Method for realizing whole-course soft reduction of continuous casting bloom

By adjusting the pulling speed and automatically detecting the roller slot value when the continuous casting machine is started and stopped, the problem that the casting blank cannot be used for light pressure during continuous casting is solved, and the stable light pressure pressure technology is achieved throughout the casting blank. Improves the quality and operating efficiency of the casting billet.

CN119016701AActive Publication Date: 2024-11-26LINGYUAN IRON & STEEL CO LTD

Patent Information

Application Number
CN202411014085.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-26
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

During continuous casting, some casting blanks cannot use light pressing technology during the start and stop casting, resulting in difficulty in quality control of casting blanks, and the existing technology lacks effective solutions.

Method used

By adjusting the pulling speed when the continuous casting machine is started and stopped, and combining with automatic detection of the roller slot value, we ensure that the casting blank can be used stably throughout the whole process, including increasing the pulling speed within t min during the pouring , does not drop to zero pull speed when the pouring is stopped, and the cooling is assisted in the crystallizer, and the roller slot detection and pressing functions are automatically judged and performed.

Benefits of technology

It is possible to achieve stable use of light pressing technology for both the head furnace and the tail furnace casting billet during continuous casting and casting, which improves the stability of the internal quality of the casting billet and rolling material, and reduces the difficulty of operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016701A_ABST
    Figure CN119016701A_ABST
Patent Text Reader

Abstract

The invention discloses a method for realizing whole-course soft reduction of a continuous casting bloom, and relates to the field of metal casting, the method comprises the following steps: when continuous casting is started to pour, the pulling speed of a continuous casting machine within t min after the continuous casting is started is increased to the working pulling speed, and the time t is obtained by adding t1, t2 and t3; wherein t1 is the time required for increasing to the casting speed from zero, t2 is the maximum running time at the casting speed, and t3 is the time when the casting speed is increased to V2 from V1; when continuous casting stops pouring, the pulling speed of the continuous casting machine is reduced but not returned to zero, and after the tail of the casting blank in the crystallizer is pulled out, the pulling speed of the continuous casting machine is increased to the working pulling speed; according to the method, the problem that part of casting blanks cannot be slightly pressed during casting starting and casting stopping of a continuous casting machine can be solved, and the soft pressing technology can be stably applied to all the casting blanks of a head furnace during casting starting and a tail furnace during casting stopping of continuous casting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal casting, and more specifically, relates to a method for realizing full-process soft reduction of continuous casting large square billets. Background Art

[0002] Round steel made of large square billets is widely used in various fields of manufacturing, among which the control of the internal quality of round steel is particularly important. At present, the light reduction technology of large square billet continuous casting is relatively mature in terms of equipment and roll gap control. The reduction technology compensates for the shrinkage at the end of solidification, thereby improving the quality of the near-center position of the ingot and the corresponding rolled product. While controlling the shrinkage of the ingot, it can also control the solidification segregation behavior, which plays an important role in improving the internal quality of the ingot and rolled product.

[0003] However, when steel enterprises apply the light reduction process, some of the ingots in the first furnace of continuous casting cannot be cast using light reduction. The main reasons are as follows: (1) When continuous casting starts, the molten steel temperature is high and the pulling speed of the continuous casting machine is slow. When the first ingot enters the reduction equipment, it shrinks greatly. However, when the pulling speed of the continuous casting machine is increased to the working pulling speed, the shrinkage of the ingot will decrease. When light reduction is applied too early, the roll gap value detected by the reduction roller near the first ingot position deviates greatly from the normal working pulling speed, which leads to inaccurate roll gap detection. (2) At present, the conditions for starting light reduction are: when the hot ingot has completely passed through the reduction roller, and the current roll gap value is detected simultaneously after the shrinkage of the ingot is stable, and then the on-site operator starts light reduction. At this time, some of the ingots in the first furnace cannot be cast using light reduction, and the process is relatively arbitrary.

[0004] Most of the ingots in the last furnace of continuous casting cannot be lightly pressed down. The main reasons are as follows: At present, the conditions for stopping light pressure reduction are as follows: When continuous casting stops production, after the pouring of molten steel in the intermediate tank is completed, the pulling speed of the continuous casting machine is adjusted to zero, and the pulling speed of the continuous casting machine is restored after the ingot is capped. At this time, the ingot at the position of the pressing roller cannot continue to be lightly pressed down because the ingot has cooled too much. At this time, most of the ingots in the last furnace of continuous casting cannot be lightly pressed down.

