Waste graphite-based regenerated negative electrode active material as well as preparation and application thereof

Through pre-oxidation, mechanical assistance and carbon coating technology, the problem of unsatisfactory regeneration performance of the graphite anode material of waste lithium-ion batteries is solved, and recycled graphite materials with excellent electrochemical properties are prepared, achieving efficient recycling and recycling.

CN119018888AActive Publication Date: 2024-11-26CENT SOUTH UNIV

Patent Information

Application Number
CN202411136857.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The regeneration performance of graphite negative electrode materials in waste lithium-ion battery recycling is not ideal, and it is difficult to adapt to high magnification and long-range cycle requirements, resulting in high recycling costs and unsatisfactory benefits.

Method used

Using pre-oxidation treatment, mechanical auxiliary treatment, combined treatment of reagent A and reagent B, combined with carbon coating technology, it selectively removes harmful impurities in graphite, optimizes its surface structure and stability, and prepares excellent electrochemistry Performance of recycled graphite negative electrode active material.

Benefits of technology

It realizes excellent fast charging and long-range cycle stability of recycled graphite materials, reduces recycling costs, and improves the recycling efficiency of graphite resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018888A_ABST
    Figure CN119018888A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of waste graphite regeneration, and particularly relates to a preparation method of a waste graphite-based regenerated negative electrode active material, which comprises the following steps: carrying out pre-oxidation treatment on a waste graphite material stripped from a waste battery in an oxidizing atmosphere, putting into a reagent A, and carrying out first-stage treatment under mechanical assistance; the preparation method comprises the following steps: adding a reagent A (with addition of # imgabs0 #) into a reactor, mixing with a reagent B (with addition of # imgabs0 #), sealing in a closed container, carrying out second-stage treatment, mixing the second-stage treatment material with a carbon source and a transition metal catalyst, molding, carbonizing, and carrying out carbon coating treatment to obtain the regenerated graphite negative electrode active material. The method provided by the invention can significantly improve the performances such as fast charging and intestinal circulation of the regenerated graphite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of waste battery recycling, and in particular relates to the field of waste battery negative electrode regeneration. Background Art

[0002] Lithium-ion batteries have been widely used in various fields due to their high energy density, long service life and good safety. However, this has also led to an increase in the amount of lithium-ion battery scrap and the problem of the proper disposal of waste lithium-ion batteries. Currently, the research focus on the recycling of waste lithium-ion batteries is concentrated on the positive electrode, and there is little research on the recycling of graphite negative electrode materials. Most companies treat waste graphite powder as solid waste, which not only wastes graphite resources, but also causes environmental pollution.

[0003] Because most of the current recycling of waste batteries uses sulfuric acid as a leaching agent, and the neutralized water after neutralization with lime is returned to the system for reuse, the carbon slag produced by the recycling of waste lithium-ion batteries will inevitably contain complex components such as calcium sulfate, nickel and cobalt metal oxides, natural graphite, artificial graphite, carbonaceous conductive agents, and hard carbon formed by carbonization of diaphragms, and even silicon dioxide dust. In addition, during the battery disassembly process, positive aluminum foil will inevitably remain in the negative electrode powder, resulting in a complex purification process and high purification cost; in addition, the key performance of the recycled graphite products, such as capacity, first effect and cycle, is difficult to achieve the product performance required by high-end graphite. Therefore, for enterprises, the recycling process is long and the recycling cost is high, but the recycling efficiency is not ideal, which will inevitably lead to a sluggish waste graphite recycling market and affect the efficient recycling of graphite resources. To this end, it is necessary to propose a new process to prepare high-end graphite negative electrodes with excellent performance. Summary of the invention

[0004] In view of the problem that the recycling performance of waste graphite materials from waste batteries is not ideal and it is difficult to adapt to the requirements of high rate and long-range cycle, the present invention provides a method for preparing waste graphite-based regenerated negative electrode active materials, aiming to regenerate regenerated graphite negative electrode active materials with excellent high rate and long-range cycle performance.

[0005] The second object of the present invention is to provide a regenerated negative electrode active material prepared by the preparation method and its application as a negative electrode active material in preparing a battery.

[0006] The third object of the present invention is to provide a battery and its negative electrode and negative electrode material.

