Method for recovering aluminum oxide from waste MTO catalyst
By reacting and calcining the waste MTO catalyst with ammonium bisulfate and ammonium bicarbonate, high-purity alumina was successfully recovered, and a high-efficiency silicon calcium phospho-silica fertilizer was prepared through activation treatment, which solved the silicon component in the waste MTO catalyst. The problem of insufficient recycling has improved resource utilization and environmental security.
Patent Information
- Application Number
- CN202310592094.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, there are few reports on the recovery of silicon components of waste MTO catalysts, resulting in low resource utilization and the deactivated waste MTO catalysts are harmful to the environment.
By reacting the waste MTO catalyst with ammonium bisulfate and ammonium bicarbonate in a solvent, alkaline ammonium aluminum carbonate is produced, and high-purity alumina is obtained by calcining treatment, while the first filter residue is mixed with calcium hydroxide and ammonia water. By activation treatment, a high-effective silicon content of calcium phospho-silicon fertilizer was prepared.
It realizes efficient recycling of alumina from waste MTO catalysts, with simple process and strong operability, which improves the comprehensive utilization value of waste catalysts, reduces the harm to the environment, and prepares high-purity Al2O3 and high-efficiency silicon phosphorus Silicon calcium fertilizer.
Smart Images

Figure CN119018916A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a waste MTO catalyst, and in particular to a method for recovering aluminum oxide from the waste MTO catalyst. Background Art
[0002] Low-carbon olefins are the most important basic raw materials for petrochemicals. As oil resources are increasingly depleted, the synthesis of low-carbon olefins using coal and natural gas as raw materials has gradually become a hot topic. In recent years, with the maturity and promotion of the coal chemical process of methanol to low-carbon olefins (MTO for short), the demand for methanol to olefins catalysts (MTO catalysts for short) has expanded rapidly.
[0003] MTO catalyst is mainly made of SAPO molecular sieve carrier and binder, and its main component is γ-Al 2 O 3 , P 2 O 5 and SiO 2 During the MTO synthesis process, the MTO catalyst will be deactivated due to coking, collapse of the molecular sieve skeleton structure, etc. The deactivated waste MTO catalyst is a harmful substance and may cause harm to the environment if not treated. Since the waste MTO catalyst is rich in elements such as silicon, aluminum, and phosphorus, it can be recycled as a resource.
[0004] In addition, the existing waste MTO catalyst recovery mainly focuses on the recovery of high value-added components such as phosphorus and aluminum, while there are few reports on the recovery of silicon components. Summary of the invention
[0005] In order to overcome at least one of the defects of the prior art, an embodiment of the present invention provides a method for recovering alumina from a waste MTO catalyst, comprising the following steps:
[0006] Performing a first reaction between the waste MTO catalyst and the raw material in a solvent to obtain a first solid-liquid mixture;
[0007] Performing solid-liquid separation on the first solid-liquid mixture to obtain a first filtrate and a first filter residue;
[0008] The first filtrate is mixed with ammonia gas or a solution containing ammonia water, and then subjected to a second reaction, and a precipitate is precipitated to obtain a second solid-liquid mixture;
[0009] performing solid-liquid separation on the second solid-liquid mixture to obtain basic ammonium aluminum carbonate solid and a second filtrate; and
[0010] The basic ammonium aluminum carbonate solid is calcined to obtain aluminum oxide;
[0011] Wherein, the raw materials include ammonium bisulfate and ammonium bicarbonate; in the first reaction, the reaction temperature is 180-300° C. and the pressure is 1.5-4.0 MPa.
[0012] A method for recovering aluminum oxide from waste MTO catalyst according to an embodiment of the present invention can utilize waste MTO catalyst to recover aluminum oxide, has a simple process flow, and is highly operable. In addition, the method can recover high-purity aluminum oxide from waste MTO catalyst with a high yield. 2 O 3 . BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The accompanying drawings are only used to illustrate specific embodiments and are not to be considered as limiting the present invention.
