Forming process for rolling ring with special-shaped end face
Through the end-face special-shaped ring forming process, the follow-up point control and calculation method of the tapered roller are used to solve the problems of long processing time and high cost in the traditional ring forging forming method, and the efficient forming and performance improvement of the ring parts are achieved.
Patent Information
- Application Number
- CN202411160012.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
AI Technical Summary
The traditional ring forging forming method is based on the maximum size of wall thickness and height during processing, resulting in long processing time, low production efficiency and high cost, and failure to effectively consider the complexity of the final cross-section shape.
The end-face special-shaped roller ring forming process is adopted, including cutting, pre-forging, upsetting, punching, pre-rolling and final rolling. Through the follow-up point control of the tapered roller, the different formation of the ring parts is gradually realized, reducing material input and Processing time, and the reasonable configuration of the diameter-axial rolling ratio of the ring parts is ensured through calculation methods, and the forging permeability and material performance are improved.
It shortens processing time, reduces raw material usage, improves the performance and service life of forgings, ensures uniform deformation and stress of the ring parts during the rolling process, refines the grain structure, and improves the material performance.
Smart Images

Figure CN119016648A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal forging and forming, and in particular to a process for forming an end face profiled rolling ring. Background Art
[0002] Ring forgings generally refer to forged parts with a ring-like appearance. For example, in the fields of energy and heavy machinery, they are used as key components for wind turbines, large compressors, oil drilling equipment, etc.; in the fields of automobiles and rail transportation, they are used to manufacture important components of engines, transmissions, and brake systems; and in the aerospace field, they are used for key components of aircraft and rocket engines, such as turbine discs, blades, casings, etc.
[0003] With the development of industrial equipment manufacturing technology, the requirements for parts are getting higher and higher. The shape of equipment parts needs to be specially designed according to actual requirements, and the cross-sectional shape of rings is becoming more and more complex. At present, the forming method for special-shaped ring forgings is: first, the raw materials are forged into blanks, and then the rings are rolled into rectangular rings. Then, the excess materials are turned off in the machining process to obtain the target rings. The traditional manufacturing method does not consider the final cross-sectional shape of the rings. The rectangular cross-sectional rings are rolled based on the maximum dimensions of wall thickness and height. The turning amount in the machining process is large, the processing time is long, the production efficiency is low, and the production cost is high.
[0004] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention discloses a process for forming an end face special-shaped ring rolling.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A process for forming an end face profiled ring rolling comprises the following steps:
[0008] Step S1, blanking;
[0009] Step S2, heating the blank before forging;
[0010] Step S3, upsetting the blank;
[0011] Step S4, punching, using a punch to punch a hole in the center of the blank, and obtaining a ring-shaped blank after punching;
[0012] Step S5, pre-rolling at one station, a first station is provided at the front side of the cone roller, and the ring blank is pre-rolled at the first station at the front side of the cone roller, the surface of the first station is smooth and has no grooves, a cone roller follower point A is provided at the first station, and during the rolling process, the cone roller completes the pre-rolling of the ring blank based on the follower point A to obtain a rectangular cross-section ring;
[0013] Step S6, second-station final rolling, the tapered roller is provided with a second station located at the rear side of the first station, the second station is provided with a groove, and a tapered roller follower point B is provided at the edge of the second station. During the rolling process, the tapered roller rolls the special-shaped ring based on the follower point B, and finally obtains a special-section ring with end face profiling.
[0014] Furthermore, in step S2, the blank is heated to the initial forging temperature of the material before forging.
[0015] Furthermore, in step S2, the blank is fully kept warm at the initial forging temperature.
[0016] Further, in step S3, the height of the blank before upsetting is recorded as H0, the height of the blank after upsetting is set to H1, and the upsetting forging ratio λ1=H0 / H1≥3.0.
[0017] Further, in step S5, the outer diameter D1, inner diameter d1, and height H1 of the ring blank before pre-rolling satisfy the following calculation relationship:
[0018] Among them, D2, d2, and H2 are the outer diameter, inner diameter, and height of the rectangular cross-section ring after pre-rolling, respectively; k1 is the rolling coefficient in the pre-rolling stage, 0.75≤k1≤1, and the larger the k1, the larger the ratio of the height to the wall thickness of the blank; V3 is the volume of the preset special-shaped ring, which is calculated using 3D modeling software according to the size of the target forging.
