Hot working method for large-thickness 980MPa-grade ultrahigh-strength steel structure

By controlling the hot press forming temperature and tempering heat treatment process, the problem of mechanical properties recovery after hot press forming of large-thick high-strength steel plates is solved, and the mechanical properties recovery of ultra-high-strength steel plates is achieved, meeting the requirements of pressure resistance and load-bearing structure.

CN119016567AActive Publication Date: 2024-11-26CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE

Patent Information

Application Number
CN202411132065.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The prior art cannot achieve the return of the mechanical properties of large-thick and high-strength steel plates to the supply level after hot-press forming, and cannot meet the requirements of pressure-resistant structures and load-bearing structures.

Method used

The heat pressing forming is performed by controlling the furnace temperature and heating rate, combining the tempering and heat treatment process, including quenching and tempering treatment, and adjusting the structural structure and mechanical properties of the steel plate. Specific steps include preheating of the steel plate, hot press forming, quenching treatment and tempering treatment to ensure that the steel plate is hot pressed in a low-strength and high-plastic range, and its strength and toughness are restored through tempering and heat treatment.

Benefits of technology

The mechanical properties recovery of ultra-high strength steel plates are achieved, meeting the requirements of pressure-resistant structures and load-bearing structures, and the yield strength is not less than 980MPa, the elongation after break is not less than 16% and the impact absorption energy of -20℃ is not less than 120J performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016567A_ABST
    Figure CN119016567A_ABST
Patent Text Reader

Abstract

The invention provides a hot working method for a large-thickness 980 MPa-grade ultrahigh-strength steel structure. The hot working method comprises the following specific steps that S1, a steel plate is preheated; s2, pressing and forming the steel plate; s3, the structural part obtained after pressing forming is loaded into a heating furnace, heating is conducted to 850-890 DEG C, heat preservation is conducted, heat preservation is conducted for a period of time t2 under the condition of 850-890 DEG C, and then the structural part is discharged out of the furnace and subjected to water cooling to the room temperature; s4, a tempering process is conducted, specifically, the structural part subjected to quenching heat treatment is loaded into a heating furnace and heated to 560-620 DEG C, heat preservation is conducted for a period of time t3 under the condition of 560-620 DEG C, and then the structural part is discharged out of the furnace and air-cooled to the room temperature; and S5, checking and accepting. According to the method, the steel plate is subjected to hot pressing forming in a low-strength and high-plasticity interval through hot pressing forming temperature control, good shape and size control can be obtained, then a structural part is subjected to quenching and tempering heat treatment, the steel plate supply state level is recovered, and the use requirements of a pressure-resistant structure and a bearing structure are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal materials, and in particular to a hot processing method for a thick 980MPa-grade ultra-high strength steel structure. Background Art

[0002] Most large-scale pressure-resistant structures or load-bearing structures require steel plates to have a certain shape, and the steel plates need to be cold-formed or hot-formed. For ultra-high-strength steel thick plates, cold-forming manufacturing is difficult and requires high equipment pressure; due to the Bauschinger effect, the performance of the steel plate after cold pressing is uneven, the yield strength of the pressure surface will be lower than before cold forming, and the yield strength of the tensile surface will be higher than before cold forming, which does not meet the technical index requirements and requires performance recovery heat treatment. The steel plate has low strength and high plasticity under high temperature conditions, and the hot-pressing manufacturing has relatively low equipment pressure requirements; after hot-pressing, the steel plate structure changes from tempered troostite to bainite + martensite, and both strength and plasticity decrease, requiring performance recovery heat treatment.

[0003] Patent No. CN 107475623A "A hot-formed high-strength steel and its processing method" introduces a hot-formed high-strength steel with a yield strength ≥450MPa and its processing method. The steel has a low alloy content and is used for the manufacture of parts. The thickness and size of the parts are small and are not suitable for the manufacture of pressure-resistant structures. Patent No. CN 115109992 B "A steel plate for pressure vessels with good hot formability and its manufacturing method" introduces a steel plate for pressure vessels with a yield strength ≥380MPa and its manufacturing method. The hot forming processing performance of the steel plate is not described, and the strength gap is large compared with the steel plate with a yield strength ≥980MPa of the present invention. Patent No. CN104936716 A "Manufacturing method of hot-pressed steel components" introduces a hot-pressed forming manufacturing method for steel parts for automobiles. The thickness of the steel plate used is only 1.4mm, which is significantly different from the hot forming manufacturing requirements of the ultra-high-strength steel thick plate of the present invention.

