MEMS sensor anti-corrosion process

Deposition of fluorine-containing coatings through CVD technology solves the protection problem of MEMS sensors in multi-layer sealing structures, achieves high accuracy and stable performance, is suitable for harsh environments, and reduces costs, solving the accuracy problem of low-pressure sensors.

CN119018845AInactive Publication Date: 2024-11-26WUXI HAOBANG HIGH TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135068.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing MEMS sensors are difficult to effectively protect electrical connections and gaps in multi-layer sealing structures, and the gel coating of low-pressure sensors affects sensitivity and accuracy, and cannot meet the accuracy requirements and application requirements in harsh environments.

Method used

The fluorine-containing coating is deposited with a thickness of 2um to 3um, filled with tiny gaps and defects, providing uniform coating and protection, and reducing costs through fluorine-containing CVD coating, and is compatible with microelectronic integrated circuit processes.

Benefits of technology

It realizes effective protection of MEMS sensors, maintains high accuracy and stable performance, is suitable for harsh environments, reduces costs and meets the accuracy requirements of low-pressure sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018845A_ABST
    Figure CN119018845A_ABST
Patent Text Reader

Abstract

The invention relates to an MEMS sensor anticorrosion technology, and belongs to the technical field of MEMS sensors, and the MEMS sensor anticorrosion technology comprises the following steps: S1, fixedly pasting a conditioning circuit on a substrate through conditioning circuit bonding glue; step S2, an MEMS sensor is fixedly pasted on the conditioning circuit through an MEMS adhesive; s3, bonding an electric connection wire; according to the method, the CVD coating technology is adopted, so that the method has imperforate permeability and excellent coating characteristics, the coating is compact and free of pinholes, tiny gaps, defects and the like in a multi-layer stacked sealing structure can be effectively filled, uniform coating can be achieved, and effective protection is achieved; the fluorine-containing CVD coating is adopted and is compatible with a microelectronic integrated circuit process, so that a thin film coating with the thickness of dozens of nanometers to dozens of microns required in different applications can be realized, effective protection can be realized for a low-pressure coating with the pressure of less than 30kPa and the precision requirement can be met, and the stable performance can be kept in various severe environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a MEMS sensor anti-corrosion process, belonging to the technical field of micro-electromechanical sensors. Background Art

[0002] MEMS (Micro Electro Mechanical Systems) integrates sensors and micro-electromechanical systems by integrating multiple micro-nano technologies. It can be used to measure and detect various physical quantities, such as pressure, temperature, flow, acceleration, angular velocity, humidity, etc. Among them, pressure sensors are the most widely used type of MEMS sensors. Pressure sensors are one of the most widely used MEMS sensors, and their applications cover many fields such as automobiles, medical care, consumption, industry, and defense. The general application of pressure sensors is dry gas applications in non-corrosive, non-ionic fluid media.

[0003] With the continuous advancement of science and technology, the continuous development of the Internet of Things, AI, and big data, the application scenarios of sensors are becoming more and more abundant, and the performance requirements for sensors are also constantly increasing, requiring sensors to be miniaturized, intelligent, low-cost, highly reliable, and able to be used in application scenarios in harsh environments. For example, MEMS may be used in application scenarios that require waterproofing, corrosion resistance, and biocompatibility. Because the structure and connection lines of MEMS sensors are more sensitive to environmental media, special protection is required to ensure the sensitivity, zero point stability, accuracy, and reliability of the sensor.

[0004] The Chinese utility model patent with announcement number CN215677407U discloses a pressure sensor. The pressure sensor includes: a shell, a pressure sensing chip and at least two layers of elastic waterproof glue. A housing space is provided in the shell, and the pressure sensing chip is arranged in the housing space. The at least two layers of elastic waterproof glue are sequentially filled in the aforementioned housing space in a direction away from the pressure sensing chip. The first layer of elastic waterproof glue covers and wraps the pressure sensing chip. The pressure sensor provided by the utility model has good waterproof reliability and can ensure that the pressure sensor has good waterproof performance under high pressure environment. However, the prior art still has the following deficiencies:

[0005] 1. When the MEMS sensor adopts a multi-layer stacking structure, the size is small, and the electrical connection spacing between ASIC (conditioning circuit, Application Specific Integrated Circuit, also known as application-specific integrated circuit), MEMS and substrate may be less than 25um, and there may be small gaps with characteristic sizes less than 25um between layers. The viscosity of the gel is relatively large, and it is difficult to completely cover the electrical connections with a spacing as small as 25um and the gaps between multiple layers. Therefore, it is difficult to effectively protect the sensor from corrosion by the medium, and the electrical connections may be short-circuited or corroded. Risks;

[0006] 2. For pressure sensors below 30kPa, gel is coated on the sensor surface. The weight of the gel on the sensor's sensitive film and the bubbles in the gel affect the sensitivity, zero point, and accuracy of the sensor. The accuracy is related to the sensor's sensitive film area, gel density, and thickness, and the accuracy is affected by more than 1%.

