Method for synchronously removing platinum-aluminum coating on surface of blade and aluminized layer in inner cavity of blade

By employing steps such as water blowing, acid immersion, and ultrasonic cleaning, combined with the corrosion-inhibiting effects of citric acid and hexamethylenetetramine, the platinum-aluminum coating on the surface and inner cavity of aero-engine blades is removed simultaneously. This solves the problem of the impact of coating removal quality on blade life and achieves efficient and low-cost coating removal.

CN119016424AInactive Publication Date: 2024-11-26STATE-OWNED SICHUAN WEST MASCH FACTORY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411361733.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies struggle to efficiently remove platinum-aluminum coatings and aluminized layers from the surface of aero-engine blades without damaging the blade substrate, and the quality of coating removal has a significant impact on the quality of the new coating and the blade's lifespan.

Method used

A combination of water blowing, acid immersion, ultrasonic cleaning and neutralization treatment is adopted. Citric acid and hexamethylenetetramine are used as corrosion inhibitors to gradually penetrate the acid into the blade cavity, simultaneously removing the surface and inner cavity coatings and protecting the nickel substrate from damage.

Benefits of technology

This method enables efficient removal of platinum-aluminum coatings and internal aluminized layers without damaging the blade substrate, ensuring the quality of the new coating and the service life of the blade. The process is simple and inexpensive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016424A_ABST
    Figure CN119016424A_ABST
Patent Text Reader

Abstract

The invention discloses a method for synchronously removing a platinum-aluminum coating on the surface of a blade and an aluminized layer in an inner cavity of the blade, and relates to the technical field of aviation equipment cleaning. The method comprises the following steps that S100, the surface of a workpiece is treated through water sand blasting; s200, the workpiece subjected to surface treatment is put into the added cleaning solution; s300, the workpiece is cleaned; the cleaning solution is composed of hydrochloric acid, phosphoric acid, citric acid, hexamethylenetetramine and water; the purpose that an aluminum coating on the surface of the blade and an inner cavity aluminized layer are removed in one step on the premise that parts are not damaged is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aviation equipment cleaning, in particular to a method for synchronously removing a platinum-aluminum coating on a blade surface and an inner cavity aluminum diffusion layer. Background Art

[0002] In the aviation industry, in order to ensure the stable operation of aircraft engine blades, a layer of coating for high temperature oxidation resistance and corrosion resistance is usually applied to the blade surface and inner cavity. Platinum aluminum coating and aluminized layer are widely used in key hot end components of advanced aircraft engines and gas turbine engines because of their excellent comprehensive performance of oxidation resistance and corrosion resistance as a high temperature protective coating.

[0003] However, after a certain period of service, the blade coating will fall off, wear out, drop off, and other faults, causing the coating to degrade or fail; at the same time, during the coating process, various factors may cause the coating preparation quality to be unqualified and require rework and repair. Due to the complex manufacturing process of blades, the processing costs of high-temperature alloys and single-crystal blades are much higher than the coating costs. If the blades are scrapped simply because the coating is unqualified, it will cause a great waste. Therefore, it is necessary to remove and rework the surface platinum-aluminum coating and the inner cavity aluminum layer of the failed and reworked blades, which will have great significance for the full service life of the blades.

[0004] The removal and re-coating of coatings may cause many changes in parts from size to structural performance. The quality of coating removal directly affects the quality of the newly applied coating. Unqualified quality will directly affect the use of the blade. Therefore, coating removal is particularly important as a pre-treatment process for coating. Exploring the removal process of platinum-aluminum coating and inner cavity aluminized layer can provide important technical guarantees for the repair of blade coatings. Summary of the invention

[0005] The object of the present invention is to provide a method for synchronously removing the platinum-aluminum coating on the blade surface and the inner cavity aluminized layer, so as to achieve the purpose of removing the aluminum coating on the blade surface and the inner cavity aluminized layer in one step without damaging the parts.

