Method for reducing steel material consumption in whole continuous casting process

By adopting countdown meter control, long-life submersible sprue, optimized stop-cast tail billet control, and stopper rod dual control system during continuous casting, the problem of high steel material consumption was solved, resulting in reduced production costs and improved efficiency.

CN119016698APending Publication Date: 2024-11-26YANGCHUN NEW STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411032038.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In existing technologies, steel consumption is high during continuous casting, leading to increased production costs and reduced corporate profits.

Method used

The countdown meter control during water inlet replacement is implemented using automated equipment, long-life submersible water inlets are used, the control of the tail billet stoppage is optimized, a stopper rod dual control system is applied, and the slide plate aperture of the molten steel ladle is improved to reduce steel slag mixing.

Benefits of technology

It effectively reduced steel consumption, improved production efficiency and metal recovery, and lowered production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016698A_ABST
    Figure CN119016698A_ABST
Patent Text Reader

Abstract

According to the method, in the continuous casting process, when the end of a current casting blank runs to the position away from the cutting position of a flame cutting machine by a certain distance, a collector nozzle is replaced, and at the moment, the length of the casting blank meets the formula of n * L1 + x, L1 is the fixed length, n is a positive integer, and x is 1 m. It is guaranteed that the length of the cut casting blank meets the requirement, the waste blank is accurately cut when the collector nozzle is replaced, and the number of waste blanks is prevented from being increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to steelmaking continuous casting, and specifically relates to a method for reducing steel material consumption in the entire continuous casting process. Background Art

[0002] Steel material consumption has always been the most critical indicator related to the benefits of steel companies and reducing their product costs. Reducing the consumption of continuous casting steel materials and increasing the continuous casting metal recovery rate can improve the benefits of steel companies and reduce production costs, thereby maximizing benefits. Continuous casting can reduce process water nozzle waste, tail waste from stopping pouring in the middle package, and slag turnover in large tanks by controlling production accidents, using automated programs to ensure accurate control of fixed-length water nozzles, and coordinating with water nozzle contractors to improve water nozzle quality under high casting speed conditions. This can turn limited molten steel into qualified ingots while ensuring quality. This will increase qualified output, reduce the cost per ton of steel, improve the company's production efficiency, and increase the company's competitiveness in the same industry. Summary of the invention

[0003] The present invention adopts a method for reducing steel material consumption in the entire continuous casting process.

[0004] Specifically, a method for reducing steel consumption in the entire continuous casting process. In the continuous casting process, when the end of the secondary ingot runs to a certain distance from the cutting position of the fire cutting machine, the water inlet is replaced. At this time, the length of the ingot satisfies: n*L1+x, L1 is the fixed length, n is a positive integer, and x is 1m.

[0005] In one embodiment, when the end of the secondary ingot runs to 9.2m away from the cutting position of the flame cutting machine, the water outlet is replaced. At this time, the length of the ingot meets the length of three qualified 11.5m fixed ingots and the length of 1m scrap ingot.

[0006] The present invention adopts automatic equipment to control the actual countdown number of meters when changing the water outlet, realizes accurate cutting when changing the water outlet, and effectively avoids the problem of excessive waste control when changing the drain outlet.

[0007] Furthermore, the drain port of the tundish adopts a long-life immersion drain port with a service life of ≥14h, thereby reducing the number of times the drain port is replaced.

[0008] Furthermore, the tail billet is controlled to be stopped, and the slag is discharged from the ladle of the previous furnace before the stop pouring. The temperature of the ladle of the stop pouring furnace is controlled at 1523-1530℃ to avoid the reduction of molten steel fluidity or the occurrence of slag rolling. In one embodiment, the edge flow is stopped first. When the liquid level in the ladle is <25t, the pulling speed is <3.5m / min; when the liquid level in the ladle is <20t, the pulling speed is <3m / min; when the liquid level in the ladle is <15t, the pulling speed is <2.5m / min; when the liquid level in the ladle is <10t, the pulling speed is <2m / min. According to the flow situation, S1 and S5 flows are stopped first, then S2 and S4 flows, and finally S3 flow is stopped to reduce the amount of molten steel remaining in the ladle as much as possible. The casting is stopped according to the fixed length of each flow, and the tail length is controlled within 2m. The pulling speed of the tail billet after the casting is stopped is controlled at 2.5-3m / min to avoid shrinkage holes being judged as scrap.