[0014] Figure 1 The present invention is a process flow chart of a method for recovering alumina from spent MTO catalyst according to an embodiment of the present invention. DETAILED DESCRIPTION
[0015] Typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various changes in different embodiments without departing from the scope of the present invention, and the descriptions therein are essentially used as illustrations rather than to limit the present invention.
[0016] See also Figure 1 As shown, one embodiment of the present invention provides a method for recovering aluminum oxide from a waste MTO catalyst, comprising the following steps:
[0017] Performing a first reaction between the waste MTO catalyst and the raw material in a solvent to obtain a first solid-liquid mixture;
[0018] Performing solid-liquid separation on the first solid-liquid mixture to obtain a first filtrate and a first filter residue;
[0019] The first filtrate is mixed with ammonia gas or a solution containing ammonia water, and then subjected to a second reaction, and a precipitate is precipitated to obtain a second solid-liquid mixture;
[0020] The second solid-liquid mixture is subjected to solid-liquid separation treatment to obtain basic ammonium aluminum carbonate (NH 4 Al(OH) 2 CO 3 ) a solid and a second filtrate; and
[0021] The solid ammonium aluminum carbonate is calcined to obtain aluminum oxide;
[0022] The raw materials include ammonium bisulfate and ammonium bicarbonate; in the first reaction, the reaction temperature is 180-300° C. and the pressure is 1.5-4.0 MPa.
[0023] In one embodiment, the waste MTO catalyst is a deactivated MTO catalyst; the waste MTO catalyst may include a SAPO series molecular sieve; further, the waste MTO catalyst includes alumina (Al 2 O 3 ), silicon dioxide (SiO 2 ) and phosphorus pentoxide (P 2 O 5 ); in the waste MTO catalyst, the mass content of aluminum oxide can be 46-50%, such as 47%, 48%, 49%; the mass content of silicon dioxide can be 19-21%, such as 20%; the mass content of phosphorus pentoxide can be 29-31%, such as 30%, and the rest are impurities.
[0024] In one embodiment, the step of obtaining a first solid-liquid mixture comprises:
[0025] providing a raw material solution, the raw material solution comprising a raw material and a solvent; and
[0026] The waste MTO catalyst is mixed with the raw material solution to react and obtain a first solid-liquid mixture.
[0027] In one embodiment, after the spent MTO catalyst is mixed with the feed solution, the alumina therein reacts with ammonium bisulfate to generate ammonium aluminum sulfate.
[0028] In one embodiment, in the raw material solution, the molar concentration of ammonium bisulfate can be 2 to 10 mol / L, for example, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L; the molar concentration of ammonium bicarbonate can be 2 to 8 mol / L, for example, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L.
[0029] In one embodiment, the solvent in the raw material solution may be water. Furthermore, the raw material solution is a mixed aqueous solution of ammonium bisulfate and ammonium bicarbonate.
[0030] In one embodiment, in the raw material solution, the molar ratio of ammonium bisulfate to ammonium bicarbonate can be 1:2 to 4:1, and can further be 1:1 to 2:1, for example, 0.8:1, 1.2:1, 1.5:1, 1.8:1, 2.5:1, 3:1, 3.5:1.
[0031] In one embodiment, the mass ratio (solid-liquid ratio) of the waste MTO catalyst to the raw material solution can be 1:3 to 1:10, and can further be 1:4 to 1:10, for example, 1:4.5, 1:5, 1:5.5, 1:6, 1:7, 1:8, 1:9.
[0032] In one embodiment, the first reaction is a dissolution reaction, and the reaction temperature of the first reaction can be 180-300°C, further 240-280°C, for example 200°C, 220°C, 250°C, 260°C, 280°C; the reaction time of the first reaction can be 0.5-2 hours, for example 1 hour, 1.5 hours.
[0033] In one embodiment, in the first reaction, the pressure of the reaction system is 1.5-4.0 MPa, further 1.5-2.5 MPa, such as 1.8 MPa, 1.9 MPa, 2.0 MPa, 2.1 MPa, 2.2 MPa, 2.5 MPa, 2.8 MPa, 3 MPa, 3.2 MPa, 3.5 MPa, 3.8 MPa. The first reaction is carried out under high pressure conditions to achieve pressure balance in the system, so that no carbon dioxide product is formed.