[0019] Further, in step S5, the outer diameter D2, inner diameter d2 and height H2 of the rectangular cross-section ring after pre-rolling satisfy the following calculation relationship:
[0020]
[0021] Among them, k2 is the rolling coefficient in the final rolling stage, 1≤k2≤1.2, and the larger k2 is, the greater the ratio of the height of the ring at the end of pre-rolling to the wall thickness is; k3 is the filling coefficient of the tapered roller, 1.5≤k3≤2.5; H4 is the depth of the groove of the special-shaped tapered roller rolling.
[0022] Furthermore, in step S6, the ring forging ratio λ2 of the final rolling=the cross-sectional area S1 of the billet ring / the cross-sectional area S2 of the special-shaped ring after the final rolling, and the ring forging ratio λ2≥2.5.
[0023] Furthermore, in step S5, the linear velocity of the main roller is v 主辊 =k4*D3(mm / s), k4 is the control coefficient of the main roller linear speed 0.15≤k4≤0.35, the outer diameter of the ring is v 环增速1 =k5*10 -3*D3 (mm / s), k5 is the control coefficient of the ring speed increase in the pre-rolling stage of a workstation 2.0≤k5≤3.5.
[0024] Furthermore, in step S6, the linear velocity of the main roller is v 主辊 =k4*D3(mm / s), k4 is the control coefficient of the main roller linear speed 0.15≤k4≤0.35, the outer diameter of the ring is v 环增速2 =k6*10 -3 *D3 (mm / s), k6 is the control coefficient of the ring speed increase in the final rolling stage of the second station, 1.5≤k6≤2.5.
[0025] The beneficial effects of the present invention are as follows:
[0026] 1. In the one-station pre-rolling, the first station of the tapered roller contacts the ring blank, further expanding the ring blank and approaching the designed pre-rolling size. Then the outer diameter of the ring continues to grow to the second station of the tapered roller, and the end face of the ring is step-rolled. The final rolling of the end face special-shaped ring is completed in one pass. The end face profiled special-shaped ring reduces the input of raw materials and shortens the processing time of the machining process.
[0027] 2. The method for calculating the billet size given in the present invention can ensure the reasonable configuration of the ring diameter-axial rolling ratio, ensure the uniform deformation and stress of the ring during the ring rolling process, improve the forgeability, refine the grain structure, and improve the internal defects of the material. In the two-station final rolling process, the pre-rolled ring size calculated according to the present invention can ensure the good filling of the end face profiling ring and the stability of the ring rolling process.
[0028] 3. Use the forging scheme of end face profiling to make the forging have more complete metal streamlines, avoid cutting metal streamlines in machining process, improve product performance and service life. The profiling step surface has a larger rolling ratio, which is conducive to grain refinement and improved material properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the steps of a process for forming a special-shaped end face ring rolling.
[0030] Figure 2 Schematic diagram of the blank state after punching.
[0031] Figure 3 This is a schematic diagram of the initial state of a pre-rolled ring forging at a workstation.
[0032] Figure 4 This is a schematic diagram of the final state of a pre-rolled ring forging at a workstation.
[0033] Figure 5 This is a schematic diagram of the initial state of the two-station final rolled ring forging.
[0034] Figure 6 This is a schematic diagram of the final state of the two-station final rolling ring forging.
[0035] Figure 7 This is a schematic diagram of the final state of the second-station final rolled ring forging in Example 2.
[0036] Figure 8 This is a schematic diagram of the final state of the second-station final rolled ring forging in Example 3.
[0037] Fig. 9 This is the end face metallographic image of the end face special-shaped ring component of Example 1.
[0038] Fig.10 This is the metallographic image of the end face of the rectangular ring of comparative example 1.
[0039] In the figure: 1, cone roller; 11, first station; 12, second station. DETAILED DESCRIPTION
[0040] The specific implementation of the present invention will be described below in conjunction with the accompanying drawings.
[0041] Embodiment 1:
[0042] A process for forming end face profiled rings, such as Figure 1 As shown, the following steps are included:
[0043] Step S1, blanking, the raw material grade is S355NL, the size is The weight is 4832kg.
[0044] Step S2, heating the billet before forging, heating the billet to the material starting forging temperature and fully keeping the temperature. In this embodiment, the billet is heated to a temperature of 1250°C, and the holding time range is (t, t+1) hours, where t = continuous casting round billet diameter / 100, and the holding time in this embodiment is specifically t = 7.