[0006] In order to achieve the above object, the present invention adopts the following technical means: A method for synchronously removing a platinum-aluminum coating on a blade surface and an inner cavity aluminized layer comprises the following steps: S100. Use water sandblasting to treat the workpiece surface; S200. The surface treated workpiece is placed in the added cleaning solution; S300. Cleaning the workpiece; The cleaning solution consists of hydrochloric acid, phosphoric acid, citric acid, hexamethylenetetramine and water.

[0007] Preferably, in step S100, the water sand blowing pressure is 0.2-0.3 MPa, and the time is 10-20 seconds.

[0008] Furthermore, the step S200 includes: S210. Configure the cleaning solution; S220. Soak the surface-treated workpiece in the cleaning solution heated to 50-70° C. for 30-60 minutes, and remove the workpiece every 10-30 minutes to clean the corrosion products during the soaking process.

[0009] Furthermore, the cleaning solution includes an acid component and a corrosion inhibition component, wherein the acid component includes 30% to 35% hydrochloric acid and 30% to 35% phosphoric acid, and the rest is water; The corrosion inhibition component includes 2-6 parts / 100ml of citric acid and 0.5-1 parts / 100ml of hexamethylenetetramine.

[0010] Furthermore, the step S300 includes: S310. Remove the workpiece from the cleaning solution and wash it with clean water; S320. Then immerse the workpiece in an ultrasonic environment; S330. Immersing the workpiece after ultrasonic cleaning in a neutralizing solution; S340. The neutralized workpiece is cleaned by water-blasting and then dried.

[0011] Furthermore, in step S320, the ultrasonic frequency is 30-50 kHz, and the ultrasonic time is 10-20 min.

[0012] Furthermore, in step S330, the neutralizing solution is a 30-50 g / L sodium carbonate solution, and the soaking time is 20-30 min.

[0013] Furthermore, in step S340, the sand blowing pressure is 0.2-0.3 MPa, the time is 10-20 s, and the drying temperature is 190-210°C.

[0014] During use, the present invention has the following beneficial effects: The process method of the present invention uses citric acid and hexamethylenetetramine as slow-release substances for the nickel-based layer, and uses hexamethylenetetramine to pair with the lone electron pair on nickel, thereby ensuring that Al reacts preferentially with the acid solution, and realizing slow-release protection for the nickel substrate in the acid solution. It is precisely because of the change in the potential of nickel that, as the workpiece is immersed, the acid solution can gradually penetrate from the pores on the blade, and then allow the acid solution to enter the inner cavity of the blade to remove the aluminized layer in the inner cavity of the blade. The protective effect of citric acid and hexamethylenetetramine on the nickel base can not only protect the surface of the nickel substrate, but also achieve good protection for the nickel substrate in the cavity on the blade. Furthermore, the method involved in the present application can simultaneously remove the platinum-aluminum coating on the surface of the gas turbine blade and the aluminized layer in the inner cavity. There is no damage to the substrate after removing the coating. The process method is simple, the equipment price is low, and the removal efficiency is high compared to the traditional removal formula. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is the surface state of the blade sample before removing the coating according to the present invention.

[0016] Figure 2 This is a metallographic image of the coating on the surface and inner cavity of the blade sample before removing the coating according to the present invention.

[0017] Figure 3 This is the surface state of the blade sample after the coating is removed according to the present invention.

[0018] Figure 4 This is a metallographic image of the blade sample surface after the coating is removed according to the present invention.

[0019] Figure 5 This is a metallographic image of the inner cavity of the blade sample after the coating is removed according to the present invention. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0021] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0023] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0024] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, or the positions or positional relationships in which the product of the invention is usually placed when in use, or the positions or positional relationships commonly understood by those skilled in the art, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.

[0025] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0026] Example 1 First, a water-blasting machine was used to blast the samples with platinum-aluminum coating and inner cavity aluminized layer after service ( Figure 1 and Figure 2 ) was subjected to water sand blasting treatment with a sand blasting pressure of 0.25 MPa and a sand blasting time of 15 s. The sand was made of 280-mesh white jade steel sand to remove the oxide film and dirt on the surface of the sample after service.

