Composite sandwich panel as well as preparation method and application thereof
By using a composite sandwich structure of high-density foam board and low-density wood board, the problems of air bubbles and explosive delamination in balsa wood sandwich materials are solved, improving the structural stability and performance of wind turbine blades and extending their service life.
Patent Information
- Application Number
- CN202411242133.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The use of balsa wood as a core material in existing wind turbine blades is prone to causing defects such as bubbles and explosive delamination, which affect the structural stability and performance of the blades.
High-density foam board is combined with low-density wood board. The foam board serves as a protective layer, reducing the amount of glue absorbed by the wood board and improving the bonding strength. High-performance foam board is prepared through a specific process and then bonded to both sides of the wood board to form a composite sandwich structure.
It improves the compressive and shear strength of composite sandwich panels, reduces adhesive absorption, enhances the overall performance and yield of wind turbine blades, and extends their service life.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of supporting plates, and in particular to a composite sandwich plate and a preparation method and application thereof. Background Art
[0002] As a renewable energy, wind power generation is a new energy source that is different from traditional energy sources. Compared with other new energy sources such as solar power generation, wind power generation has more scale and economic advantages. Especially with the gradual depletion of coal resources, the rising calls for environmental protection and the concern about climate change, as well as people's deepening understanding of the various disadvantages of traditional energy, many countries in the world have invested a lot of manpower, material and financial resources to develop environmentally friendly new energy sources, which has led to the rapid expansion of the wind power industry.
[0003] The upstream materials of the wind power industry mainly include towers, wind turbines, nacelles, main shafts, cables and blades. Wind turbine blades are one of the core components of wind turbines. Their good design, reliable quality and superior performance are the decisive factors to ensure the normal and stable operation of wind turbines.
[0004] From the perspective of wind turbine blade structure, it is mainly composed of reinforcement materials, sandwich materials, matrix materials, surface coatings and structural adhesives between different parts. In the application of wind turbine blades, the structural core material is the key material of wind turbine blades, which can greatly ensure the stability of the laminate, while improving the strength and rigidity of the blade structure, reducing the weight of the blade, preventing local instability, and further improving the impact resistance and load resistance of the entire blade. The sandwich materials currently used in wind turbine blades mainly include balsa wood, PVC foam, PET foam, etc. Among them, although balsa wood is light in texture, its structure is very strong, with low density, high strength, sound insulation, heat insulation and other properties, and is usually used in the root of the blade. The foam board has a low density and a light texture, but the structural performance of the foam board is weaker than that of balsa wood, and is usually used in the middle and front ends of the blades.
[0005] In response to the above-mentioned related technologies, the applicant found that balsa wood, as a natural wood, is the main source of water in the vacuum infusion molding material system. In addition, its internal capillaries are closed-cell structures, which will induce bubbles, explosions and delamination defects in wind turbine blades. Summary of the invention
[0006] In order to improve the comprehensive performance of wind turbine blades, the present application provides a composite sandwich panel and a preparation method and application thereof.
[0007] In a first aspect, the present application provides a composite sandwich panel material, which adopts the following technical solution.
[0008] A composite sandwich panel comprises a wood board and foamed boards arranged on both sides of the wood board, wherein the density of the wood board is 100-200 kg / m3 The density of the foamed board is 200-300 kg / m 3 The thickness of the foamed board is 8-30% of the thickness of the wood board.
[0009] By adopting the above technical solution, high-density foam board is compounded with low-density wood board. The compressive strength of the composite sandwich panel can reach 13.0-14.2MPa, and the shear strength can reach 2.8-3.1MPa, with excellent mechanical properties. In addition, the foam board acts as a protective layer on both sides of the wood board, replacing the wood board in direct contact with the poured resin during pouring, reducing the amount of glue absorbed by the wood board and avoiding the defect of wood glue absorption. The amount of glue absorption is as low as 0.8-1.3kg / m 3 , improve the bonding strength between the core material and the resin in the wind turbine blade, improve the overall performance of the blade, extend the service life of the blade, and at the same time improve the yield of blade preparation.
[0010] Furthermore, the density of the wood board is 100-180 kg / m 3 The density of the foamed board is 230-300 kg / m 3 The thickness of the foamed board is 8-25% of the thickness of the wood board.
[0011] Furthermore, the density of the wood board is 100-150 kg / m 3 The density of the foamed board is 250-300 kg / m 3 The thickness of the foamed board is 8-20% of the thickness of the wood board.