[0005] At present, there are no good solutions to the above problems existing in steel mills. Summary of the invention

[0006] The purpose of the present invention is to address the deficiencies in the prior art and to provide a method for achieving light reduction throughout the continuous casting of large square billets. The method can solve the problem that some billets cannot be lightly reduced when the continuous casting machine starts or stops pouring, and can achieve the stable application of light reduction technology to all billets in the head furnace when continuous casting starts and in the tail furnace when continuous casting stops.

[0007] In order to achieve the above object, the present invention provides a method for achieving full-process soft reduction of continuous casting large square billets, the method comprising:

[0008] When continuous casting starts pouring, the continuous casting machine will increase the casting speed to the working casting speed within t min after the continuous casting starts pouring. The calculation formula of time t is:

[0009] t=t1+t2+t3 (1)

[0010] Among them, t1 is the time required for the pulling speed to increase from zero to the pulling speed at the start of pouring, t2 is the maximum running time at the pulling speed at the start of pouring, and t3 is the time when the pulling speed increases from V1 to V2;

[0011] When the continuous casting stops pouring, the pulling speed of the continuous casting machine is reduced but not returned to zero. After the tail of the ingot in the crystallizer is pulled out, the pulling speed of the continuous casting machine is increased to the working pulling speed.

[0012] Optionally, the distance L1 is calculated as follows:

[0013] L1=V1*t1 (2)

[0014] Among them, L1 is the maximum distance when the pulling speed is increased to V1 during pouring;

[0015] t1 is the time when the casting speed of the continuous casting machine increases from zero to V1;

[0016] V1 is the minimum pulling speed required for pouring.

[0017] Optionally, the calculation formula of L2 is:

[0018] L2=V1*t2 (3)

[0019] Among them, L2 is the distance of uniform motion when the pouring speed is V1;

[0020] t2 is the maximum time of uniform speed operation when the pouring speed is V1.

[0021] Optionally, the calculation formula of L3 is:

[0022]

[0023] Among them, L3 is the maximum distance when the pulling speed increases from V1 to V2;

[0024] V2 is the working speed of the continuous casting machine;

[0025] a is the acceleration.

[0026] Optionally, the acceleration a is less than 0.06 m / min 2 .

[0027] Optionally, t3 is calculated as:

[0028] V2=V1+at3 (5).

[0029] Optionally, the relationship between L2 and L and L1 and L3 is:

[0030] L2=L-L1-L3 (6).

[0031] Alternatively, L=the length of the continuous casting head furnace scrap cutting-0.25*(the number of the involved reduction rolls-1).

[0032] Optionally, the method further comprises:

[0033] When the head position of the first furnace casting billet passes the first pressing roller by a distance S1, the first pressing roller contacts the surface of the first furnace casting billet and automatically detects the roll gap value, and starts light pressing;

[0034] When the head position of the first furnace casting billet passes the second pressing roller by a distance S1, the second pressing roller contacts the surface of the first furnace casting billet and automatically detects the roll gap value;

[0035] When the first pressing roller starts to move to the pressing position by a distance S2, the second pressing roller starts to press lightly;

[0036] When the head position of the first furnace casting billet passes the third pressing roller by a distance S1, the third pressing roller contacts the surface of the first furnace casting billet and automatically detects the roll gap value;

[0037] When the second pressing roller starts to move the pressing position by a distance S2, the third pressing roller starts light pressing;

[0038] The subsequent actions of the pressing roller are analogous.

[0039] Optionally, displacement sensors are provided on the first pressing roller, the second pressing roller and the third pressing roller.

[0040] Optionally, the distance S1 and the distance S2 are calculated as follows:

[0041] S1 = 2* waste length of continuous casting head furnace / 3;

[0042] S2 = roller spacing + 0.25 m.

[0043] Optionally, the method further comprises:

[0044] First, determine whether the head end of the scrap cut portion of the last furnace billet of the casting has passed through the first pressing roller;

[0045] When passing through the first pressing roller, the first pressing roller stops light pressing and turns to a hot billet pressing state;

[0046] Then, determining whether the head end of the scrap cut portion of the last furnace billet of the casting has passed through the second pressing roller;

[0047] When passing through the second pressing roller, the second pressing roller stops light pressing and turns to a hot billet pressing state;

[0048] The subsequent actions of the pressing roller are analogous.