[0027] Then, 30 mL of hydrochloric acid, 30 mL of phosphoric acid, 4 g of citric acid, 0.75 g of hexamethylenetetramine, and 40 mL of water were placed in a water bath and heated at 60 °C for 20 min to obtain a mixed solution; After that, the mixed solution was heated at 35 °C for 20 min, and the sample with platinum-aluminum coating and inner cavity aluminum layer was placed in the cleaning solution and reacted for 40 min. During the reaction, the solution was stirred with a magnetic stirrer, and the sample was taken out every 20 min, and the dust on the surface was wiped off with a non-woven cloth. After the reaction is completed, the sample is immediately taken out from the removal solution and washed with water to remove the impurities remaining on the sample; At the same time, the cleaned samples were further ultrasonically cleaned at a frequency of 40kHz for 15 min to remove the corrosion products on the surface; Then, the ultrasonically cleaned sample was placed in a prepared 40 g / L sodium carbonate solution and neutralized for 25 min to remove the residual acid after the reaction; Finally, the neutralized sample was placed in an air heating furnace at 200°C for 2 h for drying under a sand blowing pressure of 0.25 MPa and a sand blowing time of 15 s.

[0028] Figure 3 This is a real picture of the parts after the platinum-aluminum coating and the inner cavity aluminum layer are removed in this embodiment. Figure 3 It can be seen that the platinum-aluminum coating is completely removed and there is no residual coating on the blade surface. After removing the platinum-aluminum coating, the blade surface is uniform in color and no obvious defects appear. In order to verify the corrosion of the metal matrix material after the platinum-aluminum coating is removed, the blade after this implementation scheme is cut and metallographically inspected. The inspection results are as follows: Figure 4 and Figure 5 As shown, the platinum-aluminum coating is removed cleanly and the metal substrate is free of corrosion and damage.

[0029] Example 2 First, a water-blasting machine was used to blast the samples with platinum-aluminum coating and inner cavity aluminized layer after service ( Figure 1 and Figure 2 ) was subjected to water sand blasting treatment with a sand blasting pressure of 0.25 MPa and a sand blasting time of 15 s. The sand was made of 280-mesh white jade steel sand to remove the oxide film and dirt on the surface of the sample after service.

[0030] Then, 35 mL of hydrochloric acid, 30 mL of phosphoric acid, 4 g of citric acid, 0.75 g of hexamethylenetetramine, and 35 mL of water were placed in a water bath and heated at 35 °C for 20 min to obtain a mixed solution; After that, the mixed solution was heated at 60 °C for 20 min, and the sample with platinum-aluminum coating and inner cavity aluminum layer was placed in the cleaning solution for 35 min. During the reaction, the solution was stirred with a magnetic stirrer, and the sample was taken out every 20 min, and the dust on the surface was wiped off with a non-woven cloth. After the reaction is completed, the sample is immediately taken out from the removal solution and washed with water to remove the impurities remaining on the sample; At the same time, the cleaned samples were further ultrasonically cleaned at a frequency of 40kHz for 15 min to remove the corrosion products on the surface; Then, the ultrasonically cleaned sample was placed in a prepared 40 g / L sodium carbonate solution and neutralized for 25 min to remove the residual acid after the reaction; Finally, the neutralized sample was placed in an air heating furnace at 200°C for 2 h for drying under a sand blowing pressure of 0.25 MPa and a sand blowing time of 15 s.

[0031] Example 3 First, a water-blasting machine was used to blast the samples with platinum-aluminum coating and inner cavity aluminized layer after service ( Figure 1 and Figure 2 ) was subjected to water sand blasting treatment with a sand blasting pressure of 0.25 MPa and a sand blasting time of 15 s. The sand was made of 280-mesh white jade steel sand to remove the oxide film and dirt on the surface of the sample after service.