[0012] Furthermore, the foam board is one or more of a PET foam board, a PVC foam board, and a SAN foam board.
[0013] Furthermore, the PET foam board comprises the following raw materials in parts by weight: 60-70 parts of PET particles, 30-35 parts of secondary materials, 0.5-0.8 parts of cross-linking agent, 1.5-2.0 parts of nucleating agent, 0.8-1.2 parts of chain extender, 0.5-1.0 parts of lubricant, and 0.4-1.0 parts of foaming agent.
[0014] Furthermore, the preparation process of the PET foam board comprises the following steps: 1) Preheating of raw materials Dry each raw material at 60-70°C for 3-4 hours, then heat to 160-170°C; 2) Preheating the extruder Preheat the extruder at 320℃ for 5-6 hours, discharge the remaining material in the extruder, add the cleaning agent, stabilize for 30 minutes, then add other raw materials except the foaming agent, until the clean material is discharged from the extruder outlet, then add the foaming agent; 3) Set the extruder temperature The temperature settings of each zone of the extruder are: Zone 1 295-300°C, Zone 2 295-300°C, Zone 3 295-300°C, Zone 4 290-295°C, Zone 5 285-295°C, Zone 6 290-295°C, Zone 7 270-275°C, Zone 8 260-265°C, Zone 9 280-285°C, Zone 9A 265-270°C, Zone 10 260-265°C, Zone 11 260-265℃, Zone 12 260-265℃, Zone 13 260-265℃, Zone 14 260-265℃, Zone 15 260-265℃, Oil Zone 1 245-255℃, Oil Zone 2 240-245℃, Oil Zone 3 235-240℃, Oil Zone 4 230-235℃, Oil Zone 5 245-250℃, Ring Network Device 275-285℃, Head 1 275-285℃, die 2 275-285℃, die 3 290-295℃, die 4 290-295℃, die 5 285-290℃, die 6 285-290℃, die 1 245-275℃, die 2 245-275℃, die 3 245-275℃, die 4 245-275℃, mixer 210-270℃; 4) Extrusion As the temperature gradually drops to the set value, the material at the outlet of the extruder gradually presents the normal shape of a foam board, and is pulled from the front puller to the rear puller, and after de-edging and flying sawing, it is cooled in a cooling tower, and then passed through a planer before being stacked; 5) Welding After the plate is cooled for 2 days, it is welded to the corresponding length as required; 6) Cutting After the welded plates are cooled for 2 days, they are cut into sheets of different sizes according to needs.
[0015] By adopting the above technical solution, using additives in a specific ratio and combining with a specific process, a high-density PT foam board with excellent stability and mechanical properties can be obtained.
[0016] Furthermore, the PVC foam board comprises the following raw materials in parts by weight: 75-80 parts of polyvinyl chloride, 1.3-1.7 parts of stabilizer, 7-8 parts of regulator, 1.1-1.8 parts of foaming agent, and 12-18 parts of lubricant.
[0017] Furthermore, the SAN foam board comprises the following raw materials in parts by weight: 75-85 parts of styrene, 7-10 parts of acrylonitrile, 1.0-1.5 parts of a crosslinking agent, 2.5-3.2 parts of a nucleating agent, 1.8-2.1 parts of a chain extender, 3-5 parts of a lubricant, and 0.3-1.0 parts of a foaming agent.
[0018] In a second aspect, the present application provides a method for preparing a composite sandwich panel, which adopts the following technical solution.
[0019] A method for preparing a composite sandwich panel comprises the following steps: The foam board is bonded to both sides of the wood board by adhesive.
[0020] In a third aspect, the present application provides an application of a composite sandwich panel, adopting the following technical solution.
[0021] An application of a composite sandwich panel material, characterized in that the composite sandwich panel material is applied to the root portion of a wind turbine blade.
[0022] By adopting the above technical solution, more choices are provided for the sandwich materials of wind turbine blades. When selecting the sandwich material at the root of the blade, not only can the infusion defects of the wood board be avoided, but also the comprehensive structural performance of the sandwich material can be guaranteed, and the sandwich material will not be too heavy to affect the overall weight of the wind turbine blade.