[0034] In one embodiment, the solid-liquid separation process may be a filtration process.
[0035] In one embodiment, the first filtrate contains cations and anions, the cations include one, two or three of ammonium ions, hydrogen ions and aluminum ions; the anions include sulfate ions and / or bicarbonate ions; further, the first filtrate includes ammonium aluminum sulfate and one or two of ammonium bisulfate and ammonium bicarbonate.
[0036] In one embodiment, the first filter residue comprises amorphous SiO 2 and P 2 O 5 .
[0037] In one embodiment, ammonia gas or aqueous ammonia may be introduced into the first filtrate to carry out the second reaction.
[0038] In one embodiment, in the step of obtaining the second solid-liquid mixture, the temperature of the system is 65-95°C, for example, 70°C, 75°C, 80°C, 85°C, 90°C; the pH value of the system is 8-12, for example, 9, 10, 11.
[0039] In one embodiment, the second solid-liquid mixture is subjected to a solid-liquid separation treatment (such as a filtration treatment) to obtain a basic ammonium aluminum carbonate precipitate and a second filtrate; the second filtrate includes ammonium bisulfate, and further, the second filtrate is an ammonium bisulfate solution.
[0040] In one embodiment, the second filtrate ammonium bisulfate solution can be used as one of the raw materials for subsequent recovery of aluminum oxide to achieve resource recycling and save costs.
[0041] In one embodiment, the solid ammonium aluminum carbonate is calcined to produce aluminum oxide, ammonia, carbon dioxide and water.
[0042] In one embodiment, the calcination temperature may be 300-500°C, such as 320°C, 350°C, 360°C, 380°C, 400°C, 420°C, 450°C, 480°C; the calcination time may be 30-90 min, such as 45 min, 60 min, 75 min. The basic ammonium aluminum carbonate is calcined at the above temperature to obtain alumina of γ-Al 2 O 3 .
[0043] In one embodiment, the CO generated by the roasting process is 2 NH 3 It can be recycled as a raw material for the preparation of ammonium bicarbonate, for example, CO 2 NH 3 The second filtrate is introduced into the ammonium bisulfate solution, and the obtained mixed solution is then added into the raw material solution for recycling.
[0044] In one embodiment, the first filter residue is further mixed with calcium hydroxide and ammonia water and then activated to obtain a phosphate-silicon-calcium mixed fertilizer. Further, the activated material can be dried, granulated, etc. to obtain a phosphate-silicon-calcium mixed fertilizer product.
[0045] In one embodiment, the first filter residue is mixed with calcium hydroxide and ammonia water and then activated; the first filter residue may include amorphous SiO 2 and P 2 O 5 ; Further, the SiO in the first filter residue 2 With Ca(OH) 2 The molar ratio of P in the first filter residue can be (0.5-1.5):1, such as 0.8:1, 1.0:1, 1.2:1; 2 O 5 With NH 4 The molar ratio of OH can be 1:(2-4), for example 1:2.5, 1:3, 1:3.5.
[0046] In one embodiment, the activation treatment includes keeping the first filter residue, calcium hydroxide and ammonia water mixture warm at an activation temperature; the activation temperature can be 70-95°C, for example, 75°C, 80°C, 85°C, 90°C; the activation time (or insulation time) can be 0.5-5 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours.
[0047] In one embodiment, the phosphate-silicon-calcium mixed fertilizer includes active calcium silicate, diammonium phosphate and ammonium hydrogen phosphate.
[0048] The method for recovering aluminum oxide from waste MTO catalyst according to one embodiment of the present invention can utilize waste MTO catalyst to recover aluminum oxide, and the process flow is simple and the operability is strong. The method can prepare aluminum oxide in waste MTO catalyst into high-purity aluminum oxide. 2 O 3 At the same time, it can also prepare phosphatic silicon calcium fertilizer with an effective silicon content higher than 20%, realize the effective recycling of waste MTO catalysts, reduce the harm of waste catalysts to the environment, and improve the comprehensive utilization value of waste catalysts.
