Preparation method of crosslinked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres

Through the preparation of crosslinked cellulose/carbon nanotubes/molybdenum disulfide hard carbon microspheres, the problems of low sodium storage capacity, large volume expansion and poor cycle life of sodium ion battery negative electrode materials are solved, and efficient sodium ion storage and Long-life electrode material, suitable for sodium ion batteries, has cost advantages and environmental friendliness.

CN119018875AActive Publication Date: 2024-11-26SICHUAN UNIV

Patent Information

Application Number
CN202310607683.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

The negative electrode materials of sodium ion batteries have problems such as low sodium storage capacity, large volume expansion and poor cycle life. The existing materials also have shortcomings in cost and environmental friendliness, making it difficult to meet the needs of the new energy industry.

Method used

The preparation method of crosslinked cellulose/carbon nanotubes/molybdenum disulfide hard carbon microspheres is adopted, and crosslinked cellulose/carbon nanotubes/disulfide with large pore structures and rich microporous structures is formed. Molybdenum hard carbon microspheres, an anode material for sodium ion batteries.

Benefits of technology

It achieves a high sodium storage capacity of 627 mAh/g and high Curlun first effect of more than 88%, while reducing the volume expansion rate, extending the cycle life of the electrode, and having environmentally friendly characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to a preparation method of crosslinked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres. Belongs to the field of battery cathode materials. The preparation method comprises the following steps: firstly, mechanically stirring microcrystalline cellulose and carbon nanotubes in an alkali urea system, cross-linking with epoxy chloropropane, and emulsifying into balls to obtain cross-linked cellulose / carbon nanotube composite microspheres; then, the crosslinked cellulose / carbon nanotube microspheres and an ammonium molybdate solution are swelled, and a carbonized precursor is obtained through high-temperature hydrothermal treatment; and finally, carrying out low-temperature dehydration and high-temperature carbonization on the precursor in a tubular furnace to obtain the crosslinked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres. The negative electrode material has a wrinkled surface and a microporous structure, and can improve the permeability of an electrolyte and promote mass transfer. Compared with the prior art, the cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microsphere negative electrode material prepared by the invention has the advantages of high specific capacity and high coulomb first efficiency, and is suitable for the field of high-capacity sodium ion battery negative electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a battery negative electrode material, and in particular to a method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres. Background Art

[0002] The development of the new energy industry has put forward higher requirements for secondary energy storage batteries. As a new type of secondary energy storage battery, sodium ion batteries (SIBs) have attracted great attention in recent years. Sodium ion batteries are safe and low-cost, especially in the environment where the cost of cobalt, copper and lithium resources is rising rapidly, sodium ion batteries have more prominent cost advantages. However, compared with lithium ion batteries (LIBs), sodium ions have larger ionic radius and solvation radius, so that solvated sodium ions are difficult to freely deintercalate in commercial graphite. Therefore, common electrodes such as graphite cannot be used as negative electrodes for sodium ion batteries. Therefore, it is of great significance to develop negative electrode materials that are more suitable for sodium ion batteries. Similarly, metal alloy negative electrode materials also have the characteristics of high specific capacity and high first efficiency. For example, Abel et al. found that the capacity retention rate of dense Ge film electrodes dropped sharply after multiple cycles under the condition of high initial capacity. Komaba et al. found that Sn also had the problem of capacity retention rate far lower than the theoretical value after multiple cycles under the condition of high theoretical capacity. However, high-capacity negative electrode materials such as B, P, As and Bi of the fifth main group are difficult to achieve engineering conditions due to their low abundance. Conversion materials represented by sulfides and phosphides undergo an embedding or alloying reaction during the conversion reaction. However, while these materials have high specific capacity, they also have the disadvantage of structural damage due to huge volume changes. At the same time, conversion materials, like some organic materials, have the problem of environmental pollution. Therefore, finding a high-capacity, low-cost battery negative electrode material has become the key to the development of sodium-ion batteries.