[0023] In summary, this application has the following beneficial effects: The high-density foam board is combined with the low-density wood board. The compressive strength of the composite sandwich panel can reach 13.0-14.2MPa, and the shear strength can reach 2.8-3.1MPa, with excellent mechanical properties. The glue absorption of the composite sandwich panel is as low as 0.8-1.3kg / m 3 , reduce the amount of resin absorbed by the blade when it is infused with resin, increase the bonding strength between the core material and the resin in the wind turbine blade, improve the overall performance of the blade, extend the service life of the blade, and at the same time increase the yield of blade preparation. DETAILED DESCRIPTION
[0024] The present application is further described in detail below with reference to the embodiments.
[0025] Raw materials and intermediate preparation examples raw material The raw materials in the examples of this application can be obtained from the market: Raw materials of PET sheets: PET granules, polyethylene terephthalate 100%; Secondary materials, scraps generated during the production of PET foam boards; Crosslinking agent, antioxidant TH-17901; Nucleating agent, silica; Chain extender, 1,2,4,5-pyromellitic dianhydride and 1,2,4-trimethylbenzene anhydride in a weight ratio of 2.5:1; Lubricant, 1,2,4,5-pyromellitic dianhydride; Blowing agent, cyclopentane; PVC foam board raw materials: Polyvinyl chloride, technical grade; Stabilizer, hydrochloric acid stabilizer Regulator, PVC foaming regulator Lubricant, PE wax Blowing agent, azodicarbonamide SAN foam board raw materials: Styrene, technical grade; Acrylonitrile, technical pure; Cross-linking agent, tetrabromobisphenol; Nucleating agent, toluene diisocyanate; Chain extender, maleic anhydride; Lubricant, acrylic; Blowing agent, ethane; Timber boards, balsa wood boards.
[0026] Preparation Example Preparation Examples I-1 to I-5 A PET foam board, the preparation process of which is as follows: 1) Preheating of raw materials Each raw material was dried at 65°C for 3.5 hours and then heated to 165°C; 2) Preheating the extruder Preheat the extruder at 320°C for 5.5 hours, discharge the remaining material in the extruder, add the cleaning agent, stabilize for 30 minutes, and then add other raw materials except the foaming agent according to the raw material ratio in Table 1 until the clean material is discharged from the extruder outlet, and then add the foaming agent; 3) Set the extruder temperature The temperature of each zone of the extruder was set according to Table 2; the screw speed of the extruder was 18.5 RPM; 4) Extrusion As the temperature gradually drops to the set value, the material at the outlet of the extruder gradually presents the normal shape of a foam board, and is pulled from the front puller to the rear puller, and after de-edging and flying sawing, it is cooled in a cooling tower, and then passed through a planer before being stacked; 5) Welding After the plate is cooled for 2 days, it is welded to the corresponding length as required; 6) Cutting After the welded plates are cooled for 2 days, they are cut into sheets of different sizes according to needs.
[0027] Table 1 Raw material ratio of PET foam board in preparation examples I-1~I-5 (kg)
[0028] Table 2 Preparation Example I-1~I-5 PET Foam Board Preparation Process Extruder Temperature Setting Table
[0029] Preparation Example I-6 Different from Preparation Example I-2, the extruder temperature setting of the PET foam board preparation process in Preparation Example I-6 is different, see Table 3 for details.
[0030] Table 3 Preparation Example I-6 PET Foam Board Preparation Process Extruder Temperature Setting Table
[0031] Preparation Example I-7 Different from Preparation Example I-2, the extruder temperature setting of the PET foam board preparation process in Preparation Example I-7 is different, see Table 4 for details.
[0032] Table 4 Preparation Example I-7 PET Foam Board Preparation Process Extruder Temperature Setting Table
[0033] Preparation Example I-8 Different from Preparation Example I-2, the extruder temperature setting of the PET foam board preparation process in Preparation Example I-8 is different, see Table 5 for details.
[0034] Table 5 Preparation Example I-8 PET Foam Board Preparation Process Extruder Temperature Setting Table
[0035] Preparation Example II-1 A PVC foam board, the preparation process of which is as follows: 1) Preparation of foam raw materials Add the raw materials into the foaming machine according to the raw material ratio in Table 6, and expand the foam raw materials into porous materials through heating and the action of the foaming agent; 2) Forming The expanded foam material is placed into a mold and formed into the desired shape and size through heating and compression; 3) Testing and packaging The prepared foam products are subjected to quality inspections, including appearance, density, strength, etc., and are packaged and shipped after meeting the requirements.