[0049] Hereinafter, a method for recovering aluminum oxide from waste MTO catalyst according to an embodiment of the present invention will be further described in conjunction with the accompanying drawings and specific examples. Wherein, unless otherwise specified, the raw materials used are all commercially available.
[0050] Example 1
[0051] S1: Take 100g of waste MTO catalyst (including SiO 2 The content is 20.31wt%, Al 2 O 3 The content is 47.51wt%, P 2 O 5 The waste MTO catalyst is 29.16wt% and the rest are impurities) and mixed with a raw material solution, the raw material solution is a mixed aqueous solution of ammonium bisulfate and ammonium bicarbonate; wherein the molar concentration of ammonium bisulfate is 8mol / L, the molar concentration of ammonium bicarbonate is 2mol / L, the molar ratio of ammonium bisulfate to ammonium bicarbonate is 4:1, and the solid-liquid ratio of the waste MTO catalyst to the raw material solution is 1:3; the mixed system is heated to 180°C, and a dissolution reaction is carried out. The reaction time is 0.5h and the pressure of the system is 2MPa to obtain a first solid-liquid mixture;
[0052] S2: After the reaction of step S1 is completed, the obtained first solid-liquid mixture is subjected to solid-liquid separation to obtain a first filtrate (a mixed solution of ammonium aluminum sulfate, ammonium bisulfate and ammonium bicarbonate) and a first filter residue;
[0053] S3: Add NH to the first filtrate 3 , the temperature is 65° C., the pH value of the solution system is 8, and a precipitation reaction is performed to obtain a second solid-liquid mixture;
[0054] S4: performing solid-liquid separation on the second solid-liquid mixture to obtain basic ammonium aluminum carbonate solid and a second filtrate;
[0055] S5: calcining the basic ammonium aluminum carbonate solid at a temperature of 300° C. for 30 min to obtain an alumina product;
[0056] S6: Mix the first filter residue with calcium hydroxide and ammonia water and perform activation treatment at an activation temperature of 70°C for 0.5h; wherein SiO 2 With Ca(OH) 2 The molar ratio is 0.5:1, P 2 O 5 With NH 4 The molar ratio of OH is 1:2; after the activation treatment is completed, a phosphate-silicon-calcium mixed fertilizer is obtained.
[0057] Example 2
[0058] This embodiment uses the same materials and processes as those in Embodiment 1, except that the composition of the waste MTO catalyst used in step S1 (SiO 2 The content is 19.65wt%, Al 2 O 3 The content is 46.78wt%, P 2 O 5 The content is 29.32wt%, and the rest are impurities); and the molar concentration of ammonium bicarbonate in step S1 is different, which is 8mol / L.
[0059] Example 3
[0060] This embodiment uses substantially the same materials and processes as those of embodiment 2, with the only difference being that the reaction temperature of step S1 is 280°C.
[0061] Example 3-1
[0062] This embodiment uses substantially the same materials and processes as those of embodiment 3, with the only difference being that the reaction temperature of step S1 is 200°C.
[0063] Example 3-2
[0064] This embodiment uses substantially the same materials and processes as those of embodiment 3, with the only difference being that the reaction temperature of step S1 is 240°C.
[0065] Example 4
[0066] This embodiment uses substantially the same materials and processes as those of Embodiment 3, with the only difference being that the solid-to-liquid ratio of the waste MTO catalyst to the raw material solution in step S1 is 1:4.
[0067] Example 4-1
[0068] This embodiment uses substantially the same materials and processes as those of Embodiment 4, with the only difference being that the solid-to-liquid ratio of the waste MTO catalyst to the raw material solution in step S1 is 1:6.
[0069] Example 4-2
[0070] This embodiment uses substantially the same materials and processes as those of Embodiment 4, with the only difference being that the solid-to-liquid ratio of the waste MTO catalyst to the raw material solution in step S1 is 1:10.
[0071] Example 5
[0072] This embodiment uses substantially the same materials and processes as those of Embodiment 4, with the only difference being that the temperature in step S3 is 95°C.
[0073] Example 5-1
[0074] This embodiment uses substantially the same materials and processes as those of Embodiment 5, with the only difference being that the temperature in step S3 is 80°C.