[0009] Furthermore, the stopper rod dual control system controls the change of stopper rod flow control and the pulling speed of the straightening machine. Under the condition of meeting the production demand, the stopper rod and the straightening machine control the liquid level of the crystallizer together. Specifically, the stopper rod control potentiometer is added to adjust or control the input to set the pulling speed. When the set pulling speed is compared with the actual pulling speed in a fixed period, the pull speed automatic control logic stopper rod opening is executed in a fixed period to control the liquid level, thereby ensuring the stability of the molten steel level in the crystallizer. When the difference between the actual liquid level and the set liquid level is less than 0.5mm, the original pulling speed is kept unchanged. When the actual liquid level is higher than the setting by 0.5mm, the pulling speed is increased. When the actual liquid level is lower than the setting by 0.5mm, the pulling speed is reduced. In a stable state, the stopper rod does not need to frequently move up and down to control the flow rate. The straightening machine slightly adjusts the pulling speed at the set pulling speed to stabilize the liquid level of the crystallizer. Under the control of the stopper rod dual control system, the stopper rod erosion rate can be effectively reduced.

[0010] Furthermore, the aperture of the slide plate of the steel ladle is modified, that is, the aperture of the slide plate is reduced to reduce the vortex generated at the water inlet of the steel ladle when the remaining molten steel is small at the end of pouring, causing the slag mixing to intensify. At the same time, the maintenance of the steel ladle base bricks is strengthened to reduce the concave area formed by the bottom being washed out, resulting in the molten steel not flowing cleanly. Specifically, the use standard of the steel ladle base bricks is formulated. When the lowest point of the base brick differs from the upper mouth of the steel ladle by more than 30mm, the base bricks at the bottom of the steel ladle need to be replaced.

[0011] In order to reduce the consumption of steel materials in continuous casting, the present invention adjusts the material of the immersion nozzle to extend the service life of the nozzle to more than 14 hours, thereby reducing the generation of waste billets due to frequent replacement of the nozzle; by using an encoder to count down the number of meters of the nozzle replacement, it is ensured that the length of the billet after cutting meets the requirements and the waste billet is accurately cut after replacing the nozzle, thereby avoiding increasing the number of waste billets; a stopper rod dual control system is developed to reduce the erosion of refractory materials in the tundish and increase the number of continuous casting furnaces of the tundish; the aperture of the slide plate of the molten steel tank is improved to reduce the slag from carrying away the molten steel. The above measures jointly promote the reduction of steel material consumption in continuous casting production, further improve production efficiency, and reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a schematic diagram of the cutting length of the ingot. DETAILED DESCRIPTION

[0013] The present invention will be further described below in conjunction with specific embodiments.

[0014] The method of reducing steel consumption in the whole process of continuous casting is achieved through the following measures in the continuous casting process:

[0015] 1. Reduce the length of billet waste when replacing the drain

[0016] The tundish is a refractory container used in short-process steelmaking and continuous casting, located between the ladle and the crystallizer. The tundish first receives the molten steel poured from the ladle, and then distributes and injects it into each crystallizer through the tundish drain port. The tundish drain port has a service life requirement, so the drain port must be replaced during the casting process to meet normal production requirements. However, the length and time of replacing the drain port directly affect the length of the waste billet when replacing the drain port. In this embodiment, the drain port is replaced when the end of the billet runs to a certain distance from the cutting position of the fire cutting machine. At this time, the length of the billet satisfies: n*L1+x, L1 is the fixed length, n is a positive integer, and x is 1m.