[0007] The graphite material obtained from the stripping of waste batteries has many impurities and defects caused by recycling, and it is difficult to regenerate materials that meet the requirements of fast charging and long circulation. In view of this problem, the present invention has been studied in depth and adopted the following solutions:

[0008] A method for preparing a waste graphite-based regenerated negative electrode active material, comprising the following steps:

[0009] Step 1:

[0010] Pre-oxidizing the waste graphite material stripped from waste batteries in an oxidizing atmosphere to obtain a pre-oxidized material;

[0011] Step 2:

[0012] The pre-oxidized material is placed in reagent A and subjected to a first stage of treatment with mechanical assistance to obtain a first stage of treated material;

[0013] The first-stage treated material and reagent B are then mixed and sealed in a sealed container for the second-stage treatment, followed by solid-liquid separation, washing and drying to obtain a two-stage treated material;

[0014] Wherein, the reagent A is an aqueous solution containing at least one solute selected from hydroxide, carbonate and bicarbonate of an alkali metal element; the reagent B contains a compound of formula 1;

[0015]

[0016] In Formula 1, R is a halogen, a C1-C6 alkyl group, a substituted alkyl group or an alkylamino group;

[0017] The first-stage processed material or the second-stage processed material comprises large particles and small particles after screening, wherein the D50 of the large particles is 8 to 12 μm; the D50 of the small particles is 2 to 5 μm;

[0018] Step 3:

[0019] The second-stage treated material is mixed with a carbon source and a transition metal catalyst, carbonized after molding, and then subjected to carbon coating treatment to obtain the regenerated graphite negative electrode active material.

[0020] The present invention innovatively pre-oxidizes the waste graphite, mechanically assists the treatment with reagent A, and combines the treatment with reagent B, and then cooperates with the subsequent two-stage carbon coating treatment, so that synergy can be achieved, and harmful impurities in the graphite can be removed with high selectivity. In addition, its surface structure, active sites and stability can also be optimized. The regenerated graphite negative electrode material prepared by the preparation method of the present invention can take into account excellent electrochemical properties, especially can improve its fast charging and long-range cycle stability.

[0021] In the present invention, the waste battery is a waste battery with graphite as the negative electrode active material; considering the market processing value, it can be a widely used waste lithium ion battery or waste sodium ion battery.

[0022] In the present invention, the waste graphite material is a negative electrode material obtained by stripping the negative electrode of a waste battery, which contains more than 50wt.% of graphite, and at least one of a conductive agent, a binder, a current collector, and an electrolyte is allowed to exist. Considering the value of the treatment process, the content of graphite in the waste graphite material can be more than 80wt.%.

[0023] In the present invention, the waste graphite material can be obtained by stripping based on conventional means.

[0024] In the present invention, the waste graphite material is placed in an oxidizing atmosphere and heated to perform gas phase pre-oxidation treatment.

[0025] In the present invention, the oxidizing atmosphere is an atmosphere containing at least one oxidizing gas selected from oxygen and ozone; further, it may be at least one of air, a mixture of oxygen and diluent gas, and a mixture of ozone and diluent gas.

[0026] In the present invention, the diluent gas includes at least one of nitrogen and inert gas.

[0027] In the present invention, the temperature of the preliminary oxidation treatment is 300 to 600°C, and further can be 330 to 420°C.

[0028] In the present invention, the pre-oxidation treatment time is 2 to 4 hours.

[0029] Preferably, the pre-oxidation process is carried out under UV light irradiation. The present invention shows that pre-oxidation treatment under UV irradiation can further optimize the physical and chemical structure of waste graphite materials, which can help strengthen the subsequent combined treatment effect of reagent A and reagent B, and can further improve the fast charging and long-range cycle performance of recycled graphite materials.

[0030] In the present invention, the alkali metal element in the solute of the reagent A is at least one of lithium, sodium and potassium. The solute can specifically be a hydroxide, carbonate, bicarbonate or other component of the alkali metal element.

[0031] Preferably, the solute is at least one of lithium hydroxide, lithium carbonate, and lithium bicarbonate, preferably two or more. The present invention shows that the use of a preferred combination of lithium compounds as a solute, further combined with mechanical strengthening of the first stage treatment and the subsequent second stage treatment, can further optimize the physical and chemical structure of waste graphite, and can further enhance the fast charging and long-range cycle performance of the recycled material.