[0007] Therefore, there is a need for a MEMS sensor anti-corrosion process that can reduce costs, achieve effective protection and meet accuracy requirements. Summary of the invention

[0008] The technical problem to be solved by the present invention is: in order to overcome the deficiencies of the prior art, a MEMS sensor anti-corrosion process is provided that realizes effective protection and meets the accuracy requirements.

[0009] The technical solution adopted by the present invention to solve the above problem is: a MEMS sensor anti-corrosion process, comprising the following steps:

[0010] Step S1, fixing the conditioning circuit on the substrate by using conditioning circuit adhesive;

[0011] Step S2, fixing the MEMS sensor on the conditioning circuit by using MEMS adhesive;

[0012] Step S3, bonding electrical connections;

[0013] Use wires to connect the pads on the conditioning circuit and the MEMS sensor to the pads on the substrate to achieve electrical connection;

[0014] Step S4, mounting the housing;

[0015] Step S5, disposing a removable protective adhesive layer on the back of the substrate;

[0016] Step S6, MEMS sensor surface coating;

[0017] A fluorine-containing coating is deposited on the surface of the sensor by CVD;

[0018] Step S7, removing the protective adhesive layer on the back of the substrate;

[0019] Step S8: cutting the substrate to form individual sensor packages.

[0020] Preferably, in step S1, the substrate is designed as a jigsaw puzzle.

[0021] Preferably, in step S8, the substrate is cut according to a jigsaw structure.

[0022] Preferably, the step S1 specifically comprises the following steps:

[0023] Step S1.1, coating a conditioning circuit adhesive on the substrate;

[0024] Step S1.2, bonding the conditioning circuit to the substrate;

[0025] Step S1.3, curing and conditioning the circuit adhesive.

[0026] Preferably, the step S2 specifically includes the following steps:

[0027] Step S2.1, applying MEMS adhesive on the conditioning circuit;

[0028] Step S2.2, bonding the MEMS sensor to the conditioning circuit;

[0029] Step S2.3, curing the MEMS adhesive.

[0030] Preferably, in step S4, the shell is made of metal or plastic.

[0031] Preferably, the shell material is metal, and the shell is bonded to the substrate by reflow.

[0032] Preferably, the shell material is plastic and is bonded by glue.

[0033] Preferably, in step S6, the coating thickness is 2um to 3um.

[0034] Preferably, the substrate is made of FR4 or ceramic.

[0035] Compared with the prior art, the advantages of the present invention are:

[0036] 1. Through CVD coating technology, it has all-pervasive penetration and excellent coating characteristics. The coating is dense and pinhole-free. It can effectively fill the tiny gaps and defects in the multi-layer stacking structure and achieve uniform coating, that is, to achieve effective protection;

[0037] 2. By adopting fluorine-containing CVD coating, which is compatible with microelectronic integrated circuit technology, thin film coatings with thicknesses of tens of nanometers to tens of microns required in different applications can be achieved. For low-pressure coatings below 30kPa, 2um to 3um coatings can achieve effective protection and meet precision requirements, and can maintain stable performance in various harsh environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 is a cross-sectional view of a single sensor package;

[0039] Figure 2 for Figure 1 A magnified view of part A;

[0040] Figure 3 for Figure 1 A magnified view of part B;

[0041] Figure 4 It is a schematic diagram of the structure of the base plate panel;

[0042] Figure 5 It is a schematic diagram of the packaging structure of the MEMS sensor substrate panel;

[0043] Figure 6 It is a schematic diagram of the structure of the protective adhesive layer;

[0044] Figure 7 It is a top view of a single sensor package;

[0045] Figure 8 It is a bottom view of a single sensor package;

[0046] Fig. 9 This is a line chart of the accuracy data of non-fluorinated Parylene coating sensors;

[0047] Fig.10 It is a line chart of the accuracy data of the fluorinated Parylene coating sensor;

[0048] Fig.11 This is a line graph of the sensitivity change of the sensor before fluorine-containing CVD coating;

[0049] Fig.12 This is a line graph showing the change in accuracy of the sensor before and after fluorine-containing CVD coating.

