer structure thermal protection coating is prepared by the following steps:
[0112] 1. Substrate surface pretreatment:
[0113] Using anhydrous ethanol as solvent, dust, grease and impurities on the surface of the substrate are removed, and then the surface of the substrate is activated to obtain a pretreated substrate;
[0114] The substrate described in step 1 is an aluminum alloy with a thickness of 3 mm, and the aluminum alloy model is 6061;
[0115] In step 1, a mechanical sandblasting process is used to activate the surface of the substrate; the sandblasting material selected for the mechanical sandblasting process is quartz sand, the sandblasting pressure is 0.2MPa, the sandblasting distance is 100mm, and the sandblasting angle is 45°;
[0116] 2. Preparation of low thermal conductivity layer:
[0117] The powder is sprayed onto the pretreated substrate surface by thermal spraying to obtain a substrate covered with a ceramic bottom layer having low thermal conductivity;
[0118] The ceramic powder with low thermal conductivity described in step 2 is ZrO2, and the particle size is 2 μm;
[0119] The thermal spraying method described in step 2 is atmospheric plasma spraying, and the process parameters are: argon is used as the main gas, hydrogen is used as the auxiliary gas, the main gas flow rate is 40NLPM, the auxiliary gas flow rate is 10NLPM, the carrier gas flow rate is 3NLPM, the plasma spray gun power is 42.5kw, the powder feeder speed is 25rpm, and the nozzle distance is 100mm; the thickness of the ceramic bottom layer with low thermal conductivity on the substrate in step 2 is 0.8mm, and the density is 87%;
[0120] 3. Preparation of high reflective layer:
[0121] The powder with high reflection is fully mixed with the binder to obtain the mixed powder; the mixed powder is sprayed onto the surface of the substrate covered with the ceramic bottom layer with low thermal conductivity by the slurry spraying method, and the coating thickness can be controlled by the spraying time; the prepared coating is dried at room temperature (25°C) for 5 hours, then cured at 240°C for 1 hour, and then polished to obtain the substrate covered with the high reflection layer, that is, the TiO2 / ZrO2 double-layer structure thermal protection coating;
[0122] The highly reflective powder described in step 3 is TiO2;
[0123] The binder described in step 3 is sodium silicate;
[0124] The mass ratio of the highly reflective powder to the binder described in step 3 is 3:2;
[0125] The process parameters of the slurry spraying method described in step 3 are: air pressure 2MPa, spraying distance 300mm, spraying time 40s;
[0126] The specific method of the polishing treatment described in step 3 is: remove the debris and dirt on the surface of the metallographic grinding and polishing machine workbench, install a 300-mesh grinding sheet on the turntable for rough grinding, adjust the metallographic grinding machine parameters, set the speed to 300r / min, and the grinding time to 3min; replace the 800-mesh grinding sheet for fine grinding, adjust the metallographic grinding machine parameters, set the speed to 600r / min, and the grinding time to 2min;
[0127] The thickness of the high reflective layer in the TiO2 / ZrO2 double-layer thermal protection coating described in step three is 0.7 mm, and the density is 79%; the average roughness of the coating surface is 0.5 μm, and the complex refractive index modulus is 2.31.
[0128] The optical properties of the TiO2 / ZrO2 double-layer thermal protection coating prepared in Comparative Example 1 were tested using a Fourier spectrometer, and the results showed that the transmittance of the coating in the 0.5-10 μm band was 0.27 and the reflectivity was 0.45.
[0129] The thermal conductivity of the TiO2 / ZrO2 double-layer thermal protection coating prepared in Comparative Example 1 was measured using a laser thermal conductivity meter, and the thermal conductivity of the coating at high temperature (1000°C) was measured to be 1.98 W / (m·K).