[0045] Step S3, upsetting the blank, the height of the blank before upsetting is recorded as H0=1599 mm, the height of the blank after upsetting is H1=400.73 mm, and the upsetting forging ratio λ1=H0 / H1=3.99≥3.0.
[0046] Step S4: punching, such as Figure 2 As shown, a punch is used to punch a hole in the center of the blank, and a ring-shaped blank is obtained after punching. The punch diameter is reasonably selected according to the weight of the blank. In this example, the punch diameter of the blank is After punching, the blank size is outer diameter D1, inner diameter d1 and height H1. The blank size calculation formula is as follows:
[0047]
[0048] Wherein, k1 is the rolling coefficient in the pre-rolling stage, 0.75≤k1≤1, the larger the k1, the larger the ratio of the height of the blank to the wall thickness, in this embodiment, k1=0.75; V3 is the volume of the target special-shaped ring forging, obtained by UG three-dimensional software modeling and calculation, V3=582783045.97mm 3 ; The specific dimensions of the blank are calculated to be D1=1421.18mm, d1=410mm, H1=400.73mm.
[0049] Step S5, pre-rolling at a station, such as Figure 3 , 4 As shown, a first station 11 is provided in front of the cone roller 1, and the ring blank is pre-rolled by the first station 11 in front of the cone roller 1. The surface of the first station 11 is smooth and has no grooves. A cone roller follower point A is provided at the first station 11. During the rolling process, the outer diameter of the blank gradually increases under the extrusion of the roller. When the outer diameter of the ring grows to align with the cone roller follower point A, the cone roller 1 moves backward, and the retreat speed of the cone roller 1 is consistent with the growth speed of the outer diameter of the ring. The cone roller 1 completes the pre-rolling of the ring blank based on the follower point A to obtain a rectangular cross-section ring. The outer diameter D2, inner diameter d2, and height H2 of the rectangular cross-section ring after pre-rolling satisfy the following calculation relationship:
[0050]
[0051] Among them, k2 is the rolling coefficient in the final rolling stage, 1≤k2≤1.2, the larger the k2 is, the larger the ratio of the height to the wall thickness of the ring after pre-rolling is; k3 is the filling coefficient of the tapered roller, 1.5≤k3≤2.5; H4 is the depth of the special-shaped tapered roller rolling groove, according to the specific dimensions of the special-shaped cross-section ring pre-designed in this embodiment, the outer diameter D3=4332mm, the inner diameter d3=3838mm, and the height H3=213mm, in this embodiment, k2=1.1, k3=2, H4=43, and the specific dimensions of the rectangular cross-section ring after pre-rolling are calculated to be D2=2189.49mm and the inner diameter d2=1520.59mm.
[0052] Among them, the linear speed of the main roller is v 主辊 =k4*D3(mm / s), k4 is the control coefficient of the main roller linear speed 0.15≤k4≤0.35, the outer diameter of the ring is v 环增速1 =k5*10 -3 *D3 (mm / s), k5 is the control coefficient of the ring speed increase in the pre-rolling stage of a station 2.0≤k5≤3.5. In this embodiment, D3=4332mm, k4=0.23, k5=2.7, and finally calculated that the main roller linear speed is 996mm / s, and the ring outer diameter ring speed increase is 12mm / s.
[0053] Step S6, second station final rolling, such as Figure 5 ,6 As shown, the cone roller 1 is provided with a second station 22 located at the rear side of the first station 11, and a groove is provided on the second station 22. In this embodiment, the cone roller follower point B is set at the inflection point position on the rear side of the bottom of the groove (the cone roller follower point B can be adjusted accordingly according to the design shape of the formed special-section ring). During the final rolling process of the second station, the outer diameter of the rectangular cross-section ring that has finished pre-rolling continues to grow under the extrusion of the roller. At this time, the follower point of the cone roller 1 will automatically switch to the follower point B under the control of the rolling program. When the outer diameter of the ring grows to align with the cone roller follower point B, the cone roller 1 moves backward, and the retreat speed of the cone roller 1 is consistent with the growth speed of the outer diameter of the ring. The cone roller 1 rolls the special-shaped ring based on the follower point B, and finally obtains a special-section ring with end face profiling. The specific dimensions of the special-section ring are outer diameter D3 = 4332mm, inner diameter d3 = 3838mm, and height H3 = 213mm.