[0050] Among them: conditioning circuit 1, conditioning circuit adhesive 2, substrate 3, MEMS sensor 4, MEMS adhesive 5, wire 6, shell 7, protective adhesive layer 8, coating 9, pad 10. DETAILED DESCRIPTION

[0051] like Figures 1 to 8 As shown, a MEMS sensor anti-corrosion process in this embodiment includes the following steps:

[0052] Step S1, fix the conditioning circuit 1 on the substrate 3 by using the conditioning circuit adhesive 2;

[0053] Step S1.1, coating the conditioning circuit adhesive 2 on the substrate 3;

[0054] Step S1.2, bonding the conditioning circuit 1 to the substrate 3;

[0055] Step S1.3, curing and conditioning the circuit adhesive 2;

[0056] In order to improve the coating efficiency, the substrate 3 is designed as a jigsaw puzzle. The substrate 3 is made of FR4 or ceramic. FR4 is a common composite material and is widely used in the electronic and electrical industry. FR4 is a thermosetting plastic composite material composed of glass fiber and epoxy resin, and has excellent insulation, mechanical strength and heat resistance.

[0057] Step S2, fix the MEMS sensor 4 on the conditioning circuit 1 by using the MEMS adhesive 5;

[0058] Step S2.1, applying MEMS adhesive 5 on the conditioning circuit 1;

[0059] Step S2.2, bonding the MEMS sensor 4 to the conditioning circuit 1;

[0060] Step S2.3, curing the MEMS adhesive 5;

[0061] Step S3, bonding electrical connections;

[0062] Use wires 6 to respectively connect the pads 10 on the conditioning circuit 1 and the MEMS sensor 4 to the pads 10 on the substrate 3 to achieve electrical connection;

[0063] Step S4, mounting the housing 7;

[0064] The shell 7 is made of metal or plastic;

[0065] When the shell 7 is made of metal, the shell 7 is bonded to the substrate 3 by reflow.

[0066] When the shell 7 is made of plastic, it is bonded by glue;

[0067] Step S5, a removable protective adhesive layer 8 is provided on the back of the substrate 3;

[0068] A removable protective adhesive layer 8 is attached or coated on the back of the substrate 3 to protect the pads 10 on the back of the substrate 3 from being covered by the film during the coating process and thus affecting the electrical connection of the MEMS sensor 4;

[0069] Step S6, coating 9 on the surface of the MEMS sensor 4;

[0070] A fluorine-containing coating 9 is deposited on the surface of the sensor by CVD (Chemical Vapor Deposition), and the thickness of the coating 9 is 2um to 3um. Since the CVD technology has all-pervasive penetration performance and excellent coating characteristics, the coating 9 is dense and pinhole-free, and can effectively fill the tiny gaps and defects in the multi-layer stacking structure and achieve uniform coating. Therefore, the coating 9 has good shielding and isolation capabilities, and can shield the corrosive measurement medium during use;

[0071] Step S7, removing the protective adhesive layer 8 on the back side of the substrate 3;

[0072] Step S8, cutting the substrate 3 according to the jigsaw structure to form a single sensor package;

[0073] In addition, the CVD coating 9 is composed of fluorinated Parylene, which is a protective polymer material. It is vapor-deposited under vacuum. The good penetrating power of Parylene active molecules can form a pinhole-free, uniformly thick transparent insulating coating inside, at the bottom, and around the component, providing the component with a complete high-quality protective coating to resist the invasion of acid, alkali, salt spray, mold, and various corrosive gases. It has excellent waterproof, moisture-proof, dust-proof and corrosion-resistant properties and is suitable for various harsh environments. Of course, the CVD coating 9 is not limited to fluorinated Parylene, and other ingredients that can achieve the same effect are also acceptable.

[0074] It should be noted that most of the current fluorine-containing adhesives are imported and are relatively expensive, while the fluorine-containing CVD coating 9 has been domestically produced, and the cost of using the fluorine-containing CVD coating 9 can be reduced by at least 5%;

[0075] Moreover, most pressure sensor applications require high-temperature reflow soldering process, with the highest reflow temperature reaching 220°C. The working temperature of ordinary Parylene protective coating is about 120°C. During high-temperature reflow, the coating is destroyed and cannot be effectively protected and used. However, fluorine-containing CVD coating 9 is both waterproof and anti-corrosive, and can withstand high temperatures.

[0076] The sensor accuracy data of fluorine-containing CVD coating and non-fluorine-containing CVD coating before and after reflow was obtained. Figure 9-10 ;

[0077] in, Fig. 9 This is a line chart of the accuracy data of the non-fluorinated Parylene coating sensor, and the coating thickness is 2.5um. According to the data, it can be concluded that the accuracy before and after high-temperature reflow is compared. During high-temperature reflow, the sensor accuracy deteriorates. After two reflows, the accuracy becomes worse, exceeding the product accuracy requirements.