[0075] Example 5-2
[0076] This embodiment uses substantially the same materials and processes as those of Embodiment 5, with the only difference being that the temperature in step S3 is 75°C.
[0077] Example 5-3
[0078] This embodiment uses substantially the same materials and processes as those of Embodiment 5, with the only difference being that the temperature in step S3 is 25°C.
[0079] Example 6
[0080] This embodiment uses substantially the same materials and processes as those of Embodiment 5, with the only difference being that the calcination temperature in step S5 is 500°C.
[0081] Example 7
[0082] This embodiment uses the same materials and processes as those of embodiment 5, except that: the SiO 2 With Ca(OH) 2 The molar ratio is 1:1.
[0083] Example 8
[0084] This embodiment uses the same materials and processes as those of embodiment 5, except that: the SiO 2 With Ca(OH) 2 The molar ratio is 1:4.
[0085] Comparative Example 1
[0086] This example uses substantially the same materials and processes as those of Example 5, with the only difference being that the raw material solution in step S1 is a mixed solution of ammonium sulfate and ammonium bicarbonate.
[0087] The effective ingredients of the alumina products and the phosphatic-silicon-calcium mixed fertilizer obtained in Examples 1 to 8 and Comparative Example 1 (according to GBT20412-2021) were tested, and the results are shown in Table 1:
[0088] Table 1
[0089]
[0090]
[0091] Referring to Example 5 and Comparative Example 1, it can be seen that the difference between the two is only the composition of the raw material solution. Example 5 uses a mixed solution of ammonium bisulfate and ammonium bicarbonate, while Comparative Example 1 uses a mixed solution of ammonium sulfate and ammonium bicarbonate. Referring to the results in Table 1, it can be seen that the alumina yield (90.4%) of Example 5 is much higher than the alumina yield (70.1%) of Comparative Example 1, and the alumina purity (97.8%) of Example 5 is significantly higher than the alumina purity (96.2%) of Comparative Example 1; and the effective silicon content (22.6%), effective calcium content (30.5%), and effective phosphorus content (23.7%) of the phosphorus-silicon-calcium mixed fertilizer of Example 5 are also much higher than the effective silicon content (18.5%), effective calcium content (25.7%), and effective phosphorus content (19.5%) of Comparative Example 1. Therefore, the embodiment of the present invention can further improve the yield and purity of the recovered alumina and the content of effective silicon, calcium and phosphorus in the phosphate-silicon-calcium mixed fertilizer by recycling the waste MTO catalyst using ammonium bisulfate and ammonium bicarbonate as raw materials.
[0092] Referring to Examples 2 to 3-2, it can be seen that the difference between them is that the reaction temperature of step S1 is different, which is 180°C, 280°C, 200°C, and 240°C, respectively. Referring to the results in Table 1, it can be seen that when other contents are not much different, the alumina yields of Examples 3 and 3-2 are significantly higher than those of other examples. Therefore, the reaction temperature of the first reaction is preferably 240-280°C.
[0093] Referring to Example 3 and Examples 4 to 4-2, it can be seen that the difference between them is that the solid-liquid ratio of the waste MTO catalyst to the raw material solution in step S1 is different, which is 1:3, 1:4, 1:6, and 1:10, respectively. Referring to the results in Table 1, it can be seen that the alumina yields of Examples 4 to 4-2 are significantly higher than those of Example 3, and thus, the solid-liquid ratio of the waste MTO catalyst to the raw material solution is preferably 1:4 to 1:10, and more preferably 1:6 to 1:10.
[0094] Referring to Example 4 and Examples 5 to 5-3, it can be seen that the difference between them is that the temperature in step S3 is different, which is 65°C, 95°C, 80°C, 75°C, and 25°C, respectively. Referring to the results in Table 1, it can be seen that the alumina yields of Examples 4 and Examples 5 to 2 are much higher than that of Example 5-3, and further, the alumina yields of Examples 5 and 5-1 are significantly higher than those of other examples. Therefore, in the step of obtaining the second solid-liquid mixture, the temperature of the system is preferably 65 to 95°C, and more preferably 80 to 95°C.
