Method for preparing calcium fluoride and co-producing feed-grade calcium hydrophosphate by using white fertilizer

By combining white fertilizer with sulfuric acid, carbonate and acid solutions, efficient recycling of calcium fluoride in white fertilizer and the production of feed-grade calcium hydrogen phosphate is achieved, and the problem of low utilization efficiency of fluorine resource in white fertilizer is solved. , improve economic benefits and environmental protection.

CN119018925APending Publication Date: 2024-11-26MIANZHU HUAPU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411162445.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art cannot effectively utilize the fluorine resources in the by-product white fertilizer, resulting in poor economic benefits and potential environmental impact, and traditional utilization methods cannot achieve effective recycling of fluorine.

Method used

By mixing white fertilizer with sulfuric acid for extraction, a crude phosphoric acid solution and dephosphorylation residue were obtained. Then desulfurized using carbonate solution, then decarbonizing the desulfurized residue with acid solution was decarbonized and calcium-depleted, and finally the crude phosphoric acid solution was lime Milk neutralization to achieve cogeneration of calcium fluoride and feed-grade calcium hydrogen phosphate.

Benefits of technology

The high-quality recycling of calcium fluoride in white fertilizer has reached more than 94%, and the quality of feed-grade calcium hydrogen phosphate has been improved, the comprehensive utilization rate and economic benefits of resources have been improved, and the generation of waste liquid has been avoided. Improves environmental protection.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of phosphorus chemical industry and fluorine chemical industry, and provides a method for preparing calcium fluoride and co-producing feed-grade calcium hydrophosphate by using a white fertilizer. The method comprises the following steps: extracting white fertilizer slurry by using sulfuric acid to obtain dephosphorized residues and a crude phosphoric acid solution, desulfurizing the dephosphorized residues by using carbonate to obtain a desulfurized mother solution and desulfurized residues, and carrying out decarbonization and calcium removal on the desulfurized residues by using an acid solution to obtain calcium fluoride; meanwhile, purifying and neutralizing the crude phosphoric acid solution to obtain feed-grade calcium hydrogen phosphate. According to the method provided by the invention, each component in the white fertilizer can be effectively recycled, especially high-quality calcium fluoride can be obtained, and meanwhile, feed-grade calcium hydrophosphate can be co-produced, so that the comprehensive utilization rate of resources and the economic benefit are high; the result of the embodiment shows that the high-quality calcium fluoride product can be obtained through the method, the calcium fluoride content reaches 94% or above, and the quality of the obtained feed-grade calcium hydrophosphate is superior to the I-type index of the calcium hydrophosphate of the national standard GB 22549-2017 feed additive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorine chemical industry and phosphorus chemical industry, and in particular to a method for preparing calcium fluoride and co-producing feed-grade calcium hydrogen phosphate by utilizing white fertilizer. Background Art

[0002] Fluorine chemical products mainly include fluorine-containing polymer materials, fluorine-containing refrigerants, fluorine-containing fine chemicals and inorganic fluoride salts, which are widely used in the fields of electronics, equipment manufacturing, construction, home appliances, pesticides, medicine, etc. The main raw material of the fluorine chemical industry chain is fluorite, commonly known as fluorspar, which is mainly composed of calcium fluoride (CaF2). It is one of the inorganic non-metallic minerals in nature. Fluorite ore with a calcium fluoride content of ≥30% is processed to form fluorite powder with a calcium fluoride content of ≥97%, which is used to produce hydrofluoric acid. Hydrofluoric acid can be used to prepare fluorine-containing refrigerants, fluorine-containing fine chemicals, inorganic fluoride salts, etc. However, fluorite is a non-renewable resource, and it is of great significance to use other raw materials to replace fluorite in the production of fluorine chemical products.

[0003] Phosphate ore, which is widely used in phosphorus chemical industry, contains about 3% fluorine. Most phosphorus chemical production enterprises are strengthening the research on the use of fluorine byproducts to process fluorine-containing products. The comprehensive utilization of fluorine resources associated with phosphate ore is not only in line with my country's basic national policy of developing a circular economy, but also a reliable path for the future development of fluorine chemical industry. my country's feed phosphate production is large-scale, and the consumption of phosphate rock accounts for about 10%. At present, the basic process of feed phosphate is still wet extraction. Through lime milk neutralization and defluorination, the byproduct is fertilizer-grade calcium hydrogen phosphate (commonly known as white fertilizer) product with a P2O5 content of about 25%. The average elemental fluorine content in white fertilizer is 15%, and the maximum can reach 20%, with an annual output of nearly 2 million tons. The traditional method of using white fertilizer is to use it as an auxiliary material to provide a phosphorus source for compound fertilizers, or to apply it directly as a low-cost fertilizer. The economic benefits of the above utilization methods are poor, and it is impossible to achieve the effective utilization of fluorine. In recent years, there has been some controversy over the impact of fluorine on crops and the ecological environment.