[0032] In the present invention, the concentration of the solute in reagent A is 1 to 5 M, and can further be 2 to 3 M;

[0033] In the present invention, the liquid-to-solid ratio of reagent A and pre-oxidation material is 2-5 ml / g;

[0034] In the present invention, the rotation speed of the mechanical auxiliary treatment stage is 400-800 rpm;

[0035] In the present invention, the first treatment period is 8 to 24 hours.

[0036] In the present invention, the first stage treatment material is pre-dispersed in water, and then the component of formula 1 is added to carry out the second stage treatment. The second stage treatment involving formula 1 of the present invention can help optimize the impurities on the graphite surface and between layers, and modify the solidification, so as to strengthen the physical and chemical structure of the surface and between layers, and further enhance the fast charging and long circulation effect of the recycled material.

[0037] In the present invention, in Formula 1, in R, the halogen is, for example, Cl. The alkyl is, for example, a straight chain or branched chain alkyl. The substituted alkyl is, for example, a hydroxyl group, an alkoxy group, or a methylene group substituted with a halogen, for example, a trifluoromethyl group.

[0038] Furthermore, the formula 1 is a composition of formula a and formula b, wherein formula a is a compound of formula 1 in which R is a halogen, especially Cl. The formula b is a compound of formula 1 in which R is a substituted alkyl, especially a halogen substituted methylene. In the composition, the molar ratio of formula a to formula b is, for example, 1:0.5 to 2. Studies have shown that the combination can further achieve synergistic modification and help to further enhance the treatment effect.

[0039] Preferably, in reagent B, the weight ratio of the first stage treated material to formula 1 is 200 to 90:1, and can further be 100 to 150:1.

[0040] Preferably, the temperature of the second treatment stage is 20-150°C, and further can be 25-50°C.

[0041] Preferably, the second stage of treatment is carried out under positive pressure; the positive pressure is preferably 0.5-2 MPa.

[0042] Preferably, the second treatment period is 4 to 12 hours, and may further be 5 to 10 hours.

[0043] In the present invention, the first-stage processed material can be screened to obtain large particles and small particles, and then the second-stage processed material can be processed to obtain the graded second-stage processed material. Alternatively, the first-stage processed material is not screened, but directly processed to obtain the graded second-stage processed material after the second-stage processed material is screened.

[0044] Preferably, the weight ratio of large particles to small particles in the first-stage processed material or the second-stage processed material is 100:20-50; further, it can be 100:35-45.

[0045] In the present invention, the carbon source may be an organic substance known in the industry that can form carbon, such as a resin, and more preferably one or more of polypropylene, polyvinyl chloride, polystyrene, and polyoxymethylene;

[0046] Preferably, the transition metal catalyst comprises a compound of at least one transition metal element selected from nickel, cobalt and manganese; preferably a nickel-containing compound;

[0047] Preferably, the weight ratio of the second-stage treated material to the carbon source and the transition metal catalyst is 100:8-15:0.5-2, and further 100:10-12:1-1.5.

[0048] The molding method may be compression molding.

[0049] Preferably, the carbonization temperature is 900-1350°C, and may further be 1100-1250°C.

[0050] Preferably, the carbonization stage is carried out under negative pressure, and the pressure of the negative pressure may be, for example, below 100 Pa.

[0051] Preferably, the carbonization time is 4 to 12 hours, and further can be 8 to 10 hours.

[0052] Preferably, the product of the carbonization treatment is combined with the second carbon source and then added for carbon coating treatment.

[0053] In the present invention, the second carbon source may be an organic matter known in the industry, for example, at least one of a solid carbon source, a liquid carbon source, and a gaseous carbon source. The solid carbon source is an organic matter in a solid state. The liquid carbon source is, for example, an organic matter that is liquid at the temperature, or a solution of an organic matter, for example, asphalt. The gaseous carbon source is an organic matter that is in another state during the heat treatment stage, for example, it may be a component such as C1 to C4 alkanes, olefins, etc.

[0054] Preferably, the temperature in the carbon coating treatment stage is 1050-1250° C., and the insulation time at this temperature is 4-8 hours.