[0130] Comparative Example 2: Fe2O3 / ZrO2 double-layer structure thermal protection coating is completed according to the following steps:
[0131] 1. Substrate surface pretreatment:
[0132] Using anhydrous ethanol as solvent, dust, grease and impurities on the surface of the substrate are removed, and then the surface of the substrate is activated to obtain a pretreated substrate;
[0133] The substrate described in step 1 is an aluminum alloy with a thickness of 3 mm, and the aluminum alloy model is 6061;
[0134] In step 1, a mechanical sandblasting process is used to activate the surface of the substrate; the sandblasting material selected for the mechanical sandblasting process is quartz sand, the sandblasting pressure is 0.2MPa, the sandblasting distance is 100mm, and the sandblasting angle is 45°;
[0135] 2. Preparation of low thermal conductivity layer:
[0136] The powder is sprayed onto the pretreated substrate surface by thermal spraying to obtain a substrate covered with a ceramic bottom layer having low thermal conductivity;
[0137] The ceramic powder with low thermal conductivity described in step 2 is ZrO2, and the particle size is 2 μm;
[0138] The thermal spraying method described in step 2 is atmospheric plasma spraying, and the process parameters are: argon is used as the main gas, hydrogen is used as the auxiliary gas, the main gas flow rate is 40NLPM, the auxiliary gas flow rate is 10NLPM, the carrier gas flow rate is 3NLPM, the plasma spray gun power is 42.5kw, the powder feeder speed is 25rpm, and the nozzle distance is 100mm;
[0139] In step 2, the thickness of the ceramic bottom layer with low thermal conductivity on the substrate is 0.55 mm, and the density is 85.4%;
[0140] 3. Preparation of high absorption layer:
[0141] The powder with high absorption is fully mixed with a binder to obtain a mixed powder; the mixed powder is sprayed onto the surface of a substrate covered with a ceramic bottom layer with low thermal conductivity by a slurry spraying method, and the coating thickness can be controlled by the spraying time; the prepared coating is dried at room temperature (25°C) for 5 hours, then cured at 240°C for 1 hour, and then polished to obtain a substrate covered with a high absorption layer, that is, a Fe2O3 / ZrO2 double-layer structure thermal protection coating;
[0142] The powder with high absorption described in step 3 is Fe2O3;
[0143] The binder described in step 3 is sodium silicate;
[0144] The mass ratio of the highly absorbent powder to the binder described in step 3 is 3:2;
[0145] The process parameters of the slurry spraying method described in step 3 are: air pressure 2MPa, spraying distance 300mm, and spraying time 55s;
[0146] The specific method of the polishing treatment described in step 3 is: remove the debris and dirt on the surface of the metallographic grinding and polishing machine workbench, install a 300-mesh grinding sheet on the turntable for rough grinding, adjust the metallographic grinding machine parameters, set the speed to 300r / min, and the grinding time to 3min; replace the 800-mesh grinding sheet for fine grinding, adjust the metallographic grinding machine parameters, set the speed to 600r / min, and the grinding time to 2min;
[0147] The thickness of the high absorption layer in the Fe2O3 / ZrO2 double-layer thermal protection coating described in step 3 is 0.95 mm, the density is 71%, and the absorption coefficient is 46895 cm -1The average roughness of the coating surface is 0.65μm.
[0148] The optical properties of the Fe2O3 / ZrO2 double-layer thermal protection coating prepared in Comparative Example 2 were tested using a Fourier spectrometer, and the results showed that the transmittance of the coating in the 0.5-10 μm band was 0.22 and the reflectivity was 0.21.
[0149] The thermal conductivity of the Fe2O3 / ZrO2 double-layer structure thermal protection coating prepared in Comparative Example 2 was measured using a laser thermal conductivity meter, and the thermal conductivity of the coating at high temperature (1000°C) was measured to be 1.9 W / (m·K).