[0054] Among them, the linear speed of the main roller is v 主辊 =k4*D3(mm / s), k4 is the control coefficient of the main roller linear speed 0.15≤k4≤0.35, the outer diameter of the ring is v 环增速2 =k6*10 -3 *D3 (mm / s), k6 is the control coefficient of the ring speed increase in the second station final rolling stage 1.5≤k6≤2.5. In this embodiment, D3=4332mm, k4=0.23, k6=1.7, and the final calculation shows that the main roller linear speed is 996mm / s and the ring outer diameter ring speed increase is 7mm / s.
[0055] The final rolling temperature of the billet is ≥850°C, and the ring rolling forging ratio λ2=the cross-sectional area of the billet ring S1 / the cross-sectional area of the final rolled special-shaped ring S2=202200 / 45274=4.5≥3.5.
[0056] Embodiment 2:
[0057] The difference from Example 1 is:
[0058] Step S6, second station final rolling, such as Figure 7 As shown, the cone roller 1 is provided with a second station 22 located at the rear side of the first station 11, and a groove is provided on the second station 22. In this embodiment, the cone roller follower point B is set at the edge position outside the cone roller groove. Similarly, when the outer diameter of the ring grows to align with the cone roller follower point B, the cone roller 1 moves backward, and the retreat speed of the cone roller 1 is consistent with the growth speed of the outer diameter of the ring. Finally, a flange forging with a T-shaped cross-sectional shape is obtained.
[0059] Embodiment 3:
[0060] The difference from Example 1 is:
[0061] Step S6, second station final rolling, such as Figure 8 As shown, the cone roller 1 is provided with a second station 22 located at the rear side of the first station 11, and a groove is provided on the second station 22. In this embodiment, the cone roller follower point B is set at the edge position outside the cone roller groove, and the cone roller follower point B is far away from the groove. Similarly, when the outer diameter of the ring grows to align with the cone roller follower point B, the cone roller 1 moves backward, and the retreat speed of the cone roller 1 is consistent with the growth speed of the outer diameter of the ring. Finally, the cross-sectional shape of the flange forging is L-shaped.
[0062] Comparative Example 1:
[0063] The same target product as in Example 1 was produced by adopting the process scheme of upsetting, punching and rectangular ring rolling. In the process of rectangular ring rolling, a ring forging with a rectangular cross-sectional shape is rolled by a rolling mill, and then the excess on the upper end face of the ring forging is removed by lathe processing to obtain a flange with the same cross-sectional shape as the designed one. The dimensions of the ring forging are D3=4332mm, d3=3838mm, and H3=213mm. The weight of the raw material is 5579kg, and the product production cycle is 75.3h.
[0064] Compared with Example 1, the raw material consumption is 4832 kg, saving 747 kg of raw materials; compared with Example 1, the product production cycle is 69.8 hours, shortening the product production cycle by 5.5 hours.
[0065] Parts performance testing:
[0066] The products of Example 1 and Comparative Example 1 were subjected to room temperature stretching, low temperature impact and grain size detection after end face sampling. The detection method for room temperature stretching is ISO 6892-1:2019, and the inspection equipment is a CMT5205 microcomputer-controlled electronic universal testing machine; the detection method for low temperature impact is ISO 148-1:2016, and the inspection equipment is a NI750 metal pendulum impact testing machine; the inspection method for grain size detection is ISO 643:2019, and the inspection equipment is a German Zeiss AXIO Observer metallographic microscope. Table 1 below shows the test results of room temperature stretching and low temperature impact of the product. The tensile strength, upper yield strength and elongation after fracture of Example 1 are slightly better than those of the rectangular ring rolling scheme of Comparative Example 1, and the impact absorption energy of low temperature impact of Example 1 is higher than that of Comparative Example 1. Fig. 9 This is the metallographic image of the end face of the special-shaped ring of Example 1. Fig.10 The metallographic image of the end face of the rectangular ring of comparative example 1. The grain size of the end face of the special-shaped ring produced in Example 1 is level 10, and the grain size of the end face of the rectangular ring produced in comparative example 1 is level 9. In summary, the special-shaped ring rolling process using step surface profiling has a larger rolling ratio. During the rolling deformation of the forging, the organization is fully deformed, the coarse-grained organization is fully broken, the grains are fine and uniform, the grains are refined, and the mechanical properties are improved at the macro level.