[0004] In summary, it is particularly important to effectively recycle fluorine and other resources in by-product white fertilizer, improve the utilization value of its components, and generate greater economic and social benefits. Summary of the invention

[0005] In view of this, the present invention provides a method for preparing calcium fluoride and co-producing feed-grade calcium hydrogen phosphate using white fertilizer. The method provided by the present invention can effectively recycle various components in the white fertilizer, especially can obtain high-quality calcium fluoride, and co-produce feed-grade calcium hydrogen phosphate, with high comprehensive resource utilization and economic benefits.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] A method for preparing calcium fluoride and co-producing feed-grade calcium hydrogen phosphate using white fertilizer comprises the following steps:

[0008] The white fertilizer slurry is mixed with sulfuric acid for extraction, and the obtained extraction slurry is separated into solid and liquid to obtain a crude phosphoric acid solution and a dephosphorization residue respectively;

[0009] Desulfurizing the dephosphorization residue with a carbonate solution, and obtaining a sulfur-containing mother liquor and desulfurization residue after solid-liquid separation;

[0010] The desulfurization residue is decarbonized and decalcified with an acid solution, and calcium fluoride and calcium-containing mother liquor are obtained after solid-liquid separation; the crude phosphoric acid solution is purified and then neutralized with lime milk to obtain the feed-grade calcium hydrogen phosphate.

[0011] Preferably, the white fertilizer slurry is obtained by beating white fertilizer; the liquid-to-solid ratio of the white fertilizer beating is 1.5 to 4:1.

[0012] Preferably, the extraction temperature is 25-40° C., and the extraction time is 1-2 h; and the SO 3 concentration in the extraction slurry is 2-3%.

[0013] Preferably, the method of desulfurizing the dephosphorization residue using a carbonate solution comprises: pulping the dephosphorization residue and mixing it with a carbonate solution for desulfurization;

[0014] The liquid-to-solid ratio of the dephosphorization slag slurry is 1.5-4.5:1; the carbonate is sodium carbonate or ammonium carbonate; and the concentration of the carbonate solution is 20-40wt%.

[0015] Preferably, the desulfurization temperature is 30-40°C and the time is 0.5-2h.

[0016] Preferably, when the carbonate is sodium carbonate, the process further comprises concentrating and crystallizing the sulfur-containing mother liquor to obtain sodium sulfate.

[0017] Preferably, the method of decarbonizing and decalcifying the desulfurized slag using an acid solution comprises: slurrying the desulfurized slag and mixing it with an acid solution for decarbonization and decalcification; the liquid-to-solid ratio of the desulfurized slag slurry is 2 to 4:1; the concentration of the acid solution is 6 to 25 wt%; the temperature of the decarbonization and decalcification is 15 to 50°C, and the time is 1 to 4 hours.

[0018] Preferably, the acid solution is a nitric acid solution;

[0019] After obtaining the calcium-containing mother liquor, the method further comprises mixing the calcium-containing mother liquor with nitric acid and ammonia water, and concentrating and crystallizing the mixture to obtain calcium ammonium nitrate.

[0020] Preferably, the method for purifying the crude phosphoric acid solution comprises: mixing the crude phosphoric acid solution with a white fertilizer slurry to desulfurize the crude phosphoric acid to obtain desulfurized crude phosphoric acid and pre-decomposed white fertilizer;

[0021] The desulfurized crude phosphoric acid and lime milk are mixed to perform defluorination to obtain purified phosphoric acid clear liquid and secondary white fertilizer;

[0022] The endpoint pH value of the defluorination is 1.8-3.5; the pre-decomposed white fertilizer and the secondary white fertilizer are returned to the step of preparing white fertilizer slurry.

[0023] Preferably, the lime milk neutralization comprises: neutralizing the purified phosphoric acid clear solution and lime milk; the neutralization endpoint pH value is 5-7.