[0055] The invention also provides a waste graphite-based regenerated negative electrode active material prepared by the preparation method.

[0056] The method described in the present invention can give the obtained product special physical and chemical characteristics, and the recycled material obtained by the method can unexpectedly show excellent performance, especially can show excellent fast charging and long-range cycle effects.

[0057] The present invention also provides the use of the waste graphite-based regenerated negative electrode active material prepared by the preparation method, which is used as the negative electrode active material to prepare an alkali metal ion battery.

[0058] In the present invention, the regenerated negative electrode active material can be used as a negative electrode active material to prepare the required alkali metal ion battery and its components based on existing conventional means and methods.

[0059] In the present invention, the alkali metal ion battery is a lithium ion battery or a sodium ion battery.

[0060] The present invention also provides a negative electrode of an alkali metal battery, which comprises the waste graphite-based regenerated negative electrode active material prepared by the preparation method.

[0061] The present invention also provides an alkali metal battery, which comprises the negative electrode of the present invention.

[0062] The alkali metal battery and the negative electrode thereof described in the present invention, in addition to comprising the waste graphite-based regenerated negative electrode active material described in the present invention, other components and structural parts can be conventional.

[0063] Beneficial Effects

[0064] The present invention innovatively pre-oxidizes the waste graphite, mechanically assists the treatment with reagent A, and combines the treatment with reagent B, and then cooperates with the subsequent two-stage carbon coating treatment, so that synergy can be achieved, and harmful impurities in the graphite can be removed with high selectivity. In addition, its surface structure, active sites and stability can also be optimized. The regenerated graphite negative electrode material prepared by the preparation method of the present invention can take into account excellent electrochemical properties, especially can improve its fast charging and long-range cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 This is the SEM image of the waste graphite of Example 1;

[0066] Figure 2 This is a SEM image of the regenerated graphite material after treatment in Example 1;

[0067] Figure 3 The lithium half-cell cycle performance diagram (0.2C) of the product obtained in Example 1;

[0068] Figure 4 The graph is a lithium half-cell cycle performance diagram of the product obtained in Example 1 (first cycled 5 times at 0.2C, then cycled to 1000 times at 1C). DETAILED DESCRIPTION

[0069] The waste graphite of the present invention can be obtained by stripping waste graphite electrodes of waste batteries. The stripping method can be conventional, for example, solvent stripping method, thermal stripping method, etc.

[0070] In the present invention, the waste graphite material obtained by stripping, in addition to mainly containing graphite, is also allowed to contain a small amount of components such as conductive agent, binder, diaphragm, electrolyte, etc. Considering the recycling value of the technical solution, the content of graphite therein can be more than 50wt%. The following cases, as typical embodiments that can be cited, can have a content between 80 and 90wt%.

[0071] The present invention provides an optional method for preparing a waste graphite-based regenerated negative electrode active material, comprising the following steps:

[0072] Step 1: Pre-treat the waste graphite carbon slag in an oxidizing atmosphere;

[0073] Step 2: placing the obtained carbon oxide slag in an aqueous solution of reagent A, performing wet ball milling, then washing the slurry, filtering, drying the filter cake, and breaking it up to obtain a first-stage processed material, which may be large particles and small particles that have been sieved and graded;

[0074] Step 3: adding the first-stage treated material to the reagent B solution containing Formula 1, stirring and reacting under closed conditions, then washing the pulp, filtering, drying the filter cake, and breaking it up to obtain the second-stage treated material;

[0075] It should be noted that the second step can also be performed without screening, and the third step can be performed directly. After the third step is completed, the large particles and small particles of the graded distribution are screened to obtain the second-stage processed material;

[0076] The median particle size D50 of the small particles and the large particles is 3-5 μm and 8-12 μm respectively. The mixing ratio of the small particles to the large particles is 20-50:100;

[0077] Step 4: Mix the second-stage processed material powder according to a certain ratio, add a certain amount of resin and nickel salt, heat and mix in a kneader, press and form, and then vacuum carbonize, break up and sieve;

[0078] Step 5: Carbon-coating the obtained powder, breaking it up, demagnetizing it, and sieving it to obtain the graphite negative electrode powder.