[0004] Therefore, the existing technical solutions are unable to restore the mechanical properties of thick high-strength steel plates to the supply level after hot-pressing to meet the use requirements of pressure-resistant structures and load-bearing structures. Summary of the invention

[0005] In view of this, the present invention aims to propose a hot processing method for large-thickness 980MPa ultra-high-strength steel structures, so as to solve the problem that after the ultra-high-strength steel thick plates are hot-pressed, the strength, toughness and plasticity of the structural parts change and cannot be restored to the supply level of the steel plates, so as to meet the use requirements of pressure-resistant structures and load-bearing structures.

[0006] In order to solve the above technical problems, the process parameters of hot pressing and tempering heat treatment of ultra-high strength steel structure of the present invention are formulated for the following reasons:

[0007] The influence of furnace charging temperature and heating rate on hot pressing forming and mechanical properties of steel plates: If the furnace charging temperature is too high and the heating rate is too fast, the temperature of the steel plate in the thickness direction will be uneven; if the heating rate is too slow, the heat treatment cycle will increase and the cost will be increased. Therefore, the furnace charging temperature and heating rate should be controlled within an appropriate range. In the present invention, the furnace charging temperature is controlled to be no higher than 400℃ and the heating rate is controlled to be no higher than 200℃ / h.

[0008] Confirmation of hot press forming parameters: The influence of temperature on tensile properties and grain size of 10CrNi8MoV steel is shown in Table 1. As the temperature increases, the strength of the steel plate decreases and the plasticity increases, which is suitable for hot press forming. If the temperature is too high, the grain size of the steel plate will be coarse, which is not conducive to the subsequent performance recovery. Therefore, it is selected to keep warm at (830-880)℃ ((1.0-1.5)×plate thickness)min; if the holding time is too short, the temperature in the thickness direction of the steel plate is uneven, and if the holding time is too long, the cost will be increased. If the temperature is too low, the strength of the steel plate is still high, and the plasticity is low. Hot press forming requires high equipment pressure, and crack defects are prone to occur when the forming curvature is small, so the final forming temperature is selected to be not less than 700℃.

[0009] Table 1 High temperature tensile properties and grain size of 10CrNi8MoV steel

[0010]

[0011]

[0012] After hot pressing, the structure of 10CrNi8MoV steel plate changes from tempered troostite to bainite + a small amount of martensite, and the yield strength, plasticity (elongation after fracture) and toughness (-20℃KV2) all decrease, which does not meet the technical requirements of steel plate. Therefore, it is necessary to perform performance recovery heat treatment (quenching and tempering heat treatment) on the hot-formed structural parts.

[0013] Confirmation of quenching and tempering heat treatment parameters: The quenching and tempering heat treatment process is quenching + tempering. If the quenching and holding temperature is low and the time is short, the austenitization effect of the organization is insufficient; if the holding temperature is high and the time is long, it is easy to cause coarse grains, which is not conducive to the subsequent performance recovery. The present invention sets the quenching system to (850-900)℃ holding ((2.5-3.0)×plate thickness) min, within which the organization can be fully austenitized. After quenching, the structure of the structural part is quenched martensite with high internal stress, and tempering treatment is required. The tempering holding temperature and holding time have a great influence on the mechanical properties of the material. If the holding temperature is low and the time is short, the material strength after tempering is high and the plastic toughness is poor. The elongation after fracture does not reach 16%, and the -20℃ KV2 does not reach 120J; if the holding temperature is high and the time is long, the material strength after tempering is low, and the yield strength does not reach 980MPa. The present invention sets the tempering system to (560-620)°C for ((4.5-5.0)×plate thickness) min to obtain a tempered bainite structure, which can ensure that the strength and toughness of the structural parts are well matched after heat treatment and that the mechanical properties meet the index requirements.