[0024] The present invention provides a method for preparing calcium fluoride and co-producing feed-grade calcium hydrogen phosphate by using white fertilizer, comprising the following steps: mixing white fertilizer slurry and sulfuric acid for extraction, separating the obtained extraction slurry into solid and liquid to obtain crude phosphoric acid solution and dephosphorization residue respectively; desulfurizing the dephosphorization residue with carbonate solution, obtaining sulfur-containing mother liquor and desulfurization residue after solid-liquid separation; decarbonizing and decalcifying the desulfurization residue with acid solution, obtaining calcium fluoride and calcium-containing mother liquor after solid-liquid separation; purifying the crude phosphoric acid solution and neutralizing it with lime milk to obtain the feed-grade calcium hydrogen phosphate. The present invention analyzes the chemical components in white fertilizer, and finds that fluorine mostly exists in the form of calcium fluoride, and some and a small amount exist in the form of fluoride such as calcium fluorophosphate, calcium fluorosilicate, fluoroaluminate, etc. The pH of white fertilizer is generally about 3.5, which is acidic, and P2O5 is mostly citric acid soluble and mostly exists in the form of calcium hydrogen phosphate. According to the characteristics of each component in the white fertilizer, the present invention first uses sulfuric acid to extract the white fertilizer slurry, converts the calcium therein into calcium sulfate precipitation and enters the dephosphorization residue, while phosphorus mainly exists in the liquid phase in the form of phosphate, and obtains a crude phosphoric acid solution; then the dephosphorization residue and carbonate are reacted, so that the sulfate in the dephosphorization residue enters the liquid phase, and the calcium is converted into calcium carbonate, and a desulfurization mother liquor and a desulfurization residue are obtained; finally, the desulfurization residue and the acid solution are mixed, and the calcium carbonate therein is converted into a soluble calcium salt, while calcium fluoride remains in the solid phase, that is, the calcium fluoride product is obtained; at the same time, the crude phosphoric acid solution is purified and neutralized to obtain feed-grade calcium hydrogen phosphate. The results of the embodiment show that the method provided by the present invention can obtain a high-quality calcium fluoride product, wherein the calcium fluoride content reaches more than 94%, and the quality of the obtained feed-grade calcium hydrogen phosphate is better than the national standard GB 22549-2017 feed additive calcium hydrogen phosphate type I index.

[0025] Furthermore, the present invention also concentrates and crystallizes the sulfur-containing mother liquor to prepare Glauber's salt, and concentrates the calcium-containing mother liquor and ammonia water to obtain calcium ammonium nitrate, thereby realizing the full element recycling of white fertilizer, further improving the comprehensive utilization rate of resources and economic benefits, while avoiding the generation of waste liquid and improving environmental protection. DETAILED DESCRIPTION

[0026] The present invention provides a method for preparing calcium fluoride and co-producing feed-grade calcium hydrogen phosphate by using white fertilizer, comprising the following steps:

[0027] The white fertilizer slurry is mixed with sulfuric acid for extraction, and the obtained extraction slurry is separated into solid and liquid to obtain a crude phosphoric acid solution and a dephosphorization residue respectively;

[0028] Desulfurizing the dephosphorization residue with a carbonate solution, and obtaining a sulfur-containing mother liquor and desulfurization residue after solid-liquid separation;

[0029] The desulfurization residue is decarbonized and decalcified by using an acid solution, and calcium fluoride and calcium-containing mother liquor are obtained after solid-liquid separation; the acid solution is a nitric acid solution or a hydrochloric acid solution;

[0030] The crude phosphoric acid solution is purified and then neutralized with lime milk to obtain the feed-grade calcium hydrogen phosphate.

[0031] The present invention mixes white fertilizer slurry and sulfuric acid for extraction, separates the solid and liquid of the obtained extraction slurry, and obtains crude phosphoric acid solution and dephosphorization residue respectively. In the present invention, the white fertilizer slurry is obtained by beating white fertilizer; the present invention has no special requirements for the white fertilizer, and the one known to those skilled in the art can be used; in a specific embodiment of the present invention, the total mass fraction of P2O5 in the white fertilizer is preferably 20.00-28.50wt%, more preferably 22.58wt%, and the mass fraction of effective P2O5 is preferably 10.00-18.00wt%, more preferably 13.53wt%; the mass fractions of other components in the white fertilizer are preferably: F: 13.00-23.00wt%, CaO: 36.0-46.0wt%, SO3: 2.0-5.0wt%, MgO: 1.0-3.0wt%, Fe2O3: 1.0-4.0wt%, Al2O3: 0.5-2.5wt%.

[0032] In the present invention, the liquid-to-solid ratio of the white fertilizer slurry is preferably 1.5-4:1, more preferably 2-3:1; the white fertilizer slurry is specifically slurrying with water; the extraction temperature is preferably 25-40°C, the time is preferably 1-2h, more preferably 1-1.5h; the sulfuric acid is preferably concentrated sulfuric acid, that is, sulfuric acid with a commercial mass fraction of 98%; the SO3 concentration in the extraction slurry is preferably 2-3wt%; in a specific embodiment of the present invention, it is preferred to control the amount of sulfuric acid added according to the SO3 concentration in the extraction slurry.

[0033] In the present invention, the chemical reaction equation involved in the extraction process is as follows:

[0034] CaHPO4+H2SO4+2H2O→H3PO4+CaSO4.2H2O↓;

[0035] Ca5(PO4)3F+5H2SO4+10H20→3H3PO4+10CaSO4.2H2O+HF↑;

[0036] 3Ca5(PO4)3F+H3PO4→5Ca3(PO4)2↓+3HF↑;

[0037] Ca(OH)2+2HF→CaF2↓+H2O.