[0079] In the optional step 1 of the present invention, the oxidizing atmosphere refers to a gas containing one or two of air, oxygen, and ozone, and the remaining gas is one or more of nitrogen, argon, and helium; wherein the volume fraction of air is 50-100%, the volume fraction of oxygen is 10-50%, and the volume fraction of ozone is 0.5-10%.

[0080] The treatment temperature in step 1 is 300-600° C., and the insulation time is 2-4 hours.

[0081] In the optional step 2 of the present invention, the reagent A is one or more of the hydroxide, carbonate or bicarbonate of lithium, sodium or potassium, preferably a mixture of sodium hydroxide and sodium carbonate. The concentration of the aqueous solution of A is 2 to 5M; the liquid-solid ratio of the aqueous solution of A to the oxidized carbon slag is 2 to 5 ml / g; the ball milling speed is 400 to 800 rpm, and the ball milling time is 8 to 24 hours;

[0082] In step 4, the resin refers to one or more of polypropylene, polyvinyl chloride, polystyrene, and polyoxymethylene; the ratio of the resin to the carbon powder (second-stage material) is 8 to 15:100; the nickel salt is one or more of nickel oxalate, nickel hydroxide, nickel acetylacetonate, nickel acetate, nickel phthalocyanine, nickel carbonate, and basic nickel carbonate, and the ratio of the nickel salt to the carbon powder is 0.5 to 2:100; the vacuum carbonization is to place the molding material in a vacuum furnace, introduce one or more of nitrogen, argon, and helium for gas exchange, then program the temperature to 900 to 1350° C., and evacuate it, maintain the system at 20 to 200 Pa, and after insulation treatment for 4 to 12 hours, naturally cool it to room temperature.

[0083] The carbon coating process described in step 5 refers to adding asphalt and then mixing, the ratio of asphalt to carbon material is 5 to 8:100, and after mixing evenly, heat treatment is performed to 1050 to 1250° C. under protective atmosphere conditions and kept warm for 4 to 8 hours.

[0084] The following is a specific implementation plan:

[0085] Example 1

[0086] Step 1: Place the waste graphite carbon slag in an oxidizing atmosphere (air) and keep it at 400°C for 2 hours;

[0087] Step 2: The carbon oxidized slag obtained in step 1 is placed in an aqueous solution of reagent A (1M sodium carbonate, 1M sodium hydroxide solution, liquid-to-solid ratio of 3 ml / g), and wet ball milled at a ball milling speed of 600±50 rpm for 12 h, followed by slurry washing, filtration, filter cake drying, and breaking up to obtain a ball milled material;

[0088] The ball mill material is sieved to obtain particles A with a D50 of 4.1 μm and particles B with a D50 of 10.3 μm; and particles A and particles B are graded at a weight ratio of 30:100 to obtain a first-stage processed material;

[0089] Step 3: Slurry a section of treated material with water at a liquid-to-solid ratio of 5 ml / g and place it in a sealed container, then add Formula 1 (Formula 1-A in this case, The weight ratio of the first-stage treated material to the first-stage treated material is 1:150), and then the container is sealed and stirred at a speed of 100-150rpm and a temperature of 40±5℃ for 6h, and then the pulp is washed, filtered, the filter cake is dried and broken up to obtain the second-stage treated material;

[0090] Step 4: The second-stage treated material, resin (polypropylene in this case), and catalyst (nickel acetate in this case) are heated and mixed in a kneader at a weight ratio of 100:10:1, and then pressed into shape, and then vacuum carbonized for 10 hours at a vacuum pressure of less than 100 Pa and a temperature of 1150±10°C to obtain a carbonized material;

[0091] Step 5: The carbonized material in step 4 and asphalt are mixed in a weight ratio of 100:6 and carbon-coated at a temperature of 1100±10°C for 6 hours, followed by breaking up, demagnetizing and sieving to obtain regenerated graphite negative electrode active material.

[0092] Electrochemical performance test method:

[0093] A certain amount of regenerated graphite negative electrode active material, binder (LA-133, CMC) and conductive carbon black (SP) were uniformly mixed in a mass ratio of 92:3:3:2, and then anhydrous ethanol and deionized water (volume ratio of 1:3) were added to make a uniform slurry, which was coated on copper foil and placed in a vacuum dryer at 120 °C for 12 h to obtain a graphite negative electrode with a loading of 8-12 mg / cm 2 of electrode sheets.