[0032] Then, 35 mL of hydrochloric acid, 35 mL of phosphoric acid, 4 g of citric acid, 0.75 g of hexamethylenetetramine, and 30 mL of water were placed in a water bath and heated at 35 °C for 20 min to obtain a mixed solution; After that, the mixed solution was heated at 60 °C for 20 min, and the sample with platinum-aluminum coating and inner cavity aluminum layer was placed in the cleaning solution for 35 min. During the reaction, the solution was stirred with a magnetic stirrer, and the sample was taken out every 20 min, and the dust on the surface was wiped off with a non-woven cloth. After the reaction is completed, the sample is immediately taken out from the removal solution and washed with water to remove the impurities remaining on the sample; At the same time, the cleaned samples were further ultrasonically cleaned at a frequency of 40kHz for 15 min to remove the corrosion products on the surface; Then, the ultrasonically cleaned sample was placed in a prepared 40 g / L sodium carbonate solution and neutralized for 25 min to remove the residual acid after the reaction; Finally, the neutralized sample was placed in an air heating furnace at 200°C for 2 h for drying under a sand blowing pressure of 0.25 MPa and a sand blowing time of 15 s.

[0033] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for synchronously removing the platinum-aluminum coating on the blade surface and the inner cavity aluminized layer, characterized in that: The following steps are involved: S100. Use water sandblasting to treat the workpiece surface; S200. The surface treated workpiece is placed in the added cleaning solution; S300. Cleaning the workpiece; The cleaning solution consists of hydrochloric acid, phosphoric acid, citric acid, hexamethylenetetramine and water.

2. The method for synchronously removing the platinum-aluminum coating on the blade surface and the inner cavity aluminized layer according to claim 1, characterized in that: In step S100, the water sand blowing pressure is 0.2-0.3 MPa, and the time is 10-20 seconds.

3. The method for synchronously removing the platinum-aluminum coating on the blade surface and the inner cavity aluminized layer according to claim 1, characterized in that: The step S200 includes: S210. Configure the cleaning solution; S220. Soak the surface-treated workpiece in the cleaning solution heated to 50-70° C. for 30-60 minutes, and remove the workpiece every 10-30 minutes to clean the corrosion products during the soaking process.

4. A method for synchronously removing the platinum-aluminum coating on the blade surface and the inner cavity aluminized layer according to any one of claims 1 to 3, characterized in that: The cleaning solution comprises an acid component and a corrosion inhibition component. The acid component comprises, by weight, 30 to 35 parts of hydrochloric acid, 30 to 35 parts of phosphoric acid, 200 to 600 parts of citric acid, 50 to 100 parts of hexamethylenetetramine, and 80 to 100 parts of water.

5. The method for synchronously removing the platinum-aluminum coating on the blade surface and the inner cavity aluminized layer according to claim 1, characterized in that: The step S300 includes: S310. Remove the workpiece from the cleaning solution and wash it with clean water; S320. Then immerse the workpiece in an ultrasonic environment; S330. Immersing the workpiece after ultrasonic cleaning in a neutralizing solution; S340. The neutralized workpiece is cleaned by water-blasting and then dried.

6. The method for synchronously removing the platinum-aluminum coating on the blade surface and the inner cavity aluminized layer according to claim 5, characterized in that: In step S320, the ultrasonic frequency is 30-50 kHz, and the ultrasonic time is 10-20 min.

7. The method for synchronously removing the platinum-aluminum coating on the blade surface and the inner cavity aluminized layer according to claim 5, characterized in that: In step S330, the neutralizing solution is a 30-50 g / L sodium carbonate solution, and the soaking time is 20-30 min.

8. The method for synchronously removing the platinum-aluminum coating on the blade surface and the inner cavity aluminized layer according to claim 5, characterized in that: In step S340, the sand blowing pressure is 0.2-0.3 MPa, the time is 10-20 seconds, and the drying temperature is 190-210°C.