[0014] The technical solution of the present invention is achieved as follows: A method for hot processing of a thick 980MPa grade ultra-high strength steel structure comprises the following specific steps:

[0015] S1: preheating the steel plate; heating the steel plate to 830-880°C and keeping it at 830-880°C for a period of time t1;

[0016] S2: Pressing and forming the steel plate; taking the steel plate out of the heating furnace, placing it on a forming mold for pressing, and air-cooling it to room temperature after forming to obtain a structural part of a certain shape;

[0017] S3: quenching treatment of structural parts; quenching process: the pressed structural parts are loaded into a heating furnace, heated to 850-890°C and kept warm for a period of t2 at 850-890°C, and then the structural parts are taken out of the furnace and water-cooled to room temperature;

[0018] S4: Tempering treatment of structural parts; Tempering process: the structural parts after quenching heat treatment are loaded into a heating furnace, heated to 560-620°C, kept at 560-620°C for a period of time t3, and then the structural parts are taken out of the furnace and air-cooled to room temperature to obtain ultra-high strength steel structural parts with restored performance;

[0019] S5: Inspection and acceptance, the mechanical properties of the structural parts meet the requirements of various indicators.

[0020] Furthermore, in step S1, the steel plate is 10CrNi8MoV ultra-high strength steel, the alloy elements Ni+Cr+Mo in the steel plate are ≥8%, the steel plate thickness H ranges from 36 to 80 mm, the room temperature yield strength is not less than 980 MPa, the elongation after fracture is not less than 16%, and the -20°C Charpy V-notch impact absorption energy is not less than 120 J.

[0021] Furthermore, in step S1, the steel plate is loaded into a heating furnace at a temperature below 400°C and heated to a temperature between 830°C and 880°C at a rate not higher than 200°C / h.

[0022] Further, in step S1, the holding time t1 = K1*H, unit: min;

[0023] Among them: K1 value range: 1.0~1.5;

[0024] H is the thickness of the steel plate.

[0025] Furthermore, in step S2, the initial pressing temperature of the steel plate is not less than 800°C, and the final forming temperature is not less than 700°C.

[0026] Furthermore, in step S3, the structural component is placed in a heating furnace at a temperature below 400°C and then heated to between 850°C and 890°C at a rate not higher than 200°C / h.

[0027] Further, in step S3, the holding time t2 = K2*H, unit: min;

[0028] Among them: K2 value range: 2.5 ~ 3.0;

[0029] H is the thickness of the steel plate.

[0030] Furthermore, in step S3, the time from when the structural component is taken out of the furnace to when it is put into the water is no more than 3.0 minutes, and the water temperature in the water tank is no higher than 40° C. during the cooling process.

[0031] Furthermore, in step S4, the structural component is placed in a heating furnace at a temperature below 400°C and then heated to between 560°C and 620°C at a rate not higher than 200°C / h.

[0032] Further, in step S4, the holding time t3 = K3*H, unit: min;

[0033] Among them: the value range of K3 is 4.5~5.0;

[0034] H is the thickness of the steel plate.

[0035] Compared with the prior art, the hot processing method of a large-thickness 980MPa-grade ultra-high-strength steel structure of the present invention has the following advantages:

[0036] 1. The hot processing method of the ultra-high strength steel plate of the present invention controls the hot pressing forming temperature so that the steel plate is hot pressed in the low strength and high plasticity range, which can obtain better shape and size control. Then the structural parts are tempered and heat treated to restore to the supply state of the steel plate, meet the use requirements of pressure-resistant structures and load-bearing structures, and obtain ultra-high strength steel structural parts with restored performance.

[0037] 2. The present invention is suitable for hot processing of steel plates with a thickness not exceeding 80 mm and a yield strength of more than 980 MPa. The process window for hot pressing and tempering heat treatment is wide and the method has strong operability. The performance of structural parts after tempering heat treatment can reach the performance level of the steel plates as delivered.

[0038] 3. The present invention aims at providing 10CrNi8MoV steel plates with a yield strength of more than 980 MPa, an elongation after fracture of not less than 16%, and an impact KV2 of more than 120 J at -20°C. After hot pressing and tempering heat treatment, the mechanical properties of the steel plates can be restored to the level of the steel plates as supplied. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0040] Figure 1 The metallographic diagram of the steel plate in the present invention;

[0041] Figure 2 Hot pressing metallographic diagram of the structural part in the present invention;

[0042] Figure 3 The metallographic diagram of the quenched and tempered state after forming in the present invention;

[0043] Description of reference numerals: DETAILED DESCRIPTION

[0044] In order to make the technical means, objectives and effects of the present invention easy to understand, the embodiments of the present invention are described in detail below with reference to specific drawings.