[0049] The present invention provides a method for realizing light reduction during the whole process of continuous casting of large square billets, and the beneficial effects are as follows: when the method starts pouring, the continuous casting machine is required to increase the pulling speed of the continuous casting machine to the working pulling speed within t min, and when the pouring of molten steel in the continuous casting intermediate tank is stopped, the pulling speed of the continuous casting machine is not returned to zero, and light and thin cold materials and other materials are added into the crystallizer to assist the cooling of the tail of the billet in the crystallizer, so as to increase the pulling speed of the continuous casting machine to the working pulling speed as soon as possible; in addition, the method automatically judges whether the head position of the billet in the first furnace and the head end of the waste cut part of the billet in the tail furnace pass through each reduction roller and the distance passed through the reduction roller, and performs the functions of roller gap detection, reduction and stopping reduction according to the set value, so as to realize that the billet in the first furnace when continuous casting starts and the billet in the tail furnace when stopping casting can all be stably lightly reduced.

[0050] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.

[0052] Figure 1 A flow chart of pressing down rollers in a method for achieving full-process soft reduction of continuous casting billets according to an embodiment of the present invention is shown.

[0053] Figure 2 A flow chart showing lifting of a reduction roller in a method for achieving full-process soft reduction of a continuous casting bloom according to an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0054] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0055] The present invention provides a method for achieving full-process soft reduction of continuous casting large square billets, the method comprising:

[0056] When continuous casting starts pouring, the continuous casting machine will increase the casting speed to the working casting speed within t min after the continuous casting starts pouring. The calculation formula of time t is:

[0057] t=t1+t2+t3 (1)

[0058] Among them, t1 is the time required for the pulling speed to increase from zero to the pulling speed at the start of pouring, t2 is the maximum running time at the pulling speed at the start of pouring, and t3 is the time when the pulling speed increases from V1 to V2;

[0059] When the continuous casting stops pouring, the pulling speed of the continuous casting machine is reduced but not returned to zero. After the tail of the ingot in the crystallizer is pulled out, the pulling speed of the continuous casting machine is increased to the working pulling speed.

[0060] Specifically, the method limits the speed-up time of the continuous casting machine. It is necessary to increase the pulling speed of the continuous casting machine to the starting casting speed. When the pulling speed reaches the starting casting speed, it is necessary to further increase the pulling speed and increase the starting casting speed to the working pulling speed. During this speed-up time, the shrinkage of the cast billet formed by casting is large. After increasing to the working pulling speed, the stable output of the cast billet can be guaranteed, and the cast billet at the position of the pressing roller can be lightly pressed down. When starting the machine, the time required for the continuous casting machine pulling speed to increase from zero to the starting casting speed is t1, the maximum time that the continuous casting machine runs at the starting casting speed is t2, and the time required for the continuous casting machine pulling speed to increase from the starting casting speed to the working pulling speed is t3. The sum of the three times is the time range required by the continuous casting machine.

[0061] Optionally, the distance L1 is calculated as follows:

[0062] L1=V1*t1 (2)

[0063] Among them, L1 is the maximum distance when the pulling speed is increased to V1 during pouring;

[0064] t1 is the time when the casting speed of the continuous casting machine increases from zero to V1;

[0065] V1 is the minimum pulling speed required for pouring.

[0066] Specifically, when pouring starts, the pulling speed does not reach the pouring pulling speed, resulting in a large shrinkage ingot length L1. The minimum pulling speed for pouring starts is a process setting. The ingot length L1 can be calculated through the minimum pulling speed and the time it takes for the pulling speed to increase from zero to the pouring pulling speed.

[0067] Optionally, the calculation formula of time t3 is:

[0068] V2=V1+at3 (5).

[0069] Specifically, t3 is the time required for the pulling speed to increase from the start-casting pulling speed to the working pulling speed. The working pulling speed V2 of the continuous casting machine is also set by the process. a is the acceleration. The acceleration time t3 can be obtained through the above parameters.