[0036] Table 6 PVC foam board raw material ratio table (kg)
[0037] Preparation Example III-1 A SAN foam board, the preparation process of which is as follows: 1) Mix According to the raw material ratio in Table 7, all raw materials were put into the reactor in proportion, heated and stirred for 40 minutes; 2) Pour into mold Pour the mixed raw materials into the mold, being careful not to exceed the maximum liquid level; 3) Polymerization reaction Put the mold into a water tank and heat the water to 60°C for 30 hours; 4) Low temperature annealing Reduce the water temperature to 40°C and keep it low for 8 hours; 5) Remove sperm embryos Remove the embryo from the mold; 6) Foaming Put the refined embryo into the foaming furnace, set the temperature rise curve, heat and foam to the specified size and take it out; 7) Cold Pressing Put the foam board into the cold press and press the cold press board to fix the size.
[0038] Table 7 SAN foam board raw material ratio table (kg)
[0039] Performance Testing The density of the foam board was tested, and the test results are shown in Table 8.
[0040] Table 8 Foam board performance test results Example
[0041] Example 1 A composite sandwich panel, the preparation method of which is as follows: The foam board is bonded to both sides of the wood board by adhesive.
[0042] The density of the wood board is 100 kg / m 3 , the density of the foam board is 300kg / m 3 The thickness of the foamed board is 8% of the thickness of the wood board. The foamed board is the PET board from Preparation Example I-1. The thickness of the composite sandwich panel is 60 mm.
[0043] Embodiment 2-10 Different from Example 1, the density of the wood board, the density of the foam board and the thickness of the foam board in Examples 2-10 are different, see Table 9 for details.
[0044] Table 9 Parameters of composite sandwich panels in Examples 1-10
[0045] Embodiment 11 Different from Example 2, the foam board in Example 11 is a PVC foam board.
[0046] Example 12 Different from Example 2, the foam board in Example 12 is a SAN foam board.
[0047] Embodiment 13 Different from Example 2, in Example 13, one of the foamed boards is a PET foamed board and the other is a SAN foamed board.
[0048] Embodiment 14 Different from Example 2, one of the foamed boards in Example 14 is a PET foamed board and the other is a PCV foamed board.
[0049] Embodiment 15 Different from Example 2, one of the foam boards in Example 15 is a PET foam board and the other is a PVC foam board.
[0050] Comparative Example Comparative Example 1 Different from Example 1, the density of the foamed board in Comparative Example 1 is 150 kg / m 3 .
[0051] Comparative Example 2 Different from Example 1, in Comparative Example 2, the ratio of the thickness of the foamed board to the thickness of the wood board is 6%.
[0052] Performance Testing The compressive strength of the composite sandwich panel was tested with reference to the ISO-844 method, the shear strength of the composite sandwich panel was tested with reference to ASTM C-273, and the glue absorption performance (resin absorption) of the composite sandwich panel was tested with reference to TR-7323. The test results are shown in Table 10.
[0053] Table 10 Composite sandwich panel performance test results
[0054] Combined with the test data in Table 10, it can be seen that the composite sandwich panel obtained by using wood board as the sandwich core and bonding foam boards on both sides not only has excellent mechanical properties but also has low glue absorption, which improves the defect of high glue absorption of wood.
[0055] Application Examples Application Example 1 According to the production process of wind turbine blades, the composite sandwich panel material obtained in Example 1 is applied to wind turbine blades.
[0056] Application Example 2-10 Different from Application Example 1, the composite sandwich panels in Application Examples 2-10 are respectively from Embodiments 2-10.
[0057] Comparative Application Examples Comparative application example 1 The difference from Application Example 1 is that in Comparative Example 1, the composite sandwich panel is replaced by a wood panel.
[0058] Performance Testing Ten professionals observed and judged the core material conditions in the wind turbine blades in the corresponding use cases and comparative application cases, and then reached a unified test conclusion. The results are shown in Table 11.
[0059] Table 11 Performance test results
[0060] It can be seen from the data in Table 11 that the composite sandwich panel of the present application is applied to wind turbine blades, which not only meets the mechanical performance requirements but also improves the whitening and delamination problems after glue injection.
[0061] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A composite sandwich panel, It is characterized in that The invention comprises a wood board and foaming boards arranged on both sides of the wood board, wherein the density of the wood board is 100-200 kg / m 3 The density of the foamed board is 200-300 kg / m 3 The thickness of the foamed board is 8-30% of the thickness of the wood board.
2. A composite sandwich panel according to claim 1, It is characterized in that The density of the wood board is 100-180 kg / m 3 The density of the foamed board is 230-300 kg / m 3 The thickness of the foamed board is 8-25% of the thickness of the wood board.