[0045] It should be noted that all the terms used in the present invention to indicate directionality and position, such as "upper", "lower", "left", "right", "front", "back", "vertical", "horizontal", "inside", "outside", "top", "lower", "lateral", "longitudinal", "center", etc., are only used to explain the relative positional relationship and connection status between the components in a certain state, and are only for the convenience of describing the present invention, rather than requiring the present invention to be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the descriptions of "first", "second", etc. in the present invention are only used for descriptive purposes, and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features.

[0046] In the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0047] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0048] The present invention discloses a method for hot processing a large-thickness 980MPa-grade ultra-high-strength steel structure, comprising the following specific steps:

[0049] S1: preheating the steel plate; heating the steel plate to 830-880°C and keeping it at 830-880°C for a period of time t1;

[0050] S2: Pressing and forming the steel plate; taking the steel plate out of the heating furnace, placing it on a forming mold for pressing, and air cooling it to room temperature after forming to obtain a structural part of a certain shape;

[0051] S3: quenching treatment of structural parts; quenching process: the pressed structural parts are loaded into a heating furnace, heated to 850-890°C and kept warm for a period of t2 at 850-890°C, and then the structural parts are taken out of the furnace and water-cooled to room temperature;

[0052] S4: Tempering treatment of structural parts; Tempering process: the structural parts after quenching heat treatment are loaded into a heating furnace, heated to 560-620°C, kept at 560-620°C for a period of time t3, and then the structural parts are taken out of the furnace and air-cooled to room temperature to obtain ultra-high strength steel structural parts with restored performance;

[0053] S5: Inspection and acceptance, the mechanical properties of the structural parts meet the requirements of various indicators.

[0054] The ultra-high strength steel plate hot processing method described in the present invention preheats the high strength steel plate before hot pressing forming, and the preheating temperature is 830-880°C and kept warm for a period of time t1 under this condition, so that the temperature in the thickness direction of the steel plate is uniform, the strength of the steel plate is reduced, the plasticity is improved, and the hot pressing forming of the steel plate is facilitated.

[0055] After hot working, the structure of the steel plate changes from tempered ropeite to bainite + a small amount of martensite, and the yield strength, plasticity (elongation after fracture) and toughness (-20℃KV2) all decrease, which does not meet the technical requirements of structural parts. Therefore, it is necessary to perform performance recovery heat treatment on the structural parts after hot pressing.

[0056] The method of the present invention adds a tempering heat treatment process, and by adjusting the charging temperature, heating rate, heating temperature and holding time of the quenching process, the structure of the structural part is transformed from bainite + a small amount of martensite to quenched martensite. At this time, the internal stress of the structural part is relatively high, and tempering treatment is required to obtain an ultra-high strength steel structural part with restored performance.

[0057] The ultra-high strength steel plate hot processing method controls the hot pressing forming temperature so that the steel plate is hot pressed in a low strength and high plasticity range, which can obtain better shape and size control, and then the structural parts are tempered and heat treated to restore to the supply state of the steel plate to meet the use requirements of pressure-resistant structures and load-bearing structures, and obtain ultra-high strength steel structural parts with restored performance, avoiding various quality problems caused by too high or too low temperature, such as coarse grains, low strength, high plasticity, or cracks during forming, etc., and can ensure that the mechanical properties of the high-strength steel plate after hot pressing reach the technical requirements of room temperature yield strength of not less than 980MPa, elongation after fracture of not less than 16%, and -20℃ Charpy V-notch impact absorption energy of not less than 120J.

[0058] Specifically, in step S1, the steel plate is 10CrNi8MoV ultra-high strength steel, the alloy elements Ni+Cr+Mo in the steel plate are ≥8%, the steel plate thickness H ranges from 36 to 80 mm, the room temperature yield strength is not less than 980 MPa, the elongation after fracture is not less than 16%, and the -20°C Charpy V-notch impact absorption energy is not less than 120 J.