[0038] After the extraction is completed, the obtained extraction slurry is subjected to solid-liquid separation. The solid-liquid separation method is preferably filtration. The liquid obtained by filtration is a crude phosphoric acid solution, and the filter residue is a dephosphorization residue; the content of insoluble P2O5 in the dephosphorization residue is preferably 0.2-2.0wt%, the content of water-soluble P2O5 is preferably 0.1-1.5wt%, the content of F is preferably 12.50-22.40wt%, and the content of SO3 is preferably 30.0-38.0wt%; the content of P2O5 in the crude phosphoric acid solution is preferably 6.0-10.0wt%, the content of F is preferably 0.5-1.2wt%, and the content of SO3 is preferably 1.0-3.0wt%.

[0039] After obtaining the dephosphorization residue, the present invention uses a carbonate solution to desulfurize the dephosphorization residue, and obtains a sulfur-containing mother liquor and a desulfurization residue after solid-liquid separation. In the present invention, the method of desulfurizing the dephosphorization residue using a carbonate solution preferably includes: slurrying the dephosphorization residue and mixing it with a carbonate solution for desulfurization. In the present invention, the liquid-solid ratio of the dephosphorization residue slurry is preferably 1.5-4.5:1, more preferably 2-3:1; the dephosphorization residue slurrying is specifically slurrying with water, and the residue slurry is obtained after slurrying; the carbonate is preferably sodium carbonate or ammonium carbonate, more preferably sodium carbonate, and further preferably industrial sodium carbonate; the concentration of the carbonate solution is preferably 20-40wt%, more preferably 30-35wt%; the molar ratio of the carbonate in the carbonate solution to the calcium sulfate in the desulfurization residue is preferably 1-1.1:1; in a specific embodiment of the present invention, the carbonate solution is preferably pumped into the residue slurry reaction tank while stirring.

[0040] In the present invention, the temperature of the first desulfurization is preferably 30-40° C., the time is preferably 0.5-2 h, and more preferably 75 min. Taking sodium carbonate as an example, the chemical reaction equation involved in the desulfurization process is as follows:

[0041] CaSO4·2H2O+Na2CO3→CaCO3↓+Na2SO4+2H2O.

[0042] After desulfurization is completed, solid-liquid separation is carried out. The solid-liquid separation method is preferably filtration. The liquid obtained by filtration is the sulfur-containing mother liquor, and the filter residue is the desulfurization residue; the SO3 content in the desulfurization residue is preferably 2.0-4.0wt%; the SO3 content in the sulfur-containing mother liquor is preferably 5.0-9.0wt%.

[0043] In the present invention, when the carbonate is sodium carbonate, it is preferred that the sulfur-containing mother liquor is concentrated and crystallized to obtain sodium sulfate. The present invention has no special requirements for the specific conditions of the concentration and crystallization, and those familiar to those skilled in the art can be used.

[0044] After obtaining the desulfurized slag, the present invention uses an acid solution to decarbonize and decalcify the desulfurized slag, and obtains calcium fluoride and calcium-containing mother liquor after solid-liquid separation. In the present invention, the method of using an acid solution to decarbonize and decalcify the desulfurized slag preferably includes: mixing the desulfurized slag with an acid solution after pulping for decarbonization and decalcification; the liquid-solid ratio of the desulfurized slag pulping is preferably 2-4:1, more preferably 2-3:1; the acid solution is preferably a nitric acid solution; the concentration of the nitric acid solution is preferably 6-25wt%, more preferably 10-20wt%; the molar ratio of nitric acid in the nitric acid solution to calcium carbonate in the desulfurized slag is preferably 2.0-2.1:1; the temperature of the decarbonization and decalcification is preferably 15-50°C, more preferably 35-45°C, and the time is preferably 1-4h, more preferably 2.5-3h; during the decarbonization and decalcification process, the acid solution reacts with the calcium carbonate in the desulfurized slag to generate a soluble calcium salt, which enters the liquid phase, and the calcium fluoride does not react and remains in the solid phase. The chemical reaction formula involved in the decarburization and decalcification process is as follows:

[0045] CaCO3+2HNO3→Ca(NO3)2+H2O+CO2↑.

[0046] After decarburization and decalcification, solid-liquid separation is performed. The solid-liquid separation method is preferably filtration. The liquid obtained by filtration is a calcium-containing mother liquor, and the filter residue is calcium fluoride. The CaF2 content in the calcium fluoride is preferably above 94wt%.