[0094] A CR2025 button battery case was used, the obtained graphite negative electrode sheet was used as the working electrode, the metal lithium sheet was used as the counter electrode, a Celgard 2400 type diaphragm was used, nickel foam was used as the counter electrode side current collector, and a solution of ethylene carbonate + dimethyl carbonate + diethyl carbonate (EC+DMC+DEC, volume ratio of 1:1:1) containing 1M LiPF6 was used as the electrolyte. The cells were assembled in a glove box under an argon atmosphere, and then compressed and packaged using a sealing machine to obtain a button lithium battery.

[0095] The battery cycle performance was tested at room temperature with a test voltage range of 0.01V to 1.5V and test rates of 0.2C, 1C, and 10C.

[0096] Example 2

[0097] Compared with Example 1, the only difference is that the conditions of step 1 are changed. The experimental group is:

[0098] Group A: The heat preservation pretreatment stage was carried out under 254nm UV light irradiation.

[0099] Group B: The oxidizing atmosphere was oxygen, the temperature of the pretreatment stage was 350°C, and the insulation treatment time was 3h;

[0100] Other operations, parameters and tests are the same as those in Example 1.

[0101] Example 3

[0102] Compared with Example 1, the only difference is that the conditions of step 2 are changed. The experimental group is:

[0103] Group A: In reagent A, an equal mole of lithium carbonate was used to replace sodium carbonate, and an equal mole of lithium hydroxide was used to replace sodium hydroxide. Other operations and parameters were the same as those in Example 1.

[0104] Group B: In reagent A, the concentration of sodium carbonate is 0.5M, the concentration of sodium hydroxide is 2M, the ball milling speed is 700±50rpm, the ball milling time is 14h, and after ball milling, particles A with a D50 of 3.6μm and particles B with a D50 of 9.6μm are obtained by sieving; and particles A and particles B are graded at a weight ratio of 40:100 to obtain a first-stage treated material;

[0105] Other operations, parameters and tests are the same as those in Example 1.

[0106] Example 4

[0107] Compared with Example 1, the only difference is that the conditions in step 3 are changed. The experimental groups are:

[0108] Group A: Formula 1 is Formula 1-B, and its structure is

[0109] Group B: Formula 1 is a mixture of Formula 1-A and Formula 1-B in a molar ratio of 1:1;

[0110] Group C: Based on Group B, pressure treatment was performed during the treatment phase, and the pressure was 1MPa;

[0111] Group D: The first-stage treated material was slurried with water at a liquid-to-solid ratio of 4 ml / g and placed in a sealed container, followed by the addition of Formula 1 (the weight ratio of Formula 1 to the first-stage treated material was 1:100), followed by the sealed container and stirring at a speed of 100-150 rpm and a temperature of 35±5°C for 8 hours, followed by slurry washing, filtration, filter cake drying, and dispersion to obtain second-stage treated materials;

[0112] Other operations and parameters are the same as in Example 1.

[0113] Example 5

[0114] Compared with Example 1, the only difference is that the ball mill material in step 2 is pre-treated with reagent B in step 3, and then washed, filtered, dried, and broken up, and then sieved and graded to obtain a second-stage processed material with a weight ratio of 30:100, which is a graded particle A with a D50 of 4.0 μm and a particle B with a D50 of 10.4 μm; and then it is subjected to subsequent treatment.

[0115] Other operations and parameters are the same as in Example 1.

[0116] Example 6

[0117] Compared with Example 1, the only difference is that the conditions of step 4 and step 5 are changed, specifically, in step 4: the second-stage treated material, the resin (polystyrene in this case), and the catalyst (nickel oxalate in this case) are heated and mixed in a kneader at a weight ratio of 100:12:1.5, and pressed into shape, and then vacuum carbonized for 8 hours at a pressure of less than 100 Pa and a temperature of 1200±10°C to obtain a carbonized material;

[0118] Step 5: The carbonized material in step 4 and asphalt are mixed in a weight ratio of 100:5 and kept at a temperature of 1200±10°C for 4 hours for carbon coating, followed by breaking up, demagnetizing and sieving to obtain regenerated graphite negative electrode active material.