[0078] Fig.10This is a line chart of the accuracy data of the fluorine-containing Parylene coating sensor, and the coating thickness is 2.5um. According to the data, it can be concluded that the accuracy of the fluorine-containing coating does not change much before and after reflow, and is basically within the range of 0.25% FS, which meets the accuracy requirements of the product;

[0079] Secondly, for harsh application scenarios such as anti-corrosion and waterproofing with low pressure <30kPa, if fluorinated silicone is used to protect the chip, for stacked products, the thickness of the silicone is up to 100 microns, and the weight of the silicone will affect the accuracy and sensitivity of the sensor. However, if a lightweight fluorinated CVD coating 9 is used, a coating thickness of 2um to 3um can form a dense, pinhole-free protective layer, and the weight has a negligible effect on the sensitivity of the sensor.

[0080] Sensitivity formula:

[0081] Among them, S is the sensitivity, ΔV is the change in the output signal when the sensor surface is under pressure, ΔP is the change in the corresponding pressure, Vin is the bridge voltage, and the unit of S is usually mV, V, MPa;

[0082] If silica gel is used, the weight of silica gel causes ΔP to be larger than the actual value, resulting in a smaller S sensitivity, while the weight of fluorine-containing CVD is negligible compared to the actual ΔP;

[0083] Fig.11 This is a line chart of sensitivity change of fluorine-containing sensor before CVD coating. The coating thickness is 2.5um. According to the data, it can be concluded that the sensitivity is slightly lower, but the change rate does not exceed 0.5%, which can be ignored.

[0084] Fig.12 This is a line chart of the accuracy change of the sensor before and after fluorine-containing CVD coating. The coating thickness is 2.5um. According to the data, the accuracy becomes higher, ±0.4% FS before coating and ±0.25% FS after coating. The main reason is that the fluorine-containing coating can prevent moisture, humidity and corrosion, so that the sensor can still maintain good accuracy in a harsh environment;

[0085] In summary, by adopting the fluorine-containing CVD coating 9, which is compatible with the microelectronic integrated circuit process, a thin film coating 9 with a thickness of tens of nanometers to tens of microns required in different applications can be achieved. For low-pressure coatings below 30kPa, 2um to 3um can achieve effective protection and meet the precision requirements, and can maintain stable performance in various harsh environments. Moreover, through the CVD coating 9 technology, it has pervasive penetration performance and excellent coating characteristics. The coating 9 is dense and pinhole-free, and can effectively fill the tiny gaps and defects in the multi-layer stacking structure and achieve uniform coating, that is, effective protection is achieved.

[0086] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A MEMS sensor anti-corrosion process, characterized in that: The steps include: Step S1, fixing the conditioning circuit (1) on the substrate (3) by using the conditioning circuit adhesive (2); Step S2, fixing the MEMS sensor (4) on the conditioning circuit (1) by using the MEMS adhesive (5); Step S3, bonding electrical connections; Using wires (6) to respectively connect the pads (10) on the conditioning circuit (1) and the MEMS sensor (4) to the pads (10) on the substrate (3) to achieve electrical connection; Step S4, mounting the housing (7); Step S5, disposing a removable protective adhesive layer (8) on the back side of the substrate (3); Step S6, coating (9) the surface of the MEMS sensor (4); Depositing a fluorine-containing coating (9) on the surface of the sensor by CVD; Step S7, removing the protective adhesive layer (8) on the back side of the substrate (3); Step S8, cutting the substrate (3) to form a single sensor package.

2. A MEMS sensor anti-corrosion process according to claim 1, characterized in that: In the step S1, the base plate (3) is designed as a jigsaw puzzle.

3. A MEMS sensor anti-corrosion process according to claim 2, characterized in that: In the step S8, the substrate (3) is cut according to the jigsaw structure.

4. The MEMS sensor anti-corrosion process according to claim 1, characterized in that: The step S1 specifically includes the following steps: Step S1.1, coating a conditioning circuit adhesive (2) on a substrate (3); Step S1.2, bonding the conditioning circuit (1) to the substrate (3); Step S1.3, curing and conditioning the circuit adhesive (2).

5. The MEMS sensor anti-corrosion process according to claim 1, characterized in that: The step S2 specifically includes the following steps: Step S2.1, applying MEMS adhesive (5) on the conditioning circuit (1); Step S2.2, bonding the MEMS sensor (4) to the conditioning circuit (1); Step S2.3, curing the MEMS adhesive (5).

6. The MEMS sensor anti-corrosion process according to claim 1, characterized in that: In the step S4, the shell (7) is made of metal or plastic.

7. A MEMS sensor anti-corrosion process according to claim 6, characterized in that: The shell (7) is made of metal, and the shell (7) is bonded to the substrate (3) by a reflow method.

8. The MEMS sensor anti-corrosion process according to claim 6, characterized in that: The shell (7) is made of plastic and is bonded by glue.

9. The MEMS sensor anti-corrosion process according to claim 1, characterized in that: In the step S6, the coating (9) has a thickness of 2 um to 3 um.