[0059] The steel plate is made of 10CrNi8MoV ultra-high strength steel, which has a yield strength of not less than 980MPa at room temperature. When the external environment is heated to 830-880°C, its yield strength is greatly reduced and the elongation after fracture is greatly improved, meeting the requirements of hot working of thick steel plates.

[0060] The steel plate material setting can avoid the problem of coarse grains and irreversible performance during hot pressing of the steel plate, while reducing the requirements for equipment pressure during hot pressing, and reducing the risk of cracks during hot pressing when the forming curvature is small.

[0061] Specifically, in step S1, the steel plate is placed in a heating furnace at a temperature below 400°C and heated to a temperature between 830°C and 880°C at a rate not higher than 200°C / h.

[0062] The setting of the furnace charging temperature and heating rate can quickly heat the steel plate to the hot pressing forming temperature, avoiding the uneven temperature in the thickness direction of the steel plate when the furnace charging temperature is too high and the heating rate is fast, which can easily cause quality problems such as cracks in the hot pressing forming. At the same time, compared with a slower heating rate, the heat treatment cycle will be increased, further improving production efficiency and helping to reduce production costs.

[0063] Specifically, in step S1, the heat preservation time t1=K1*H, unit: min;

[0064] Among them: K1 value range: 1.0~1.5;

[0065] H is the thickness of the steel plate.

[0066] The setting of the holding time t1 is based on the thickness of the steel plate, the material and the efficiency of the heating equipment, so that the internal and external temperatures of the heated material are consistent, ensuring that the steel plate obtains relatively ideal performance.

[0067] The setting of the insulation time t1 fully considers the thickness, material and efficiency of the steel plate and avoids the inconsistency of the internal temperature of the steel plate caused by insufficient insulation time t1, which leads to quality problems during hot pressing. It also prevents the defect of reduced production efficiency caused by too long insulation time.

[0068] Specifically, in step S2, the initial pressing temperature of the steel plate is not less than 800°C, and the final forming temperature is not less than 700°C.

[0069] When the temperature of the steel plate is lower than 700℃, its yield strength and elongation after fracture change significantly, causing the strength and plasticity of the steel plate to be higher than the set value, increasing the pressure requirements of the equipment, and easily generating defects such as cracks during the forming process.

[0070] This setting regulates the temperature of the steel plate during the hot pressing process, avoiding the temperature drop of the steel plate due to too long hot pressing time or other factors, which causes a significant change in the mechanical properties of the steel plate, reduces problems such as cracks during the hot pressing process, and helps to improve the product quality of structural parts and ensure the mechanical properties of structural parts.

[0071] Specifically, in step S3, the structural component is placed in a heating furnace at a temperature below 400°C and then heated to between 850°C and 890°C at a rate not higher than 200°C / h.

[0072] The setting of the furnace charging temperature and the heating rate can quickly heat the structural parts to the quenching temperature, reduce the thermal stress generated in the structural parts during the rapid heating process, and improve the quenching quality; at the same time, it avoids excessive heating that causes uneven temperature distribution inside the structural parts, thermal stress and deformation, and increases the heat treatment cycle compared to a slower heating rate, further improving production efficiency and helping to reduce production costs.

[0073] Specifically, in step S3, the holding time t2=K2*H, unit: min;

[0074] Among them: K2 value range: 2.5 ~ 3.0;

[0075] H is the thickness of the steel plate.

[0076] The setting of the holding time t2 is based on the thickness of the structural part and the required phase change process to ensure that the temperature inside the structural part is uniform and the phase change is sufficient.

[0077] The setting of the holding time t2 can make the structure of the structural part fully austenitized, which is conducive to the formation of uniform martensite inside the structural part after rapid cooling, reducing the residual stress inside the structural part, and improving the stability and durability of the structure of the structural part.

[0078] Specifically, in step S3, the time from when the structural parts are taken out of the furnace to when they are put into the water is no more than 3.0 minutes, and the water temperature in the water tank is no higher than 40° C. during the cooling process.

[0079] Take the structural parts out of the heating furnace and cool them in water within 3 minutes to reduce the residence time of the structural parts at high temperature and the transformation of austenite to pearlite and other tissues; at the same time, avoid exposing the structural parts to the air for a long time to avoid large temperature gradients on the surface and inside of the structural parts, thereby generating thermal stress.