[0017] The length of the crystallizer liquid surface from the cutting machine to the fire cutter is 25.9m. Taking the 11.5m fixed length as an example, the end of the billet runs to 9.2m from the cutting position of the fire cutter. At this time, the length of the billet satisfies: 3*L1+1m, that is, the length of three qualified 11.5m fixed length billets and the length of 1m scrap billets are met. The length of the crystallizer liquid surface from the fire cutter gun position is 25.90m. According to the fixed length of the billet cutting of 11.65m, the encoder length runs to 9.10m as the cutting point for the third billet. After on-site verification, when the billet is at a position of about 9.20m and the countdown meter display is 0, the billet encoder runs to the 9.2m position, see Figure 1 .

[0018] When the cold billet length is 11.5m, the countdown meter display on the table returns to 0m. At this time, the stopper rod is closed and the nozzle is replaced. After the fire cutting machine cuts three billets according to the fixed length, the reconnection point is 1.05m away from the head in front of the fourth billet. The cold billet length is 11.5cm, the hot billet length is 11.65cm, and the shrinkage rate is 1.013, because the billet has thermal expansion and contraction.

[0019] Of course, in this embodiment, automated equipment is used to control the actual countdown number of meters when changing the water outlet, so as to achieve precise cutting when changing the water outlet, and effectively avoid the problem of excessive waste control when changing the drain outlet.

[0020] The pouring process, for example, one pouring time is 28 hours, if the drain outlet is replaced after 14 hours, it can be understood as replacing the drain outlet during the pouring process.

[0021] 2. Improve the life of the drain

[0022] With the development of steelmaking continuous casting technology, the submerged nozzle has also made great progress. The structure and material of the submerged nozzle are constantly improving, playing a decisive role in increasing production and improving steel quality. The submerged nozzle is located between the tundish and the crystallizer in the continuous casting process. It is a guide pipe for molten steel to flow from the tundish to the crystallizer. Its function is to prevent secondary oxidation of molten steel; control the flow state and injection speed of molten steel; promote the floating of inclusions and prevent non-metallic inclusions of protective slag from being drawn into the molten steel. The submerged nozzle is one of the most important functional refractory components in the continuous casting process, and its service life determines the number of furnaces for multi-furnace continuous casting. Therefore, a long-life submerged nozzle should be used.

[0023] The long-life immersion downspout is made by the following method: 40 parts of zirconium oxide particles, 30 parts of zirconium oxide fine powder, 5 parts of zirconium oxide micropowder, 3 parts of metal powder additive, 5 parts of binder and 2 parts of zirconium oxide fiber are weighed in proportion, the above raw materials are mixed and granulated, and the granulated material is compounded on the outer wall of the slag line of the downspout, isostatically pressed into a green body, and fired at 800-1000°C to obtain a finished product.

[0024] Effectively improve the corrosion resistance and thermal shock resistance, reduce the outer diameter erosion rate, thereby increasing the service life of the immersion drain, which can be up to ≥14h. During the process, the drain replacement is reduced from 15 times / pouring to 5 times / pouring.

[0025] 3. Control of the tail billet after stopping pouring

[0026] In order to better control the tail billet after stopping pouring, it is required to discharge slag in the tundish of the previous furnace before stopping pouring, and the temperature of the tundish of the stopping furnace is controlled at 1523-1530℃ to avoid the decrease of molten steel fluidity or the occurrence of slag curling. Considering the deformation of the tundish, the edge flow is stopped first. When the liquid level of the tundish is <25t, the pulling speed is <3.5m / min; when the liquid level of the tundish is <20t, the pulling speed is <3m / min; when the liquid level of the tundish is <15t, the pulling speed is <2.5m / min; when the liquid level of the tundish is <10t, the pulling speed is <2m / min. According to the flow situation, S1 and S5 flows are stopped first, then S2 and S4 flows, and finally S3 flow is stopped to reduce the amount of residual molten steel in the tundish as much as possible. Each flow is stopped according to the fixed length, the tail length is controlled within 2m, and the pulling speed of the tail billet after stopping pouring is controlled at 2.5-3m / min to avoid shrinkage. The casting machine is divided into five flows, and the above S1-S5 flows represent the 1st to 5th flows respectively.