[0119] Other operations, parameters and tests are the same as those in Example 1.

[0120] Comparative Example 1

[0121] Compared with Example 1, the only difference is that the waste graphite is not processed in step 1, but is directly used as a raw material in step 2 and subsequent processing. Other operations, parameters and tests are the same as in Example 1.

[0122] Comparative Example 2

[0123] Compared with Example 1, the only difference is that in step 2, reagent A is replaced by water, and the solute is not added. Other operations and parameters are the same as in Example 1.

[0124] Comparative Example 3

[0125] Compared with Example 1, the only difference is that in step 2, no classification and grading treatment is performed, and the ball mill is directly used as a raw material for step 3 and subsequent treatments. Other operations and parameters are the same as in Example 1.

[0126] Comparative Example 4

[0127] Compared with Example 1, the only difference is that in step 3, Formula 1 is not added, and other operations and parameters are the same as those in Example 1.

[0128] Comparative Example 5

[0129] Compared with Example 1, the only difference is that in step 3, hydrochloric acid is used to replace the formula 1 (the molar amount of Cl is the same), and the other operations and parameters are the same as in Example 1.

[0130] Comparative Example 6

[0131] Compared with Example 1, the only difference is that in step 3, an equimolar amount of Replace the formula 1, and other operations and parameters are the same as those in Example 1.

[0132] Comparative Example 7

[0133] Compared with Example 1, the only difference is that the product of step 1 is directly processed in step 3, then the product of step 3 is processed in step 2, and then the product of step 2 is processed in step 4 and subsequent steps.

[0134] Other operations and parameters are the same as in Example 1.

[0135] The electrochemical performance test results of each case are shown in Table 1 and Table 2

[0136] Table 1

[0137]

[0138]

[0139] Table 2

[0140]

[0141] It can be seen from the examples and comparative examples that the process described in the present invention can significantly optimize the physical and chemical structure of the recycled material and improve its fast charging and long cycle effects.

Claims

1. A method for preparing waste graphite-based regenerated negative electrode active materials, characterized in that the steps include: Step 1: Pre-oxidizing the waste graphite material stripped from waste batteries in an oxidizing atmosphere to obtain a pre-oxidized material; Step 2: The pre-oxidized material is placed in reagent A and subjected to a first stage of treatment with mechanical assistance to obtain a first stage of treated material; The first-stage treated material and reagent B are then mixed and sealed in a sealed container for the second-stage treatment, followed by solid-liquid separation, washing and drying to obtain a two-stage treated material; Wherein, the reagent A is an aqueous solution containing at least one solute selected from hydroxide, carbonate and bicarbonate of an alkali metal element; the reagent B contains a compound of formula 1; In Formula 1, R is a halogen, a C1-C6 alkyl group, a substituted alkyl group or an alkylamino group; The first-stage processed material or the second-stage processed material comprises large particles and small particles after screening, wherein the D50 of the large particles is 8 to 12 μm; the D50 of the small particles is 2 to 5 μm; Step 3: The second-stage treated material is mixed with a carbon source and a transition metal catalyst, carbonized after molding, and then subjected to carbon coating treatment to obtain the regenerated graphite negative electrode active material.

2. The method for preparing the waste graphite-based regenerated negative electrode active material according to claim 1, characterized in that: The waste batteries are waste batteries with graphite as the negative electrode active material; preferably waste lithium ion batteries or waste sodium ion batteries; Preferably, the waste graphite material is a negative electrode material obtained by stripping the negative electrode of a waste battery, which contains more than 50wt.% of graphite, and at least one of a conductive agent, a binder, a current collector, and an electrolyte is allowed to exist.

3. The method for preparing the waste graphite-based regenerated negative electrode active material according to claim 1, characterized in that: The oxidizing atmosphere is an atmosphere containing at least one oxidizing gas selected from oxygen and ozone; further, it may be at least one of air, a mixture of oxygen and diluent gas, and a mixture of ozone and diluent gas; Preferably, the diluent gas includes at least one of nitrogen and an inert gas; Preferably, the temperature of the pre-oxidation treatment is 300-600°C; Preferably, the pre-oxidation treatment time is 2 to 4 hours; Preferably, the pre-oxidation process is carried out under UV light irradiation.