[0080] Keeping the water temperature in the water tank no higher than 40℃ can ensure the cooling speed of the structure, reduce the thermal stress generated by the structural parts during the cooling process, and ensure the cooling effect.

[0081] This structural component cooling process helps to ensure the quenching effect, reduce the generation of thermal stress, and improve production efficiency and quenching quality.

[0082] Specifically, in step S4, the structural component is placed in a heating furnace at a temperature below 400°C and then heated to between 560°C and 620°C at a rate not higher than 200°C / h.

[0083] By controlling the charging temperature and heating time, the charging temperature and heating rate can quickly heat the structural parts to the tempering temperature, avoiding uneven temperature in the thickness direction of the structural parts when the charging temperature is too high and the heating rate is too fast, which can easily cause quality problems such as deformation and thermal stress concentration, and provide a stable temperature environment for subsequent insulation treatment.

[0084] This setting can eliminate residual stress and brittleness inside the structural parts, adjust the hardness and toughness of the structural parts, and improve the organizational structure, thereby meeting the mechanical property requirements of the structural parts.

[0085] Specifically, in step S4, the holding time t3=K3*H, unit: min;

[0086] Among them: the value range of K3 is 4.5~5.0;

[0087] H is the thickness of the steel plate.

[0088] By setting the holding time t3, the tempering time of the structural parts is based on the thickness of the structural parts to ensure that the structural parts are kept at the tempering temperature for a sufficient time, fully release the residual stress, make the internal structure of the structural parts uniform, reduce the uneven structure caused by the previous processes such as quenching, and improve the overall performance of the structural parts.

[0089] The setting of the holding time t3 can make the hardness and toughness of the structural parts reach the optimal balance state, meet the mechanical property requirements of the structural parts, avoid excessive tempering while ensuring the tempering effect, adjust the overall mechanical properties of the structural parts, help improve production efficiency, expand the scope of use, and adapt to the tempering processing of structures with different thicknesses.

[0090] Specifically, in step S5, the mechanical properties of the structural parts are as follows: room temperature yield strength is not less than 980 MPa, elongation after fracture is not less than 16%, and -20°C Charpy V-notch impact absorption energy is not less than 120 J.

[0091] The mechanical property requirements of the structural parts set up in this way can meet the technical requirements of the operating conditions, facilitate the inspection of the structural parts, and ensure the stability of product quality in mass production.

[0092] Example

[0093] For three kinds of ultra-high strength 10CrNi8MoV steel plates with different thickness specifications, hot pressing and tempering heat treatment were carried out according to the hot working method of the present invention. The main alloy components and mechanical properties of the steel plates of the three embodiments are shown in Table 2. The steel plates were pressed and tempered according to the parameters shown in Table 3. The mechanical properties of the structural parts after heat treatment are shown in Table 4. The typical metallographic structures are shown in Table 5. Figure 1-3 It should be noted that the present invention is not limited to these embodiments.

[0094] Table 2 Alloy composition and mechanical properties of steel plates in the example

[0095]

[0096] Table 3 Forming and heat treatment process of the embodiment

[0097]

[0098] Table 4 Mechanical properties of structural parts of the embodiment

[0099]

[0100] Table 5 Metallographic structure of Example 3

[0101] Example 3 Availability Hot Pressed State After forming, tempering Metallographic structure Tempered troostite Bainite + a small amount of martensite Tempered troostite Grain size, grade 8.5 8.5 8.5

[0102] The present invention obtains the optimal hot pressing temperature range and performance recovery heat treatment process parameters of 10CrNi8MoV ultra-high strength steel through hot pressing forming temperature research and tempering heat treatment process research. The present invention provides a method for hot processing and manufacturing structural parts for 10CrNi8MoV ultra-high strength steel with a thickness not exceeding 80 mm and a yield strength of more than 980 MPa. The final structural parts have a yield strength of more than 980 MPa, an elongation after fracture of not less than 16%, an impact KV2 of more than 120 J at -20°C, and good matching of strength and toughness. The hot pressing forming and tempering heat treatment process window proposed by the present invention is relatively wide, has strong operability, and can be used in marine engineering, shipbuilding, mechanical engineering and other fields.