[0047] In the present invention, when the acid solution is a nitric acid solution, the process further comprises concentrating and crystallizing the calcium-containing mother liquor after mixing with nitric acid and ammonia water to obtain calcium ammonium nitrate; the present invention has no special requirements on the dosage of the nitric acid and ammonia water, and nitric acid and ammonia water can be added to the calcium-containing mother liquor according to the indicators of ammonium nitrogen and nitrate nitrogen in agricultural calcium ammonium nitrate; the present invention has no special requirements on the specific conditions of the concentration and crystallization, and those familiar to those skilled in the art can be adopted.

[0048] After obtaining the crude phosphoric acid solution, the present invention purifies the crude phosphoric acid solution and then neutralizes it with lime milk to obtain the feed-grade calcium hydrogen phosphate. In the present invention, the method for purifying the crude phosphoric acid solution preferably includes: mixing the crude phosphoric acid solution and white fertilizer slurry to perform crude phosphoric acid desulfurization to obtain desulfurized crude phosphoric acid and pre-decomposed white fertilizer; mixing the desulfurized crude phosphoric acid and lime milk to perform defluorination to obtain purified phosphoric acid clear solution and secondary white fertilizer; the endpoint pH value of the defluorination is 1.8 to 3.5, more preferably 2.3; the pre-decomposed white fertilizer and secondary white fertilizer are returned to the step of preparing white fertilizer slurry; the preparation method of the white fertilizer slurry used for crude phosphoric acid desulfurization is consistent with the white fertilizer slurry used in the extraction step, which will not be repeated here; in the crude phosphoric acid desulfurization, the white fertilizer The molar ratio of P in the slurry to SO3 in the crude phosphoric acid is preferably 1.0-1.1:1; the temperature for desulfurization of the crude phosphoric acid is preferably 30-40°C, and the time for desulfurization of the crude phosphoric acid is preferably 1-2h, more preferably 1h; the present invention utilizes white fertilizer slurry to remove sulfur from the crude phosphoric acid solution, that is, the residual sulfuric acid in the crude phosphoric acid solution is used to pre-decompose the raw white fertilizer to achieve the purpose of saving sulfuric acid; filtration is performed after the second desulfurization to obtain desulfurized crude phosphoric acid and pre-decomposed white fertilizer; in the present invention, the SO3 content in the desulfurized crude phosphoric acid is preferably 0.30-0.60wt%.

[0049] In the present invention, the mass fraction of CaO in the lime milk is preferably 6-15%, more preferably 8-13%; the defluorination temperature is preferably 35-40°C, and the time is preferably 1-2h, more preferably 1.5-2h; during the defluorination process, CaO reacts with fluorine in the desulfurized crude phosphoric acid to generate calcium fluoride precipitate, thereby achieving defluorination; after the defluorination is completed, filtration is performed to obtain purified phosphoric acid clear liquid and secondary white fertilizer; the SO3 content in the purified phosphoric acid clear liquid is preferably 0.10-0.35%, the F content is preferably 0.009-0.0185%, and the P2O5 content is preferably 3.0-7.0%; the pre-decomposed white fertilizer and the secondary white fertilizer are returned to the white fertilizer beating step, specifically returned to the extraction step as raw materials and used in combination with the initial white fertilizer raw material to improve the total fluorine yield.

[0050] In the present invention, the lime milk neutralization preferably comprises: neutralizing the purified phosphoric acid clear solution and lime milk; the neutralization end point pH value is 5-7, preferably 6.5; the neutralization temperature is preferably 40-45°C, more preferably 40-41°C, the neutralization time is preferably 2-3h, more preferably 2-2.5h; the lime milk used for the neutralization is the same as the lime milk used for defluorination, which will not be repeated here.

[0051] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] Example 1

[0053] (1) 1000 g of white fertilizer was mixed with water at a liquid-to-solid ratio of 2:1 and pumped into a stirred reaction tank, 210 g of concentrated sulfuric acid (98 wt%) was slowly added, and the reaction was carried out for 1 h at a reaction temperature of 25° C. The dephosphorization residue and crude phosphoric acid solution were filtered out.

[0054] Among them, the chemical composition of white fertilizer is: total P2O5: 22.58wt%, effective P2O5: 13.53wt%, F: 18.35wt%, CaO: 45.01wt%, SO3: 3.79wt%, MgO: 1.58wt%, Fe2O3: 1.15wt%, Al2O3: 0.6%;

[0055] The chemical composition of the dephosphorization residue is: insoluble P2O5: 0.95wt%, water-soluble P2O5: 1.31wt%, F: 15.84wt%, CaO: 41.36wt%, SO3: 32.68wt%, MgO: 0.94wt%, Fe2O3: 0.9wt%, Al2O3: 0.5wt%;

[0056] (2) The dephosphorization residue is slurried in a stirring reaction tank at a liquid-solid ratio of 2:1, 200g of industrial sodium carbonate is weighed, water is added to prepare a 30% solution, and the solution is pumped into the residue slurry reaction tank while stirring. The reaction temperature is 30°C and the reaction time is 75min, so that the sulfate ions in the residue enter the liquid phase, and the desulfurization residue is filtered and separated to obtain the chemical composition of the desulfurization residue: total P2O5: 1.20wt%, F: 23.40wt%, CaO: 50.11wt%, SO3: 3.70wt%. The obtained sulfur-containing mother liquor is concentrated and crystallized to produce Glauber's salt.