[0027] 4. Process waste control

[0028] The life of the tundish lining and the number of continuous casting furnaces are important economic and technical indicators for measuring the production capacity of the continuous casting machine. By increasing the life of the tundish lining and the number of continuous casting furnaces, it is possible to not only stabilize the production rhythm of the steelmaking process, effectively improve the operating rate of the continuous casting machine, and reduce the number of tundish replacements, but also reduce the refractory cost and the steel-out temperature in front of the furnace, and improve the metal recovery rate.

[0029] The working principle of the stopper mechanism is that after the electric cylinder receives the command from the controller, it drives the mechanism to execute the switch movement. The position sensor in the electric cylinder transmits the current stopper position to the control system in time, and the control system determines the stopper position to execute opening or closing according to the liquid level of the product finisher. After completing a switch, the position sensor transmits the position to the control system again, and then determines the stopper switch according to the liquid level, and repeats this cycle until the molten steel level in the product finisher reaches the set value. However, the current on-site tracking found that the use of the original automatic control method of the crystallizer stopper, the frequent stopper jitters have a great impact on the sensitivity of the electric cylinder, the wear of the stopper mechanism, and the erosion of the stopper tip, which not only greatly reduces the service life of the electric cylinder and the stopper mechanism, but also causes production accidents due to the loosening of the bolts of the stopper mechanism and the stopper body due to the high-frequency jitter. In addition, the frequency of stopper loss of control caused by the erosion of the stopper due to the molten steel scouring caused by the jitter of the stopper is also very high.

[0030] In this embodiment, the stopper rod dual control system is adopted to realize the automatic and precise control of the crystallizer stopper rod. At the same time, the stopper rod control potentiometer is added to the post operation panel to adjust or control the input to set the pulling speed. When the set pulling speed is compared with the actual pulling speed in a fixed period, the automatic pulling speed control logic stopper rod opening is executed in a fixed period to control the liquid level, thereby ensuring the stability of the molten steel level in the crystallizer. If the difference between the actual liquid level and the set liquid level is less than 0.5mm, the original pulling speed is kept unchanged. If the actual liquid level is higher than the setting 0.5mm, the pulling speed is increased. If the actual liquid level is lower than the setting 0.5mm, the pulling speed is reduced. The original method of controlling the liquid level in the crystallizer is changed to a method of realizing dual-range control of a single stopper rod liquid level automatic control and a pulling speed automatic control. This method not only solves the equipment loss caused by the high-frequency jitter of the original stopper rod automatic control, but also reduces the problems of crystallizer liquid level fluctuation and stopper rod erosion during the production process. It also solves the problem of billet running away in the crystallizer due to the sudden interruption of the injection flow in the tundish during the production process. It effectively reduces the instability of the crystallizer liquid level at high pulling speeds and the occurrence of steel leakage accidents caused by serious loss of control of stopper rod erosion at the end of pouring. However, since the stopper rod is basically in an inactive state in the stopper rod dual control system, molten steel is prone to crusting around the stopper rod in the tundish, causing the stopper rod to fail to move normally.

[0031] The stopper rod dual control system is used to control the change of stopper rod flow control and the pulling speed of the straightening machine. Under the condition of meeting the production demand, the stopper rod and the straightening machine control the liquid level of the crystallizer together. In a stable state, the stopper rod does not need to frequently move up and down to control the flow rate. The straightening machine slightly adjusts the pulling speed at the set pulling speed to stabilize the liquid level of the crystallizer. Under the control of the stopper rod dual control system, the erosion rate of the stopper rod can be effectively reduced. The number of continuous casting furnaces is increased from 35 to 45, the number of pouring starts is reduced by more than 10 per month, and 100 tons of scrap is saved per month.

[0032] 5. Reduce the excess of steel ladle

[0033] For example, if the total weight of molten steel is 120 tons, including 118 tons of pure molten steel and 2 tons of slag, only 117 tons of molten steel are actually produced. The final 2 tons of slag + 1 ton of molten steel is actually a mixture of steel slag. The ultimate goal is to reduce the mixing of steel slag with molten steel.

[0034] The converter is the process of smelting molten iron into molten steel with the required composition, temperature and quality of the steel grade. During this process, materials need to be added to participate in the reaction, resulting in the presence of some slag in addition to the molten steel. However, if the slag and molten steel are not separated well, the slag will easily be brought out of the molten steel, thus affecting the molten steel yield.