[0070] Optionally, the distance L3 is calculated as follows:

[0071]

[0072] Specifically, L3 is the distance the billet runs when the casting speed is increased from V1 to V2. The running distance L3 can be obtained through the above parameters.

[0073] Optionally, the acceleration a is less than 0.06 m / min 2 .

[0074] Specifically, the acceleration a is a fixed value determined according to the fluctuation of the liquid level. Generally, the acceleration a of a large square billet is less than 0.06m / min. 2 Through the above parameters, we can get the acceleration time of t3 and the running distance L3.

[0075] Optionally, the relationship between L and L1 and L2 and L3 is:

[0076] L=L1+L2+L3 (5)

[0077] Optionally, the calculation formula of time t2 is:

[0078] L2=V1*t2 (6)

[0079] Among them, L2 is the distance of uniform motion when the pouring speed is V1;

[0080] t2 is the maximum time of uniform speed operation when the pouring speed is V1.

[0081] Specifically, t2 is the maximum time of uniform pulling speed during pouring, the pulling speed V1 during pouring is set by the process, and L2 can be calculated from L, L1, and L3.

[0082] Alternatively, L=the length of the continuous casting head furnace scrap cutting-0.25*(the number of the involved reduction rolls-1).

[0083] Specifically, the length of the ingot produced during the two periods from startup to casting speed and from casting speed to working casting speed can be calculated. The maximum time of casting speed operation can be calculated through four parameters: the scrap cutting length of the first furnace, the number of rollers involved in the pressing down, and the running distance from startup to casting speed and from casting speed to working casting speed.

[0084] Optionally, the method further comprises:

[0085] When the head position of the first furnace casting billet passes the first pressing roller at a distance S1, the first pressing roller contacts the surface of the first furnace casting billet and detects the roll gap value, and then starts light pressing;

[0086] When the head position of the first furnace casting billet passes the second pressing roller by a distance S1, the second pressing roller contacts the surface of the first furnace casting billet and detects the roll gap value;

[0087] When the first pressing roller starts to move to the pressing position by a distance S2, the second pressing roller starts to press lightly;

[0088] When the head position of the first furnace casting billet passes the third pressing roller by a distance S1, the third pressing roller contacts the surface of the first furnace casting billet and detects the roll gap value;

[0089] When the second pressing roller starts to move to the pressing position by a distance S2, the third pressing roller starts to press lightly;

[0090] The subsequent actions of the pressing roller are analogous.

[0091] Specifically, the method executes the roller gap detection, pressing down and stopping pressing down action instructions according to the set distance, which greatly reduces the operating difficulty of on-site workers and provides a guarantee for improving the internal quality stability of the ingot and rolled product.

[0092] Optionally, displacement sensors are provided on the first pressing roller, the second pressing roller and the third pressing roller.

[0093] Specifically, when it is monitored that the head of the first furnace billet passes through the first pressing roller, the first pressing roller descends to contact with the upper surface of the billet. When it is monitored that the head of the first furnace billet passes the first pressing roller S1 distance, the current position of the pressing roller can be measured by the displacement sensor, and the roller gap value, that is, the thickness of the billet passing through the first pressing roller, can be calculated. The pressing distance of the first pressing roller is adjusted according to the process requirements and the existing billet thickness, and the billet is pressed down. When it is monitored that the head of the first furnace billet passes through the second pressing roller, the second pressing roller descends to contact with the upper surface of the billet. The surface is contacted, when the head of the first furnace ingot passes the second pressing roller S1, the roller gap value is detected by the displacement sensor, and the moving distance of the first pressing roller starting to press down is confirmed. When the first pressing roller starts to move the distance S2, the second pressing roller adjusts the pressing distance of the second pressing roller according to the roller gap value detected by the second pressing roller, and presses down the ingot through the pressing action of the second pressing roller; the subsequent pressing rollers adopt the same steps and press down after detecting the roller gap value, ultimately providing a guarantee for improving the internal quality stability of the ingot and rolled product.

[0094] In addition, in this method, the roll gap values ​​of the various pressing rolls are not detected synchronously. Each pressing roll performs the roll gap value detection operation one by one. After the roll gap value is detected, the billet is pressed down. The roll gap detection value and the pressing are performed separately to avoid deviations in the amount of billet pressing down.

[0095] Optionally, the distance S1 and the distance S2 are calculated as follows:

[0096] S1 = 2* waste length of continuous casting head furnace / 3;

[0097] S2 = roller spacing + 0.25 m.