[0057] (3) The desulfurized residue was slurried in a stirred reaction tank at a liquid-solid ratio of 2:1, 1100g of a 20wt% nitric acid solution was added, and the mixture was reacted at 35°C for 2.5h to remove the calcium carbonate component. After the reaction was completed, 380.9g of high-fluorine-containing high-quality calcium fluoride solid phase was obtained by filtration and separation. The chemical composition of calcium fluoride was: F: 45.86wt%, Ca: 48.28wt%, SO3: 1.83wt%, total P2O5: 0.89wt%, SiO2: 1.29wt%, Fe2O3: 0.85wt%, Al2O3: 0.048wt%, MgO: 0.22wt%; the calcium fluoride content was 94.16wt%, and the total fluorine recovery rate was 95.2wt%. The calcium nitrate mother liquor obtained after filtration was supplemented with ammonia water and nitric acid to adjust the ammonium nitrogen and nitrate nitrogen indicators, and concentrated and crystallized to produce agricultural calcium ammonium nitrate.

[0058] (4) The crude phosphoric acid solution obtained in step (1) can be processed into feed-grade calcium hydrogen phosphate. The specific steps are as follows: The chemical composition of crude phosphoric acid is: P2O5: 6.78wt%, F: 0.97wt%, SO3: 2.05wt%, CaO: 0.15wt%, MgO: 0.28wt%, Fe2O3: 0.31wt%, Al2O3: 0.004wt%.

[0059] 200g of the above-mentioned raw material white fertilizer is slurried with water at a liquid-solid ratio of 2:1, and gradually pumped into the obtained crude phosphoric acid solution for reaction for 1h, and the reaction temperature is 30°C to remove SO3 in the crude phosphoric acid. After separation, desulfurized crude phosphoric acid and pre-decomposed white fertilizer are obtained. The desulfurized crude phosphoric acid enters the next step, and the pre-decomposed white fertilizer returns to the above-mentioned first step and is used in combination with the raw material white fertilizer. The chemical composition of the obtained desulfurized crude phosphoric acid is: P2O5: 7.24wt%, F: 0.89wt%, SO3: 0.54wt%, CaO: 0.45wt%, MgO: 0.47wt%, Fe2O3: 0.37wt%, Al2O3: 0.001wt%.

[0060] The obtained crude phosphoric acid was pumped into 553g (containing CaO: 12.24wt%) lime milk solution while stirring, the reaction time was controlled at 1.5h, the reaction temperature was 35°C, the pH value at the reaction end point was 2.3, and solid phase secondary white fertilizer and purified phosphoric acid clear liquid were obtained after filtration and separation; the obtained secondary white fertilizer was 135.6g, the secondary white fertilizer was returned to the raw material section for use with the raw white fertilizer, and the purified phosphoric acid clear liquid was entered into the neutralization and production of feed-grade calcium hydrogen phosphate section for use.

[0061] The chemical composition of the secondary white fertilizer is: total P2O5: 28.72wt%, effective P2O5: 22.34wt%, SO3: 1.72wt%, CaO: 37.98wt%, MgO: 1.68wt%, F: 18.47wt%, Fe2O3: 6.09wt%, Al2O3: 1.2wt%;

[0062] The chemical composition of the purified phosphoric acid clear liquid is: P2O5: 3.41wt%, F: 0.01wt%, SO3: 0.28wt%, CaO: 1.04wt%, MgO: 0.26wt%, Fe2O3: 0.07, Al2O3: 0.001wt%.

[0063] The obtained purified phosphoric acid clear liquid was stirred and pumped into 522g (containing CaO: 12.24wt%) lime milk solution, the reaction time was controlled at 2.0h, the reaction temperature was 40°C, the reaction end point pH value was 6.5, and solid phase feed grade calcium hydrogen phosphate was obtained after filtration and separation, the total recovery rate of P2O5 reached 89%, and the mother liquor containing a small amount of phosphorus was recovered in a traditional way and discharged in compliance with the standards. The obtained feed grade calcium hydrogen phosphate index is: total P: 18.5wt%, Ca: 24.73wt%, F: 0.16wt%, citric acid soluble P: 17.10wt%, As: 9.0mg / kg, Pb: 16.0mg / kg, Cd: 4.0mg / kg, Cr: 12.0mg / kg, free water: 2.5%, and its quality is better than the national standard GB 22549-2017 feed additive calcium hydrogen phosphate type I index.