[0150] Comparative Example 3: ZrO2 single-layer thermal protection coating is prepared by the following steps:
[0151] 1. Substrate surface pretreatment:
[0152] Using anhydrous ethanol as solvent, dust, grease and impurities on the surface of the substrate are removed, and then the surface of the substrate is activated to obtain a pretreated substrate;
[0153] The substrate described in step 1 is an aluminum alloy with a thickness of 3 mm, and the aluminum alloy model is 6061;
[0154] In step 1, a mechanical sandblasting process is used to activate the surface of the substrate; the sandblasting material selected for the mechanical sandblasting process is quartz sand, the sandblasting pressure is 0.2MPa, the sandblasting distance is 100mm, and the sandblasting angle is 45°;
[0155] 2. Preparation of low thermal conductivity layer:
[0156] The ceramic powder with low thermal conductivity is sprayed onto the pretreated substrate surface by thermal spraying to obtain a substrate covered with a ceramic bottom layer with low thermal conductivity, namely, a ZrO2 single-layer structure thermal protection coating;
[0157] The ceramic powder with low thermal conductivity described in step 2 is ZrO2, and the particle size is 2 μm;
[0158] The thermal spraying method described in step 2 is atmospheric plasma spraying, and the process parameters are: argon is used as the main gas, hydrogen is used as the auxiliary gas, the main gas flow rate is 40NLPM, the auxiliary gas flow rate is 10NLPM, the carrier gas flow rate is 3NLPM, the plasma spray gun power is 42.5kw, the powder feeder speed is 25rpm, and the nozzle distance is 100mm;
[0159] In step 2, the thickness of the ceramic bottom layer with low thermal conductivity on the substrate is 1.2 mm, and the density is 82%;
[0160] The specific method of the polishing treatment described in step 2 is: remove the debris and dirt on the surface of the metallographic grinding and polishing machine workbench, install a 300-mesh grinding sheet on the turntable for rough grinding, adjust the metallographic grinding machine parameters, set the speed to 300r / min, and the grinding time to 3min; replace the 800-mesh grinding sheet for fine grinding, adjust the metallographic grinding machine parameters, set the speed to 600r / min, and the grinding time to 2min;
[0161] The average surface roughness of the ZrO2 single-layer thermal protection coating described in step 2 is 0.75 μm;
[0162] The optical properties of the ZrO2 single-layer thermal protection coating prepared in Comparative Example 3 were tested using a Fourier spectrometer, and the results showed that the transmittance of the coating in the 0.5-10 μm band was 0.75, and the reflectivity was 0.17.
[0163] The thermal conductivity of the ZrO2 single-layer thermal protection coating prepared in Comparative Example 3 was measured using a laser thermal conductivity meter. The thermal conductivity of the coating at high temperature (1000° C.) was found to be 2.3 W / (m·K).
[0164] Figure 2 This is a cross-sectional morphology image of the TiO2 / Fe2O3 / ZrO2 thermal conductive and radiation composite shielding multilayer structure thermal protection coating material prepared in Example 1, obtained by SEM electron microscope scanning;
[0165] from Figure 2 It can be seen that the internal distribution of the structural coating is uniform, with a small amount of pores, and the coating thicknesses are: low thermal conductivity layer thickness 0.25mm, high absorption layer thickness 0.95mm, and high reflection layer thickness 0.3mm.
[0166] Figure 3 The infrared reflectivity spectrum and infrared transmittance spectrum are shown in FIG. (a) is the infrared reflectivity spectrum of the TiO2 / Fe2O3 / ZrO2 thermal conductive and radiation composite shielding multilayer structure thermal protective coating material prepared in Example 1; (b) is the infrared transmittance spectrum of the TiO2 / Fe2O3 / ZrO2 thermal conductive and radiation composite shielding multilayer structure thermal protective coating material prepared in Example 1;
[0167] from Figure 3 It can be seen that the multi-layer thermal protection coating material has high reflectivity and absorptivity in the 0.5-10 μm band, and the coating transmittance is less than 0.1 in the entire band.