[0098] Specifically, the distance S1 that the billet passes through the rollers is selected based on the following principles: the billet surface temperature does not change much and the billet shrinkage is relatively stable.

[0099] Optionally, the method further comprises:

[0100] First, determine whether the head end of the scrap cut portion of the last furnace billet of the casting has passed through the first pressing roller;

[0101] When passing through the first pressing roller, the first pressing roller stops light pressing and turns to the hot billet pressing state;

[0102] Then determine whether the head end of the scrap cut portion of the last furnace billet of the casting has passed through the second pressing roller;

[0103] When passing through the second pressing roller, the second pressing roller stops light pressing and turns to the hot billet pressing state;

[0104] The subsequent actions of the pressing roller are analogous.

[0105] Example

[0106] like Figure 1 to Figure 2 As shown, the present invention provides a method for achieving full-process soft reduction of continuous casting large square billets, the method comprising:

[0107] When continuous casting starts pouring, the continuous casting machine will increase the casting speed to the working casting speed within t min after the continuous casting starts pouring. The calculation formula of time t is:

[0108] t=t1+t2+t3 (1)

[0109] Among them, t1 is the time required for the pulling speed to increase from zero to the pulling speed at the start of pouring, t2 is the maximum running time at the pulling speed at the start of pouring, and t3 is the time when the pulling speed increases from V1 to V2;

[0110] When the continuous casting stops pouring, the pulling speed of the continuous casting machine is reduced but not returned to zero. After the tail of the ingot in the crystallizer is pulled out, the pulling speed of the continuous casting machine is increased to the working pulling speed.

[0111] In this embodiment, the calculation formula of the distance L1 is:

[0112] L1=V1*t1 (2)

[0113] Among them, L1 is the maximum distance when the pulling speed is increased to V1 during pouring;

[0114] t1 is the time when the casting speed of the continuous casting machine increases from zero to V1;

[0115] V1 is the minimum pulling speed required for pouring.

[0116] In this embodiment, the calculation formula of time t3 is:

[0117] V2=V1+at3 (3)

[0118] Where a is the acceleration;

[0119] V2 is the working speed of the continuous casting machine.

[0120] In this embodiment, the calculation formula of L3 is:

[0121]

[0122] Among them, L3 is the maximum distance when the pulling speed increases from V1 to V2;

[0123] V2 is the working speed of the continuous casting machine;

[0124] t3 is the time corresponding to when the pulling speed increases from V1 to V2;

[0125] a is the acceleration.

[0126] In this embodiment, the relationship between L2 and L and L1 and L3 is:

[0127] L2=L-L1-L3 (5)

[0128] In this embodiment, L=the scrap length of the continuous casting head furnace-0.25*(the number of rollers involved in the reduction-1).

[0129] In this embodiment, the calculation formula of time t2 is:

[0130] L2=V1*t2 (6)

[0131] Among them, L2 is the distance of uniform motion when the pouring speed is V1;

[0132] t2 is the maximum time of uniform speed operation when the pouring speed is V1.

[0133] In this embodiment, the acceleration a is less than 0.06 m / min 2 .

[0134] In this embodiment, the method further includes:

[0135] When the head position of the first furnace casting billet passes the first pressing roller at a distance S1, the first pressing roller contacts the surface of the first furnace casting billet and detects the roll gap value, and then starts light pressing;

[0136] When the head position of the first furnace casting billet passes the second pressing roller by a distance S1, the second pressing roller contacts the surface of the first furnace casting billet and detects the roll gap value;

[0137] When the first pressing roller starts to move to the pressing position by a distance S2, the second pressing roller starts to press lightly;

[0138] When the head position of the first furnace casting billet passes the third pressing roller by a distance S1, the third pressing roller contacts the surface of the first furnace casting billet and detects the roll gap value;

[0139] When the second pressing roller starts to move to the pressing position by a distance S2, the third pressing roller starts to press lightly;

[0140] The subsequent actions of the pressing roller are analogous.

[0141] In this embodiment, displacement sensors are provided on the first pressing roller, the second pressing roller and the third pressing roller.

[0142] In this embodiment, the distance S1 and the distance S2 are calculated as follows:

[0143] S1 = 2* waste length of continuous casting head furnace / 3;

[0144] S2 = roller spacing + 0.25 m.