[0003] Hard carbon material is a graphite-like material with short-range order, long-range disorder, and rich pseudo-bulk graphitized domains. Its irregular ion channels and large interlayer spacing facilitate the rapid insertion and extraction of sodium ions. At the same time, hard carbon materials have the advantages of high specific capacity, low sodium storage voltage, stable cycle and environmental friendliness, which makes it a negative electrode material with great development potential. However, hard carbon materials also have the characteristics of low Coulomb efficiency and poor cycle life, which seriously restricts the further development of hard carbon materials. Molybdenum disulfide is a two-dimensional layered metal alloy compound. The sodium storage behavior of molybdenum disulfide has been widely studied. It mainly relies on alloy transformation to store sodium. The current highest experimental sodium storage capacity is 640 mAh / g, which is much higher than hard carbon. However, due to the large volume expansion of molybdenum disulfide during charging and discharging, the volume expansion rate is usually as high as 130%, so the powdering of molybdenum disulfide electrode is more serious, which is not conducive to the formation of a stable SEI film. Based on the above characteristics, the strategy of molybdenum disulfide / carbon composite can effectively inhibit the expansion of molybdenum disulfide electrode and increase the cycle life of electrode. Summary of the invention

[0004] In view of the shortcomings of the background technology, the present invention provides a method for preparing a cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microsphere which is suitable for both industrial applications and laboratories and has high sodium storage capacity, low volume expansion rate and good cycle life. The specific scheme is as follows: A method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres, characterized in that: (1) Preparation of cross-linked cellulose / carbon nanotube microspheres: 5.0 g microcrystalline cellulose, 8.0 g NaOH, and 6.0 g thiourea were added to 85 mL deionized water, and mechanically stirred in an ice-water bath at 500 r / min for 10 min. Then, 0-2.0 mg carbon nanotubes were added and mechanically stirred until a black suspension was obtained. Then, 0-2.0 mL epichlorohydrin was added to form an aqueous phase. 80 mL white oil, 160 mL isooctane, 2.5 g Tween-80, and 8.0 g Span-80 were prepared to form an oil phase. Under mechanical stirring at 500 r / min, 20 mL of the aqueous phase was dispersed into 240 mL of the oil phase for 20 min. Then, 240 mL of 75% ethanol was used to regenerate the microspheres. The microspheres were centrifuged at 7500 r / min, washed three times with 100 mL of ethanol, and then freeze-dried under reduced pressure to obtain the finished cross-linked cellulose / carbon nanotube microspheres. (2) Preparation of cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres: 0-8.0 g ammonium molybdate tetrahydrate and 8.0 g thiourea were dissolved in 100 mL deionized water, and then 0-6.0 g of the cross-linked cellulose / carbon nanotube microspheres obtained in the previous step were added. The mixture was mechanically stirred at 30 °C for 48 h, and then transferred to a polytetrafluoroethylene-lined autoclave, kept at 200 °C for 18 h, and then centrifuged at 7500 r / min to obtain cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres. The microspheres were repeatedly rinsed with 250 mL deionized water for 3-5 times and dried at 65 °C for 24 h. (3) Carbonization process: Heating: 50 ~ 180℃ heating for 60 min, keep at 180℃ for 60 min, heating from 180 ~ 230℃ for 1800 min, keep at 230℃ for 60 min, heating from 230 ~ 1350℃ for 375 min, keep at 1350℃ for 120 min; Cooling: cool down to 200℃ at 3℃ / min, then stop heating.

[0005] As a preference: (1) A method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres as claimed in claim 1, characterized in that in the preparation process of the cross-linked cellulose / carbon nanotube microspheres cited in step (1), the amount of carbon nanotubes added is 0 to 2.0 mg, and the amount of epichlorohydrin added is 0 to 2.0 mL; (2) The method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres as claimed in claim 1, characterized in that in the preparation process of the cross-linked cellulose / carbon nanotube microspheres cited in step (1), the mass ratio of alcohol to water for regenerating the microspheres using 240 mL 75% ethanol is ethanol: water = 1:9 to 9:1; (3) The method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres according to claim 1, characterized in that in the preparation process of the cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres cited in step (2), the amount of ammonium molybdate tetrahydrate used is 0 to 8.0 g; (4) The method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres according to claim 1, characterized in that in the preparation process of the cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres cited in step (2), the mass of the cross-linked cellulose / carbon nanotube microspheres added is 0 to 6.0 g; (5) A method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres as claimed in claim 1, characterized in that in the carbonization process cited in step (3), the first dehydration temperature is increased from 50 to 180°C for 60 min, and then kept at 180°C for 60 min; The method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres as claimed in claim 1, characterized in that the carbonization process cited in step (3) is kept at 1350°C for 120 min, and the carbonization temperature is 900~1600°C.