[0168] Figure 4 The infrared transmittance spectrum of the TiO2 / ZrO2 double-layer thermal protection coating prepared in Comparative Example 1;
[0169] from Figure 4It can be seen that the transmittance of the double-layer structure in the 1-5 μm band reaches more than 0.2. Compared with the three-layer structure, the lack of a high absorption layer greatly increases its transmittance.
[0170] Figure 5 The infrared transmittance spectrum of the Fe2O3 / ZrO2 double-layer thermal protection coating prepared in Comparative Example 2;
[0171] from Figure 5 It can be seen that the transmittance of the double-layer structure in the 2-5 μm band reaches above 0.2, indicating that the lack of a high-reflection layer increases its transmittance.
[0172] Figure 6 The infrared transmittance spectrum of the ZrO2 single-layer thermal protection coating prepared in Comparative Example 3.
[0173] from Figure 6 It can be seen that the transmittance of the single-layer ZrO2 structure coating reaches above 0.75. Compared with the above structure, the lack of high absorption layer and high reflection layer greatly increases the transmittance.
Claims
1. A method for preparing a multi-layer structure thermal protective coating material with heat conduction and radiation composite shielding, characterized in that The preparation method is specifically completed according to the following steps:
1. Substrate surface pretreatment: Removing dust, grease and impurities from the surface of the substrate, and then activating the surface of the substrate to obtain a pretreated substrate; 2. Preparation of low thermal conductivity layer: A thermal insulation layer with low thermal conductivity is prepared on the surface of the substrate by a spraying method; The thermal conductivity of the thermal insulation layer with low thermal conductivity described in step 2 is less than 2 W / (m·K); The functional component of the heat insulation layer in step 2 is one or a combination of ZrO2, Si3N4 and rare earth acid ceramics; 3. Preparation of high absorption layer: A middle layer with high infrared absorption is prepared on the thermal insulation layer by spraying; The functional component of the intermediate layer with high infrared absorption in step 3 has high infrared absorption in the 0.5 μm to 10 μm band and is one or a combination of transition metal oxides, carbon-based materials and narrow bandgap semiconductor materials; 4. Preparation of high reflective layer: A high-reflection layer is prepared on the middle layer with high infrared absorption by spraying, and a multi-layer structure thermal protection coating material with heat conduction and radiation composite shielding is finally obtained after polishing. The functional component of the high reflective layer described in step 4 has high infrared reflectivity in the 0.5 μm to 10 μm band and is any one of metal oxides, two-dimensional materials and noble metals; The effective thermal conductivity of the multi-layer thermal protective coating material with thermal conductivity and radiation composite shielding described in step 4 is less than 1W / (m·K), the infrared transmittance in the 0.5μm to 10μm band is less than 0.12, and the infrared reflectivity is greater than 0.
4.
2. The method for preparing a multi-layer structure thermal protective coating material with heat conduction and radiation composite shielding according to claim 1, characterized in that The substrate described in step one is any one of a metal-based material and a ceramic-based composite material; the metal-based material is carbon steel, aluminum alloy, titanium alloy or nickel-based alloy; the ceramic-based composite material is C / C, C / SiC, SiC / SiC; in step one, water, methanol, ethanol, ammonia water, potassium hydroxide solution, nitric acid or hydrochloric acid is used to clean the substrate to remove dust, grease and impurities on the surface of the substrate.
3. The method for preparing a multi-layer structure thermal protective coating material with heat conduction and radiation composite shielding according to claim 2, characterized in that The mass fraction of the ammonia water is 1% to 5%, the mass fraction of the potassium hydroxide solution is 5% to 10%, the mass fraction of the nitric acid is 10% to 30%, and the mass fraction of the hydrochloric acid is 10% to 20%.