[0145] In this embodiment, the method further includes:

[0146] First, determine whether the head end of the scrap cut portion of the last furnace billet of the casting has passed through the first pressing roller;

[0147] When passing through the first pressing roller, the first pressing roller stops light pressing and turns to the hot billet pressing state;

[0148] Then determine whether the head end of the scrap cut portion of the last furnace billet of the casting has passed through the second pressing roller;

[0149] When passing through the second pressing roller, the second pressing roller stops light pressing and turns to the hot billet pressing state;

[0150] The subsequent actions of the pressing roller are analogous.

[0151] In summary, when the process stipulates that the "waste cutting length of the continuous casting head furnace" is 4m, and there are four pressing rollers involved in the pressing, then through the formula "L = waste cutting length of the continuous casting head furnace - 0.25 * (the number of rollers involved in the pressing - 1)", it is calculated that L = 4-(4-1) * 0.25 = 3.25m; when the process stipulates that the minimum pulling speed required for pouring is 0.3m / min, then V1 = 0.3m / min; the time t1 required to increase the pulling speed to the pouring pulling speed is determined according to the actual operating conditions, usually t1 = 0.5min; the continuous casting machine working pulling speed V2 is also determined by the process, and the value V2 = 0.4m / min; the acceleration a of the casting machine pulling speed from V1 to V2 is specified by the process, and this paper selects a = 0.06m / min 2 .

[0152] From the formula V2=V1+at3, it can be deduced that: t3=(0.4-0.3) / 0.06=1.7min;

[0153] By formula It can be calculated that: L3 = 0.3*1.7 + 1 / 2*0.06*1.7*1.7 = 0.6m;

[0154] From the formula L=L1+L2+L3, we can deduce that: L2=LL 1- -L3=3.25-0.3*0.5-0.6=2.5m;

[0155] From the formula L2 = V1 * t2, it can be deduced that: t2 = 2.5 / 0.3 = 8.4min;

[0156] From the formula t=t1+t2+t3, it can be calculated that: t=0.5+8.3+1.7=10.5min.

[0157] Finally, the maximum time of the pulling speed operation at the start of pouring is t2=8.3min; t=10.5min, that is, the total time for the pulling speed to increase from 0 to the working pulling speed after continuous casting cannot exceed 10.5min.

[0158] During the continuous casting process, when the pouring of molten steel in the continuous casting intermediate tank stops, the pulling speed of the continuous casting machine is reduced appropriately, but the pulling speed does not return to zero. At the same time, the tail of the ingot in the auxiliary crystallizer is cooled. After the tail of the ingot is pulled out of the crystallizer, the pulling speed of the continuous casting machine is increased to the working pulling speed to ensure that the ingot at the pressing roller position has the ability to be lightly pressed down.

[0159] When the process stipulates that the scrap cutting length of the continuous casting head furnace is 4m, S1=2*4 / 3=2.7m; when the roller spacing between adjacent pressure rollers in the continuous casting machine is 1.2m, S2=1.2+0.25=1.45m. In this way, when the head position of the first furnace billet passes through the first pressing roller, the first pressing roller is fitted with the surface of the billet, and when the distance of the head position of the first furnace billet passing the first pressing roller reaches 2.7m, the first pressing roller detects the roll gap value, and at the same time, the first pressing roller presses down the billet; when the head position of the first furnace billet passes through the second pressing roller, the second pressing roller is fitted with the surface of the billet, and when the distance of the head position of the first furnace billet passing the second pressing roller reaches 2.7m, the second pressing roller detects the roll gap value to confirm the distance moved by the first pressing roller to the starting pressing position, and when the billet moves 1.45m from the starting pressing position of the first pressing roller, the second pressing roller presses down the billet, and the subsequent operations of the third and fourth pressing rollers are similar.

[0160] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A method for achieving full soft reduction during continuous casting of large square billets. It is characterized in that The method includes: When continuous casting starts pouring, the continuous casting machine will increase the casting speed to the working casting speed within t min after the continuous casting starts pouring. The calculation formula of time t is: t=t 1 +t 2 +t 3 (1) Among them, t 1 The time required for the pulling speed to increase from zero to the pouring speed, t 2 is the maximum running time at the pouring speed, t 3 The pulling speed is V 1 Increase to V 2 time of day; When the continuous casting stops pouring, the pulling speed of the continuous casting machine is reduced but not returned to zero. After the tail of the ingot in the crystallizer is pulled out, the pulling speed of the continuous casting machine is increased to the working pulling speed.