[0064] Example 2

[0065] (1) 836.7g of white fertilizer and 135.6g of the secondary white fertilizer in Example 1 were mixed, and water was added to the stirred reaction tank at a liquid-solid ratio of 3.5:1, and 200g of concentrated sulfuric acid (98%) was slowly added. The reaction temperature was 40°C, the reaction time was about 1.5h, and the reaction temperature was filtered to obtain dephosphorization residue and crude phosphoric acid solution. The chemical composition of the dephosphorization residue is: insoluble P2O5: 1.3wt%, water-soluble P2O5: 0.8wt%, F: 16.33%, CaO: 40.79wt%, SO3: 33.21wt%, MgO: 0.86wt%, Fe2O3: 0.74wt%, Al2O3: 0.4wt%. The chemical composition of the crude phosphoric acid solution is: P2O5: 7.53wt%, SO3: 2.45wt%, CaO: 0.16wt%, MgO: 0.10wt%, F: 1.17wt%, Fe2O3: 0.06wt%, Al2O3: 0.002wt%.

[0066] (2) The dephosphorization residue is slurried in a stirring reaction tank at a liquid-solid ratio of 3:1, 200g of industrial sodium carbonate is weighed, water is added to prepare a 30wt% solution, and the solution is pumped into the residue slurry reaction tank while stirring. The reaction temperature is 40°C and the reaction time is 75min, so that the sulfate ions in the residue enter the liquid phase, and the desulfurization residue is filtered and separated to obtain the chemical composition of the desulfurization residue: total P2O5: 1.59wt%, F: 22.80wt%, CaO: 51.74wt%, SO3: 2.85wt%. The obtained mother liquor is concentrated and crystallized to produce Glauber's salt.

[0067] (3) The desulfurized residue was slurried in a stirred reaction tank at a liquid-solid ratio of 2:1, 1150g of 20wt% nitric acid solution was added, and the mixture was reacted at 42°C for 2.0h to remove the calcium carbonate component. After the reaction was completed, the solid phase of high-fluorine-containing high-quality calcium fluoride was obtained by filtration and separation. The chemical composition of calcium fluoride was: F: 45.01wt%, Ca: 47.8wt%, SO3: 1.08wt%, total P2O5: 0.54wt%, SiO2: 0.89wt%, Fe2O3: 0.90wt%, Al2O3: 0.033wt%, MgO: 0.16wt%; the calcium fluoride content was 92.50wt%, and the total fluorine recovery rate was 96.8wt%. The filtered calcium nitrate mother liquor was supplemented with ammonia water and nitric acid to adjust the ammonium nitrogen and nitrate nitrogen indicators, and concentrated and crystallized to produce agricultural calcium ammonium nitrate.

[0068] (4) The crude phosphoric acid solution obtained in step (1) can be processed into feed-grade calcium hydrogen phosphate for sale. The specific steps are as follows:

[0069] 200g of the above-mentioned raw material white fertilizer is slurried with water at a liquid-solid ratio of 2:1, and gradually pumped into the obtained crude phosphoric acid solution for reaction for 1h, and the reaction temperature is 40°C to remove SO3 in the crude phosphoric acid. After separation, desulfurized crude phosphoric acid and pre-decomposed white fertilizer are obtained. The desulfurized crude phosphoric acid enters the next step, and the pre-decomposed white fertilizer returns to the above-mentioned first step and is used in combination with the raw material white fertilizer. The chemical composition of the obtained desulfurized crude phosphoric acid is: P2O5: 8.02wt%, F: 1.08wt%, SO3: 0.32wt%, CaO: 0.61wt%, MgO: 0.37wt%, Fe2O3: 0.24wt%, Al2O3: 0.002wt%.

[0070] The obtained desulfurized crude phosphoric acid was pumped into 644g (containing CaO: 9.97wt%) lime milk solution while stirring, the reaction time was controlled at 2.0h, the reaction temperature was 40°C, the pH value at the reaction end point was 2.3, and solid phase secondary white fertilizer and purified phosphoric acid clear liquid were obtained after filtration and separation. The secondary white fertilizer was returned to the raw material section for use with the raw white fertilizer, and the purified phosphoric acid clear liquid was entered into the neutralization and production of feed-grade calcium hydrogen phosphate section for use.

[0071] The chemical composition of secondary white fertilizer is: total P2O5: 29.13wt%, effective P2O5: 23.62wt%, SO3: 1.43%, CaO: 36.38wt%, MgO: 1.29wt%, F: 19.82wt%, Fe2O3: 5.88wt%, Al2O3: 0.82wt%.