4. The method for preparing a multi-layer structure thermal protective coating material with heat conduction and radiation composite shielding according to claim 1, characterized in that In step 1, a mechanical sandblasting process is used to activate the surface of the substrate; the sandblasting material selected for the mechanical sandblasting process is silica sand, quartz sand or ceramic beads, the sandblasting pressure is 0.2MPa~0.6MPa, the sandblasting distance is 100mm~300mm, and the sandblasting angle is 45~90°.
5. The method for preparing a multi-layer structure thermal protective coating material with heat conduction and radiation composite shielding according to claim 1, characterized in that The rare earth acid salt ceramic described in step 2 is type, type, Type, wherein A is one or a combination of Sc, Yb, Lu, Er, Tm, Dy, Ho, La, Y, Gd, Ti, Sm, Nd and Eu; B is Zr, Ce or Hf; C is Ta or Nb.
6. The method for preparing a multi-layer structure thermal protective coating material with heat conduction and radiation composite shielding according to claim 1, characterized in that The powder particle size of the functional component of the thermal insulation layer described in step 2 is 1μm to 10μm; the thickness of the thermal insulation layer with low thermal conductivity on the substrate in step 2 is 0.01mm to 1mm, the density is greater than 70%, and the thermal conductivity is less than 2W / mK.
7. The method for preparing a multi-layer structure thermal protective coating material with heat conduction and radiation composite shielding according to claim 1, characterized in that The transition metal oxide described in step three is Fe3O4, Fe2O3, CuO, MnO2, Co2O3 or ZnO; the carbon-based material is nanocarbon black or graphene; and the narrow bandgap semiconductor material is cadmium selenide or bismuth selenide.
8. The method for preparing a multi-layer structure thermal protective coating material with heat conduction and radiation composite shielding according to claim 1, characterized in that The thickness of the intermediate layer with high infrared absorption in step 3 is 0.01 mm to 2 mm, the density is greater than 60%, and the absorption coefficient is greater than 10000 cm -1 .
9. The method for preparing a multi-layer structure thermal protection coating material with heat conduction and radiation composite shielding according to claim 1, characterized in that The metal oxide described in step four is TiO2 or Al2O3; the two-dimensional material is BN, indium selenide or transition metal disulfide; the noble metal is Pt or Pt alloy; the thickness of the high reflective layer described in step four is 0.01mm~1mm, the density is greater than 60%, and the complex refractive index modulus is greater than 2.
10. The method for preparing a multi-layer structure thermal protection coating material with heat conduction and radiation composite shielding according to claim 1, characterized in that The specific method of polishing treatment described in step 4 is: remove the debris and dirt on the surface of the workbench of the metallographic grinding and polishing machine, install the 300-mesh grinding sheet on the turntable for rough grinding, adjust the parameters of the metallographic grinding machine, set the speed to 300r / min, and the grinding time for 3min; replace the 800-mesh grinding sheet for fine grinding, adjust the parameters of the metallographic grinding machine, set the speed to 600r / min, and the grinding time for 2min. The average roughness Ra of the coating surface is less than 2μm; the spraying method described in steps 2, 3, and 4 is: thermal spraying or slurry spraying; the binder in the slurry spraying is one or a combination of potassium silicate, aluminum silicate, silica sol and aluminum phosphate.
Citation Information
Patent Citations
Nano silicon oxide heat-insulating material with radiation shield layer and preparation method thereof
CN103693938A
Surface-toughened alumina fiber rigid heat-insulation tile multilayer composite material, coating composition, and preparation method and application of composite materia
CN108455978A
High-energy laser protection multilayer composite material coating structure and manufacturing method thereof
CN113549862A
High-temperature-resistant multilayer thermal insulation material based on multifunctional reflecting screen, and preparation method thereof
CN113858724A
Thermal protection composite coating and manufacturing method thereof
CN114411080A
Cited By
High reflection-high emission-low thermal conductivity synergistic thermal protection coating and preparation method
CN122879640A
A high-reflectivity, high-emissivity, and low-thermal-conductivity synergistic thermal protective coating and its preparation method
CN122879640B