[0006] The beneficial effects of the present invention are as follows: 1) The present invention uses cross-linked cellulose / carbon nanotube microspheres as carriers and adopts a spatially confined manner to in-situ grow molybdenum disulfide nanosheets on the surface of the microspheres to obtain cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres; Through low-temperature dehydration and high-temperature carbonization, cross-linked cellulose / carbon nanotubes / molybdenum disulfide hard carbon microspheres are obtained; The cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres prepared by the present invention have interconnected macroporous structures and abundant microporous structures, which are conducive to the rapid penetration of electrolytes; The cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres prepared by the present invention have a sodium storage capacity of up to 627 mAh / g for NaPF6 electrolyte, and a coulombic first efficiency of more than 88%. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] Figure 1 : Schematic diagram, SEM scanning electron microscope image, particle size distribution, thermogravimetric, and pore size distribution diagram of the method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres; Figure 2 : TEM transmission electron microscope image, XRD, Raman spectrum and XPS characterization image of cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres prepared by the method of the present invention; Figure 3 :The half-cell cyclic voltammetry curve, EIS impedance curve, constant current charge and discharge curve, rate performance and cycle performance curve of cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres prepared by the method of the present invention. DETAILED DESCRIPTION

[0008] The following examples further illustrate the content of the present invention, but should not be construed as limiting the present invention. Without departing from the spirit and essence of the present invention, modifications or substitutions made to the methods, steps or conditions of the present invention all fall within the scope of the present invention.

[0009] Example 1 Cross-linked cellulose / carbon nanotubes / molybdenum disulfide hard carbon microspheres.

[0010] 1. Preparation of cross-linked cellulose / carbon nanotubes / molybdenum disulfide hard carbon microspheres In this example, the preparation of cross-linked cellulose / carbon nanotubes by the microemulsion method is used as the starting step. First, nano-molybdenum disulfide is in situ grown on the surface of the cross-linked cellulose / carbon nanotube microspheres by the spatial confinement method, and then it is carbonized at high temperature to obtain cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres.

[0011] (1) Preparation of cross-linked cellulose / carbon nanotube microspheres 5.0 g microcrystalline cellulose, 8.0 g NaOH, and 6.0 g thiourea were added to 85 mL deionized water, and mechanically stirred in an ice-water bath at 500 r / min for 10 min. Then, 0.5 mg carbon nanotubes were added, and mechanically stirred until a black suspension was obtained. Then, 1.5 mL epichlorohydrin was added to form an aqueous phase. 80 mL white oil, 160 mL isooctane, 2.5 g Tween-80, and 8.0 g Span-80 were prepared to form an oil phase. Under mechanical stirring at 500 r / min, 20 mL of the aqueous phase was dispersed into 240 mL of the oil phase for 20 min, and then 240 mL of 75% ethanol was used to regenerate the spheres. The spheres were centrifuged at 7500 r / min, washed 3 times with 100 mL of ethanol, and then freeze-dried under reduced pressure to obtain the finished cross-linked cellulose / carbon nanotube microspheres. (2) Preparation of cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres 4.0 g of ammonium molybdate tetrahydrate and 8.0 g of thiourea were dissolved in 100 mL of deionized water, and then 2.0 g of the cross-linked cellulose / carbon nanotube microspheres obtained in the previous step were added, and mechanical stirring was carried out at 30°C for 48 h. The mixture was transferred to a polytetrafluoroethylene-lined autoclave, kept at 200°C for 18 h, and then centrifuged at 7500 r / min to obtain cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres. The microspheres were repeatedly rinsed with 250 mL of deionized water for 3 to 5 times and dried at 65°C for 24 h. (3) Carbonization process Heating: 50 ~ 180℃ for 60 min, keep at 180℃ for 60 min, 180 ~ 230℃ for 1800 min, keep at 230℃ for 60 min, 230 ~ 1350℃ for 375 min, keep at 1350℃ for 120 min; Cooling: cool down to 200℃ at 3℃ / min, then stop heating.

[0012] 2. Half-cell assembly Half-cell assembly and testing, preparation of negative electrode sheet: 0.92 g cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres, 0.03 g Super P, 0.10 g 1.5 wt% sodium carboxymethyl cellulose solution, 0.07 g 40 wt% styrene-butadiene rubber solution, 0.60 g deionized water, homogenized for 20 min, using a four-sided preparation device, the slurry is evenly applied to the surface of a single-sided polished copper foil with a thickness of 100 μm, dried at 105 ° C for 8 h, and the sheet diameter of the sheet cutter is 12 mm; preparation of positive electrode sheet: metallic sodium is pressed to a thickness of 0.8 mm using a roller press, and the sheet diameter is 12 mm; button cell assembly order (from bottom to top): positive electrode shell, spring, gasket, sodium sheet, glass fiber separator, sodium hexafluorophosphate electrolyte (1 mol / L NaPF 6 Dissolved in ethylene carbonate: ethylene carbonate, volume ratio of 1:1), negative electrode sheet, negative electrode shell. All assembly processes are carried out in an anaerobic chamber (O 2 concentration ≤ 0.5 ppm, water concentration ≤ 0.1 ppm).