[0103] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for hot processing of thick 980MPa ultra-high strength steel structures. It is characterized in that The specific steps include: S1: Preheating the steel plate; heat the steel plate to 830-880℃ and keep it at 830-880℃ for a period of time t 1 ; S2: Pressing and forming the steel plate; taking the steel plate out of the heating furnace, placing it on a forming mold for pressing, and air cooling it to room temperature after forming to obtain a structural part of a certain shape; S3: Quenching treatment of structural parts; Quenching process: put the pressed structural parts into the heating furnace, heat them to 850-890℃ and keep them warm for a period of time t 2 , and then the structural parts are taken out of the furnace and water-cooled to room temperature; S4: Tempering treatment of structural parts; Tempering process: put the structural parts after quenching heat treatment into the heating furnace, heat to 560 ~ 620 ℃, keep warm at 560 ~ 620 ℃ for a period of time t 3 , and then the structural parts are taken out of the furnace and air-cooled to room temperature to obtain ultra-high strength steel structural parts with restored performance; S5: Inspection and acceptance, the mechanical properties of the structural parts meet the requirements of various indicators.

2. The hot working method of the thick 980MPa grade ultra-high strength steel structure according to claim 1, It is characterized in that In step S1, the steel plate is 10CrNi8MoV ultra-high strength steel, the alloy elements Ni+Cr+Mo in the steel plate are ≥8%, the steel plate thickness H ranges from 36 to 80 mm, the room temperature yield strength is not less than 980 MPa, the elongation after fracture is not less than 16%, and the -20°C Charpy V-notch impact absorption energy is not less than 120 J.

3. The hot working method of the thick 980MPa grade ultra-high strength steel structure according to claim 2, It is characterized in that In step S1, the steel plate is placed in a heating furnace at a temperature below 400°C and heated to a temperature between 830°C and 880°C at a rate not higher than 200°C / h.

4. The hot working method of the thick 980MPa grade ultra-high strength steel structure according to claim 1, It is characterized in that In step S1, the holding time t 1 =K 1 *H, unit: min; Where: K 1 The value range of is: 1.0~1.5; H is the thickness of the steel plate.

5. The hot working method of the thick 980MPa grade ultra-high strength steel structure according to claim 1, It is characterized in that In step S2, the initial pressing temperature of the steel plate is not less than 800°C, and the final forming temperature is not less than 700°C.

6. The hot working method of the thick 980MPa grade ultra-high strength steel structure according to claim 1, It is characterized in that In step S3, the structural component is placed in a heating furnace at a temperature below 400°C and then heated to between 850°C and 890°C at a rate not higher than 200°C / h.

7. The hot working method of the thick 980MPa grade ultra-high strength steel structure according to claim 6, It is characterized in that In step S3, the holding time t 2 =K 2 *H, unit: min; Where: K 2 The value range of is: 2.5~3.0; H is the thickness of the steel plate.

8. The hot working method of the thick 980MPa grade ultra-high strength steel structure according to claim 1, It is characterized in that In step S3, the time from when the structural parts are taken out of the furnace to when they are put into the water is no more than 3.0 minutes, and the water temperature in the water tank is no higher than 40° C. during the cooling process.

9. The hot working method of a thick 980MPa grade ultra-high strength steel structure according to claim 1, It is characterized in that In step S4, the structural component is placed in a heating furnace at a temperature below 400°C and then heated to between 560°C and 620°C at a rate not higher than 200°C / h.

10. The hot working method of the thick 980MPa grade ultra-high strength steel structure according to claim 9, It is characterized in that In step S4, the holding time t 3 =K 3 *H, unit: min; Where: K 3 The value range of is: 4.5~5.0; H is the thickness of the steel plate.

Citation Information

Patent Citations

  • Manufacturing process of high-strength steel large-diameter thick-walled tees

    CN102284671A

  • Hot press molding method for spherical head made of 10CrNi3MoV steel

    CN105256116A

  • Heat treatment method for reducing yield ratio of ultrahigh-strength maritime work steel EH890

    CN114058793A

  • High-alloy Cr-Ni-Mo-V steel hollow part grain refinement method

    CN115874029A

  • Low-yield-ratio ultra-high-strength high-toughness steel for pressure hulls and preparation method therefor

    US20220002849A1

Cited By

  • Stainless steel plate forming method

    CN120169947A