[0072] The chemical composition of the purified phosphoric acid clear liquid is: P2O5: 5.79wt%, F: 0.018wt%, SO3: 0.18wt%, CaO: 1.20wt%, MgO: 0.32wt%, Fe2O3: 0.03wt%, Al2O3: 0.006wt%.

[0073] The obtained purified phosphoric acid clear liquid was pumped into 642g (containing CaO: 12.24wt%) lime milk solution while stirring, the reaction time was controlled at 2.5h, the reaction temperature was 41°C, the pH value at the reaction end point was 6.5, and solid feed-grade calcium hydrogen phosphate was obtained after filtration and separation. The total recovery rate of P2O5 reached 90%, and the mother liquor containing a small amount of phosphorus was neutralized and recovered in a traditional manner and then discharged in compliance with the standards.

[0074] The obtained feed-grade calcium hydrogen phosphate has the following indicators: total P: 18.37wt%, Ca: 25.01wt%, F: 0.145wt%, citric acid-soluble P: 17.34wt%, As: 6.0mg / kg, Pb: 11.0mg / kg, Cd: 2.0mg / kg, Cr: 8.0mg / kg, free moisture: 1.8wt%; its quality is better than the national standard GB 22549-2017 feed additive calcium hydrogen phosphate type I indicator.

[0075] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing calcium fluoride and co-producing feed-grade calcium hydrogen phosphate using white fertilizer, It is characterized in that The following steps are involved: The white fertilizer slurry is mixed with sulfuric acid for extraction, and the obtained extraction slurry is separated into solid and liquid to obtain a crude phosphoric acid solution and a dephosphorization residue respectively; Desulfurizing the dephosphorization residue with a carbonate solution, and obtaining a sulfur-containing mother liquor and desulfurization residue after solid-liquid separation; Decarbonizing and decalcifying the desulfurization residue with an acid solution, and obtaining calcium fluoride and a calcium-containing mother liquor after solid-liquid separation; The crude phosphoric acid solution is purified and then neutralized with lime milk to obtain the feed-grade calcium hydrogen phosphate.

2. The method according to claim 1, It is characterized in that The white fertilizer slurry is obtained by beating white fertilizer; the liquid-to-solid ratio of the white fertilizer beating is 1.5-4:

1.

3. The method according to claim 1 or 2, It is characterized in that The extraction temperature is 25-40°C and the time is 1-2 hours; SO in the extraction slurry 3 The concentration is 2-3%.

4. The method according to claim 1, It is characterized in that The method for desulfurizing the dephosphorization residue using a carbonate solution comprises: slurrying the dephosphorization residue and mixing it with a carbonate solution for desulfurization; the liquid-to-solid ratio of the dephosphorization residue slurry is 1.5-4.5:1; the carbonate is sodium carbonate or ammonium carbonate; and the concentration of the carbonate solution is 20-40wt%.

5. The method according to claim 4, It is characterized in that The desulfurization temperature is 30-40°C and the time is 0.5-2h.

6. The method according to claim 4 or 5, It is characterized in that When the carbonate is sodium carbonate, the method further comprises concentrating and crystallizing the sulfur-containing mother liquor to obtain sodium sulfate.

7. The method according to claim 1, It is characterized in that The method for decarbonizing and decalcifying the desulfurized slag using an acid solution comprises: slurrying the desulfurized slag and mixing it with an acid solution for decarbonizing and decalcifying; the liquid-to-solid ratio of the desulfurized slag slurry is 2 to 4:1; the concentration of the acid solution is 6 to 25 wt%; the temperature of the decarbonization and decalcification is 15 to 50°C, and the time is 1 to 4 hours.

8. The method according to claim 1, It is characterized in that The acid solution is a nitric acid solution; After obtaining the calcium-containing mother liquor, the method further comprises mixing the calcium-containing mother liquor with nitric acid and ammonia water, and concentrating and crystallizing the mixture to obtain calcium ammonium nitrate.

9. The method according to claim 1, It is characterized in that The method for purifying the crude phosphoric acid solution comprises: mixing the crude phosphoric acid solution with white fertilizer slurry to desulfurize the crude phosphoric acid to obtain desulfurized crude phosphoric acid and pre-decomposed white fertilizer; The desulfurized crude phosphoric acid and lime milk are mixed to perform defluorination to obtain purified phosphoric acid clear liquid and secondary white fertilizer; The endpoint pH value of the defluorination is 1.8-3.5; the pre-decomposed white fertilizer and the secondary white fertilizer are returned to the step of preparing white fertilizer slurry.

10. The method according to claim 9, It is characterized in that The lime milk neutralization comprises: neutralizing the purified phosphoric acid clear solution and lime milk; the neutralization end point pH value is 5-7.