4. The method for preparing the waste graphite-based regenerated negative electrode active material according to claim 1, characterized in that: The alkali metal element in the solute of the reagent A is at least one of lithium, sodium and potassium; Preferably, the solute is at least one of lithium hydroxide, lithium carbonate and lithium bicarbonate, preferably two or more; Preferably, the concentration of the solute in reagent A is 1 to 5 M; Preferably, the liquid-to-solid ratio of reagent A and pre-oxidation material is 2-5 ml / g; Preferably, the rotation speed of the mechanically assisted treatment stage is 400-800 rpm; Preferably, the first treatment period is 8 to 24 hours.

5. The method for preparing the waste graphite-based regenerated negative electrode active material according to claim 1, characterized in that: The first stage treatment material is pre-dispersed in water, and then the component of formula 1 is added to carry out the second stage treatment; Preferably, in Formula 1, R is Cl, trifluoromethyl, dialkylamino or tert-butyl; Preferably, in reagent B, the weight ratio of the first stage treated material to formula 1 is 200 to 90:1; Preferably, the temperature of the second treatment stage is 20 to 150°C; Preferably, the second stage of treatment is carried out under positive pressure; the positive pressure is preferably 0.5-2 MPa; Preferably, the second treatment period is 4 to 12 hours; Preferably, the first-stage processed material is screened to obtain large particles and small particles, and then the second-stage processed material is processed; or, the first-stage processed material is not screened, and directly processed to the second-stage processed material, and then screened to obtain the second-stage processed material; Preferably, the weight ratio of large particles to small particles in the first-stage processed material or the second-stage processed material is 100:20-50; further, it can be 100:35-45.

6. The method for preparing the waste graphite-based regenerated negative electrode active material according to claim 1, characterized in that: The carbon source is a resin, more preferably one or more of polypropylene, polyvinyl chloride, polystyrene and polyoxymethylene; Preferably, the transition metal catalyst comprises a compound of at least one transition metal element selected from nickel, cobalt and manganese; preferably a nickel-containing compound; Preferably, the weight ratio of the second-stage treated material to the carbon source and the transition metal catalyst is 100:8-15:0.5-2; Preferably, the molding method is compression molding; Preferably, the carbonization temperature is 900-1350°C; Preferably, the carbonization stage is carried out under negative pressure; Preferably, the carbonization time is 4 to 12 hours; Preferably, the product of the carbonization treatment and the second carbon source are combined and then added to perform carbon coating treatment; Preferably, the second carbon source is at least one of a solid carbon source, a liquid carbon source, and a gaseous carbon source; Preferably, the temperature in the carbon coating treatment stage is 1050-1250° C., and the insulation time at this temperature is 4-8 hours.

7. A waste graphite-based regenerated negative electrode active material obtained by the preparation method according to any one of claims 1 to 6.

8. An application of the waste graphite-based regenerated negative electrode active material obtained by the preparation method according to any one of claims 1 to 6, characterized in that: It is used as negative electrode active material to prepare alkali metal ion batteries; Preferably, the alkali metal ion battery is a lithium ion battery or a sodium ion battery.

9. A negative electrode of an alkali metal battery, characterized in that: The invention relates to a waste graphite-based regenerated negative electrode active material prepared by the preparation method according to any one of claims 1 to 6.

10. An alkali metal battery, characterized in that: The negative electrode according to claim 9 is included.

Citation Information

Patent Citations

  • Method for pretreating waste graphite material and preparing long-circulation graphite active material

    CN116281999A

  • Regenerated graphite negative electrode active material as well as preparation and application thereof

    CN117125708A

  • Failure graphite-based regenerated graphite material for waste batteries and preparation method and application of failure graphite-based regenerated graphite material

    CN118183729A

  • Carbon-coated graphite material taking waste batteries as raw materials and preparation method of carbon-coated graphite material

    CN118486939A

  • Negative electrode material, preparation method therefor and application thereof, and negative electrode plate and application

    US20240262692A1

Cited By

  • Negative electrode recovery method and negative electrode graphite powder

    CN121085262A

  • Repair and regeneration method of retired graphite, regenerated graphite negative electrode material and lithium battery

    CN121553936A