2. The method for achieving full soft reduction during continuous casting of large square billets according to claim 1, It is characterized in that Distance L 1 The calculation formula is: L 1 =V 1 *t 1 (2) Among them, L 1 When pouring begins, the pulling speed is increased to V 1 The maximum distance when t 1 To increase the casting speed of the continuous casting machine from zero to V 1 time; V 1 The minimum pulling speed required for pouring.

3. The method for achieving full soft reduction during continuous casting of large square billets according to claim 1, It is characterized in that L 2 The calculation formula is: L 2 =V 1 *t 2 (3) Among them, L 2 V is the pulling speed at the beginning of pouring 1 Distance traveled at a constant speed t 2 It is the maximum running time when the pouring speed is started.

4. The method for achieving full soft reduction during continuous casting of large square billets according to claim 1, It is characterized in that L 3 The calculation formula is: Among them, L 3 The pulling speed is V 1 Increase to V 2 The maximum distance when V 2 Working speed of continuous casting machine; a is acceleration, which is less than 0.06m / min 2 .

5. The method for achieving full soft reduction during continuous casting of large square billets according to claim 4, It is characterized in that t 3 The calculation formula is: V 2 =V 1 +at 3 (5)。 6. The method for achieving full soft reduction during continuous casting of large square billets according to claim 3, It is characterized in that L 2 With L and L 1 and L 3 The relationship is: L 2 =LL 1 -L 3 (6) 7. The method for achieving full soft reduction during continuous casting of large square billets according to claim 6, It is characterized in that L = waste cutting length of continuous casting head furnace - 0.25*(number of rollers involved in pressing down - 1).

8. The method for achieving full soft reduction during continuous casting of large square billets according to claim 1, It is characterized in that The method further includes: When the head position of the first furnace casting billet passes the first pressing roller by a distance S1, the first pressing roller contacts the surface of the first furnace casting billet and automatically detects the roll gap value, and starts light pressing; When the head position of the first furnace casting billet passes the second pressing roller by a distance S1, the second pressing roller contacts the surface of the first furnace casting billet and automatically detects the roll gap value; When the first pressing roller starts to move to the pressing position by a distance S2, the second pressing roller starts to press lightly; When the head position of the first furnace casting billet passes the third pressing roller by a distance S1, the third pressing roller contacts the surface of the first furnace casting billet and automatically detects the roll gap value; When the second pressing roller starts to move the pressing position by a distance S2, the third pressing roller starts light pressing; The subsequent actions of the pressing roller are analogous.

9. The method for achieving full soft reduction during continuous casting of large square billets according to claim 8, It is characterized in that The first pressing roller, the second pressing roller and the third pressing roller are provided with displacement sensors; The distance S1 and distance S2 are calculated as follows: S1 = 2* waste length of continuous casting head furnace / 3; S2 = roller spacing + 0.25 m.

10. The method for achieving full soft reduction during continuous casting of large square billets according to claim 9, It is characterized in that The method further includes: First, determine whether the head end of the scrap cut portion of the last furnace billet of the casting has passed through the first pressing roller; When passing through the first pressing roller, the first pressing roller stops light pressing and turns to a hot billet pressing state; Then, determining whether the head end of the scrap cut portion of the last furnace billet of the casting has passed through the second pressing roller; When passing through the second pressing roller, the second pressing roller stops light pressing and turns to a hot billet pressing state; The subsequent actions of the pressing roller are analogous.

Citation Information

Patent Citations

  • Adjusting method of slab caster roll gap under unsteady state pouring condition

    CN105057625A

  • Roll gap control method and device under light pressing or heavy pressing

    CN111001772A

  • Method and device for light rolling-reduction in continuous casting equipment

    JP2010240727A

Cited By

  • Control process for reducing shrinkage cavities of slab continuous casting tail blank

    CN120679965A

  • Static soft reduction control model based on PLC and Wincc

    CN120696383A

  • Method for controlling non-pressing length of billet head and pressing method of continuous casting billet

    CN121017489A