[0035] In this embodiment, the aperture of the slide plate of the steel ladle is modified, that is, the aperture of the slide plate is reduced to reduce the vortex generated at the water inlet of the steel ladle when the remaining molten steel is small at the end of pouring, causing the slag mixing to intensify. At the same time, the maintenance of the steel ladle seat bricks is strengthened to reduce the concave area formed by the bottom being washed out, resulting in the molten steel not flowing cleanly. Specifically, the use standard of the steel ladle seat bricks is formulated. When the lowest point of the steel ladle seat bricks differs from the upper mouth of the steel ladle by more than 30mm, the steel ladle bottom seat bricks need to be replaced.

Claims

1. A method for reducing steel consumption in the entire continuous casting process, characterized in that: In the continuous casting process, when the end of the secondary billet runs to a certain distance from the cutting position of the fire cutting machine, the water inlet is replaced. At this time, the length of the billet satisfies: n*L1+x, L1 is the fixed length, n is a positive integer, and x is 1m.

2. The method for reducing steel consumption in the entire continuous casting process according to claim 1, characterized in that: When the end of the secondary ingot runs to 9.2m away from the cutting position of the fire cutting machine, the water outlet is replaced. At this time, the length of the ingot meets the length of three qualified 11.5m fixed-length ingots and the length of 1m ingot waste.

3. The method for reducing steel consumption in the entire continuous casting process according to claim 1 or 2, characterized in that: Use automated equipment to control the countdown in meters when changing the water outlet.

4. The method for reducing steel consumption in the entire continuous casting process according to claim 1, characterized in that: The water outlet of the tundish is a long-life immersion water outlet with a service life of ≥14h.

5. The method for reducing steel consumption in the entire continuous casting process according to claim 4 is characterized in that: The long-life immersion downspout is manufactured by the following method: 40 parts of zirconium oxide particles, 30 parts of zirconium oxide fine powder, 5 parts of zirconium oxide micropowder, 3 parts of metal powder additive, 5 parts of binder and 2 parts of zirconium oxide fiber are weighed in proportion, mixed and granulated, and then compounded on the outer wall of the slag line of the downspout, isostatically pressed into a green body, and fired at 800-1000°C.

6. The method for reducing steel consumption in the entire continuous casting process according to claim 1 or 4, characterized in that: Before stopping pouring, the slag is discharged from the middle ladle of the previous furnace, and the temperature of the middle ladle of the stopping pouring furnace is controlled at 1523-1530℃.

7. The method for reducing steel consumption in the entire continuous casting process according to claim 6, characterized in that: Stop the side flow first, when the liquid level in the tundish is <25t, the pulling speed is <3.5m / min; when the liquid level in the tundish is <20t, the pulling speed is <3m / min; when the liquid level in the tundish is <15t, the pulling speed is <2.5m / min; when the liquid level in the tundish is <10t, the pulling speed is <2m / min; according to the flow situation, stop S1 and S5 flow first, then stop S2 and S4 flow, and finally stop S3 flow to reduce the amount of residual molten steel in the tundish, stop pouring at a fixed length for each flow, control the tail length within 2m, and control the pulling speed of the tail billet at 2.5-3m / min when stopping pouring.

8. The method for reducing steel consumption in the entire continuous casting process according to claim 6, characterized in that: The stopper rod dual control system controls the change of stopper rod flow control and the pulling speed of the straightening machine. Under the condition of meeting the production demand, the stopper rod and the straightening machine control the liquid level of the crystallizer together. When the difference between the actual liquid level and the set liquid level is less than 0.5mm, the original pulling speed is kept unchanged. When the actual liquid level is higher than the set level by 0.5mm, the pulling speed is increased. When the actual liquid level is lower than the set level by 0.5mm, the pulling speed is reduced.

9. The method for reducing steel consumption in the entire continuous casting process according to claim 6, characterized in that: Reduce the aperture of the slide plate of the steel ladle; at the same time, when the lowest point of the steel ladle seat brick differs from the upper mouth of the steel ladle by more than 30mm, the steel ladle bottom seat brick needs to be replaced.