3. A composite sandwich panel according to claim 1, It is characterized in that The density of the wood board is 100-150 kg / m 3 The density of the foamed board is 250-300 kg / m 3 The thickness of the foamed board is 8-20% of the thickness of the wood board.
4. The composite sandwich panel according to claim 1, It is characterized in that The foam board is one or more of a PET foam board, a PVC foam board, and a SAN foam board.
5. A composite sandwich panel according to claim 4, It is characterized in that The PET foam board comprises the following raw materials in parts by weight: 60-70 parts of PET particles, 30-35 parts of secondary materials, 0.5-0.8 parts of crosslinking agent, 1.5-2.0 parts of nucleating agent, 0.8-1.2 parts of chain extender, 0.5-1.0 parts of lubricant and 0.4-1.0 parts of foaming agent.
6. A composite sandwich panel according to claim 5, It is characterized in that The preparation process of the PET foam board comprises the following steps: 1) Preheating of raw materials Dry each raw material at 60-70°C for 3-4 hours, then heat to 160-170°C; 2) Preheating the extruder Preheat the extruder at 320℃ for 5-6 hours, discharge the remaining material in the extruder, add the cleaning agent, stabilize for 30 minutes, then add other raw materials except the foaming agent, until the clean material is discharged from the extruder outlet, then add the foaming agent; 3) Set the extruder temperature The temperature settings of each zone of the extruder are: Zone 1 295-300°C, Zone 2 295-300°C, Zone 3 295-300°C, Zone 4 290-295°C, Zone 5 285-295°C, Zone 6 290-295°C, Zone 7 270-275°C, Zone 8 260-265°C, Zone 9 280-285°C, Zone 9A 265-270°C, Zone 10 260-265°C, Zone 11 260-265℃, Zone 12 260-265℃, Zone 13 260-265℃, Zone 14 260-265℃, Zone 15 260-265℃, Oil Zone 1 245-255℃, Oil Zone 2 240-245℃, Oil Zone 3 235-240℃, Oil Zone 4 230-235℃, Oil Zone 5 245-250℃, Ring Network Device 275-285℃, Head 1 275-285°C, die 2 275-285°C, die 3 290-295°C, die 4 290-295°C, die 5 285-290°C, die 6 285-290°C, die 1 245-275°C, die 2 245-275°C, die 3 245-275°C, die 4 245-275°C, mixer 210-270°C; 4) Extrusion As the temperature gradually drops to the set value, the material at the outlet of the extruder gradually presents the normal shape of a foam board, and is pulled from the front puller to the rear puller, and after de-edging and flying sawing, it is cooled in a cooling tower, and then passed through a planer before being stacked; The screw speed of the extruder is 17-19RPM; 5) Welding After the plate is cooled for 2 days, it is welded to the corresponding length as required; 6) Cutting After the welded plates are cooled for 2 days, they are cut into sheets of different sizes according to needs.
7. The composite sandwich panel according to claim 4, It is characterized in that The PVC foam board comprises the following raw materials in parts by weight: 75-80 parts of polyvinyl chloride, 1.3-1.7 parts of a stabilizer, 7-8 parts of a regulator, 1.1-1.8 parts of a foaming agent, and 12-18 parts of a lubricant.
8. The composite sandwich panel according to claim 4, It is characterized in that The SAN foam board comprises the following raw materials in parts by weight: 75-85 parts of styrene, 7-10 parts of acrylonitrile, 1.0-1.5 parts of a crosslinking agent, 2.5-3.2 parts of a nucleating agent, 1.8-2.1 parts of a chain extender, 3-5 parts of a lubricant, and 0.3-1.0 parts of a foaming agent.
9. A method for preparing the composite sandwich panel according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The foam board is bonded to both sides of the wood board by adhesive.
10. An application of the composite sandwich panel material according to any one of claims 1 to 7, It is characterized in that The composite sandwich panel is applied to the blade root of a wind turbine blade.
Citation Information
Patent Citations
Megawatt level composite material wind electricity blade vacuum guiding and forming technique
CN101456256A
Cores for composite material sandwich panels
CN110198833A
Automotive interior trim part
CN202368005U
Lightweight material and method of production
EP1524105A2
Method for producing compound components
EP2886322A1
Cited By
High-performance sandwich wind power blade core material and preparation method thereof
CN120862818A