Claims

1. A method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres, characterized in that The steps include: (1) Preparation of cross-linked cellulose / carbon nanotube microspheres: 5.0 g microcrystalline cellulose, 8.0 g NaOH, and 6.0 g thiourea were added to 85 mL deionized water, and mechanically stirred in an ice-water bath at 500 r / min for 10 min. Then, 0.5 mg carbon nanotubes were added and mechanically stirred until a black suspension was obtained. Then, 1.5 mL epichlorohydrin was added to form an aqueous phase. 80 mL white oil, 160 mL isooctane, 2.5 g Tween-80, and 8.0 g Span-80 were prepared to form an oil phase. Under mechanical stirring at 500 r / min, 20 mL of the aqueous phase was dispersed into 240 mL of the oil phase for 20 min, and then 240 mL of 75% ethanol was used to regenerate the microspheres. The microspheres were centrifuged at 7500 r / min, washed three times with 100 mL of ethanol, and then freeze-dried under reduced pressure to obtain the finished cross-linked cellulose / carbon nanotube microspheres. (2) Preparation of cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres: 4.0 g of ammonium molybdate tetrahydrate and 8.0 g of thiourea were dissolved in 100 mL of deionized water, and then 2.0 g of the cross-linked cellulose / carbon nanotube microspheres obtained in the previous step were added. The mixture was mechanically stirred at 30 °C for 48 h, transferred to a polytetrafluoroethylene-lined autoclave, kept at 200 °C for 18 h, and then centrifuged at 7500 r / min to obtain cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres. The microspheres were repeatedly rinsed with 250 mL of deionized water for 3 to 5 times and dried at 65 °C for 24 h. (3) Carbonization process: Heating: 50 ~ 180℃ heating for 60 min, 180℃ holding for 60 min, 180 ~ 230℃ heating for 1800 min, 230℃ holding for 60 min, 230 ~ 1350℃ heating for 375 min, 1350℃ holding for 120 min; Cooling: Cool down to 200℃ at 3℃ / min, then stop heating.

2. The method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres according to claim 1, characterized in that In the preparation process of cross-linked cellulose / carbon nanotube microspheres cited in step (1), the amount of carbon nanotubes added is 0~2.0 mg.

3. The method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres according to claim 1, characterized in that In the preparation process of the cross-linked cellulose / carbon nanotube microspheres cited in step (1), the mass ratio of alcohol to water for regenerating the microspheres using 240 mL of 75% ethanol is ethanol: water = 1:9 to 9:

1.

4. The method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres according to claim 1, characterized in that In the preparation process of the cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres cited in step (2), the amount of ammonium molybdate tetrahydrate used is 0 ~ 8.0 g.

5. The method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres according to claim 1, characterized in that In the preparation process of cross-linked cellulose / carbon nanotube / molybdenum disulfide microspheres cited in step (2), the mass of cross-linked cellulose / carbon nanotube microspheres added is 0 ~ 6.0 g.

6. The method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres according to claim 1, characterized in that In the carbonization process described in step (3), the first dehydration temperature is raised from 50 to 180°C for 60 min and then kept at 180°C for 60 min.

7. The method for preparing cross-linked cellulose / carbon nanotube / molybdenum disulfide hard carbon microspheres according to claim 1, characterized in that In the carbonization process described in step (3), the temperature is kept at 1350°C for 120 min, and the carbonization temperature is 900 ~ 1600°C.

Citation Information

Patent Citations

  • Chitosan microspheres prepared from chitosan solution with pH value of 6-8 and preparation method of chitosan microspheres

    CN111748109A

  • Process for producing an electron emitter with a coating containing carbon nanotubes

    DE102016013279A1

  • Physical separate-phase dynamic polymer and use thereof

    WO2018137507A1

Cited By

  • Ammonia-oxidized lignin-coated cellulose-based hard carbon negative electrode material as well as preparation method and application thereof

    CN121085242A