[0095] Referring to Examples 5, 7, and 8, it can be seen that the difference between them is that the SiO 2 With Ca(OH) 2 The molar ratios of are different, which are 0.5:1, 1:1, and 1:4. As shown in Table 1, the contents of effective silicon, effective calcium, and effective phosphorus in Examples 5 and 7 are significantly higher than those in Example 8. 2 With Ca(OH) 2 The molar ratio is preferably (0.5-1):1.
[0096] Unless otherwise defined, the terms used in the present invention have the meanings commonly understood by those skilled in the art.
[0097] The embodiments described in the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, changes and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above embodiments, but is only limited by the claims.
Claims
1. A method for recovering aluminum oxide from spent MTO catalyst, comprising the following steps: Performing a first reaction between the waste MTO catalyst and the raw material in a solvent to obtain a first solid-liquid mixture; Performing solid-liquid separation on the first solid-liquid mixture to obtain a first filtrate and a first filter residue; The first filtrate is mixed with ammonia gas or a solution containing ammonia water, and then subjected to a second reaction, and a precipitate is precipitated to obtain a second solid-liquid mixture; The second solid-liquid mixture is subjected to solid-liquid separation treatment to obtain basic ammonium aluminum carbonate solid and a second filtrate; as well as The basic ammonium aluminum carbonate solid is calcined to obtain aluminum oxide; Wherein, the raw materials include ammonium bisulfate and ammonium bicarbonate; in the first reaction, the reaction temperature is 180-300° C. and the pressure is 1.5-4.0 MPa.
2. The method according to claim 1, comprising: Providing a raw material solution, wherein the raw material solution comprises the raw material and the solvent; as well as mixing the waste MTO catalyst with the raw material solution to react; Wherein, in the raw material solution, the molar concentration of ammonium bisulfate is 2 to 10 mol / L, and the molar concentration of ammonium bicarbonate is 2 to 8 mol / L; and / or, In the raw material solution, the molar ratio of ammonium bisulfate to ammonium bicarbonate is 1:2 to 4:
1.
3. The method according to claim 2, wherein: The mass ratio of the waste MTO catalyst to the raw material solution is 1:3 to 1:10, further 1:4 to 1:10, further 1:6 to 1:10; and / or, In the raw material solution, the molar ratio of ammonium bisulfate to ammonium bicarbonate is 1:1 to 2:1; and / or, The solvent includes water.
4. The method according to claim 1, wherein: In the first reaction, the reaction temperature is 240-280° C. and the pressure is 1.5-2.5 MPa; and / or, The reaction time of the first reaction is 0.5 to 2 hours.
5. The method according to claim 1, wherein: In the step of obtaining the second solid-liquid mixture, the temperature of the system is 65 to 95° C., further 80 to 95° C.; and the pH value is 8 to 12.
6. The method according to claim 1, wherein: The calcination temperature is 300-500°C; and / or, The calcination time is 30 to 90 minutes; and / or, The CO2 and NH3 produced by the roasting treatment are recycled as raw materials for preparing ammonium bicarbonate; further, the CO2 and NH3 produced by the roasting treatment can be introduced into the second filtrate, and then the obtained mixed solution is added to the reaction system of the first reaction.
7. The method according to claim 1, wherein: The first filter residue is mixed with calcium hydroxide and ammonia water for activation treatment to obtain a phosphatic-silicon-calcium mixed fertilizer; and / or, The spent MTO catalyst comprises alumina, silicon dioxide and phosphorus pentoxide.
8. The method according to claim 7, wherein: The first filter residue includes amorphous SiO2 and P2O5; the molar ratio of SiO2 to Ca(OH)2 in the first filter residue is (0.5-1.5):1, further (0.5-1):1; the molar ratio of P2O5 to NH4OH in the first filter residue is 1:(2-4).
9. The method according to claim 7, wherein: The activation temperature is 70-95° C., and the activation time is 0.5-5 hours.
10. The method according to claim 1, wherein: The first filtrate contains cations and anions, wherein the cations include one, two or three of ammonium ions, hydrogen ions and aluminum ions; and the anions include sulfate ions and / or bicarbonate ions.