[0067] Table 1 Comparison of physical and chemical properties
[0068]
[0069] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0070] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A process for forming end face profiled ring rolling, characterized in that: The following steps are involved: Step S1, blanking; Step S2, heating the blank before forging; Step S3, upsetting the blank; Step S4, punching, using a punch to punch a hole in the center of the blank, and obtaining a ring-shaped blank after punching; Step S5, pre-rolling at one station, a first station is provided at the front side of the cone roller, and the ring blank is pre-rolled at the first station at the front side of the cone roller, the surface of the first station is smooth and has no grooves, a cone roller follower point A is provided at the first station, and during the rolling process, the cone roller completes the pre-rolling of the ring blank based on the follower point A to obtain a rectangular cross-section ring; Step S6, second-station final rolling, the tapered roller is provided with a second station located at the rear side of the first station, the second station is provided with a groove, and a tapered roller follower point B is provided at the edge of the second station. During the rolling process, the tapered roller rolls the special-shaped ring based on the follower point B, and finally obtains a special-section ring with end face profiling.
2. The process for forming end face profiled ring rolling according to claim 1, characterized in that: In step S2, the blank is heated to the initial forging temperature of the material before forging.
3. The process for forming end face profiled ring rolling according to claim 2 is characterized in that: In step S2, the blank is sufficiently kept warm at the initial forging temperature.
4. The process for forming end face profiled ring rolling according to claim 1, characterized in that: In step S3, the height of the blank before upsetting is recorded as H0, and the height of the blank after upsetting is set to H1, and the upsetting forging ratio λ1=H0 / H1≥3.
0.
5. The process for forming end face profiled ring rolling according to claim 4 is characterized in that: In step S5, the outer diameter D1, inner diameter d1, and height H1 of the ring blank before pre-rolling satisfy the following calculation relationship: Among them, D2, d2, and H2 are the outer diameter, inner diameter, and height of the rectangular cross-section ring after pre-rolling, respectively; k1 is the rolling coefficient in the pre-rolling stage, 0.75≤k1≤1, and the larger the k1, the larger the ratio of the height to the wall thickness of the blank; V3 is the volume of the preset special-shaped ring, which is calculated using 3D modeling software according to the size of the target forging.
6. The process for forming end face profiled ring rolling according to claim 5, characterized in that: In step S5, the outer diameter D2, inner diameter d2 and height H2 of the pre-rolled rectangular cross-section ring satisfy the following calculation relationship: Among them, k2 is the rolling coefficient in the final rolling stage, 1≤k2≤1.2, and the larger k2 is, the greater the ratio of the height of the ring at the end of pre-rolling to the wall thickness is; k3 is the filling coefficient of the tapered roller, 1.5≤k3≤2.5; H4 is the depth of the groove of the special-shaped tapered roller rolling.
7. The process for forming end face profiled ring rolling according to claim 6, characterized in that: In step S6, the ring forging ratio λ2 of the final rolling is equal to the cross-sectional area S1 of the billet ring / the cross-sectional area S2 of the special-shaped ring after the final rolling, and the ring forging ratio λ2 is ≥ 2.
5.
8. The process for forming end face profiled ring rolling according to claim 7 is characterized in that: In step S5, the main roller linear velocity is v 主辊 =k4*D3(mm / s), k4 is the control coefficient of the main roller linear speed 0.15≤k4≤0.35, the outer diameter of the ring is v 环增速1 =k5*10 -3 *D3 (mm / s), k5 is the control coefficient of the ring speed increase in the pre-rolling stage of a workstation 2.0≤k5≤3.
5.
9. The process for forming end face profiled ring rolling according to claim 8, characterized in that: In step S6, the main roller linear velocity is v 主辊 =k4*D3(mm / s), k4 is the control coefficient of the main roller linear speed 0.15≤k4≤0.35, the outer diameter of the ring is v 环增速2 =k6*10 -3 *D3 (mm / s), k6 is the control coefficient of the ring speed increase in the final rolling stage of the second station, 1.5≤k6≤2.5.
Citation Information
Patent Citations
Integral forming method for axial special-shaped ring forge piece
CN115430801A
Preparation method of wind power tower drum flange
CN116213638A
Forming method for rolling ring with special-shaped inner diameter
CN117600368A
Special-shaped ring piece rolling device
CN213671625U
Method for producing a contoured ring rolling product
EP3328572A1