Production process for improving anti-falling performance of lithium-aluminum-silicon glass
Through the low-temperature short-term preheating and low-temperature long-term salt bath strengthening process, the compressive stress instability caused by uneven ion distribution in the lithium-aluminum silicon glass is solved, which significantly improves its fall resistance and achieves a more uniform deep stress And better anti-fall effect.
Patent Information
- Application Number
- CN202411417839.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-26
AI Technical Summary
The existing lithium-aluminum silicon glass preheated for a long time at high temperatures leads to uneven internal ion distribution, unstable compressive stress, and poor fall resistance.
Low-temperature short-term preheating and low-temperature long-term salt bath strengthening technology, the molten salt of sodium nitrate and potassium nitrate is strengthened twice, and the mass ratio of sodium salt to potassium salt is controlled, and the replacement of Na ions and Li ions is promoted, thereby improving Deep stress uniformity and fall resistance.
The anti-falling performance of lithium-aluminum silicon glass is significantly improved, the deep stress is more uniform, and the sodium stress curve is smoother, avoiding the internal structural instability caused by high-temperature salt baths and enhancing the anti-falling ability of the glass.
Smart Images

Figure CN119019099A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass processing, and in particular to a production process for improving the anti-drop performance of lithium aluminosilicate glass. Background Art
[0002] In real life, mobile phones may be accidentally dropped, fall to the ground, or pierce through hard objects, causing the screen to break. In order to improve the drop resistance, the industry has upgraded the sodium aluminum silicate glass previously used by the industry to lithium aluminum silicate glass by increasing the direction of the deep compressive stress inside the product.
[0003] The drop resistance of glass of the same thickness is related to (KIC / Y*C)+CS30 / CS50, CT value, CS30 / CS50 / CS70 and the width of surface microcracks, where KIC is the fracture toughness, Y is the coefficient, C is the width of surface microcracks, CS30 / CS50 / CS70 / CS90 are the compressive stress at a depth of 30μm / 50μm / 70μm / 90μm of the glass, and CT value is the central tensile stress of the glass.
[0004] When stimulated by a hard object, the force diffuses from the outside to the inside. The greater the compressive stress, the longer it takes for the fragments to break, and the better the anti-drop effect. To improve the falling ball impact resistance of the glass cover, the following aspects can be used: 1. The fracture toughness of the glass can be improved, and the raw material components of the glass and the skeleton structure of the glass can be changed. For example, SiO2, Al2O3, GeO2, V2O5, P2O5 and B2O3; because the above oxides are ionic compounds, composed of ionic bonds, each ionic bond has a corresponding bond energy, bond length and bond angle. The stronger the bond energy, the shorter the bond length, and the smaller the bond angle, the greater the strength of the hard object piercing and tearing resistance; 2. The internal structure is changed by some oxides (Na2O, Li2O and K2O, etc.) to change the network structure. For example, the accumulation of lithium ions with small diameters in lithium oxide reacts with sodium ions with larger diameters during the chemical replacement process, and the ion distribution is more dense, and the compressive stress is increased; 3. The smaller the microcracks on the surface of the product, the greater the energy required for the falling ball impact to tear it open.
[0005] Since the fracture toughness depends on the component design of the raw material itself and cannot be changed, it is necessary to make further improvements in the microcrack width, deep compressive stress (multi-directional diffusion delay) and compressive stress uniformity at the same depth (lateral diffusion delay) to slow down the deep stress slope curve. Summary of the invention
[0006] In order to overcome the shortcomings and deficiencies in the prior art, the object of the present invention is to provide a production process for improving the anti-drop performance of lithium aluminosilicate glass.
[0007] The object of the present invention is achieved by the following technical solution: A production process for improving the anti-drop performance of lithium aluminosilicate glass, comprising the following steps:
[0008] (1) Primary strengthening: preheat the lithium aluminosilicate glass at 300-320°C for 10-20 min, then place it in a mixed molten salt of sodium nitrate and potassium nitrate at 385-410°C for strengthening for 5-7 h, drip the strengthened glass with salt for 4-6 min, and then transfer it to room temperature for cooling;
[0009] (2) Secondary strengthening: preheat the lithium aluminum silicate glass at 300-320°C for 10-20 minutes, then place it in a molten salt of potassium nitrate and strengthen it at 380-390°C for 60-90 minutes. After dripping salt on the strengthened glass for 4-6 minutes, transfer it to room temperature for cooling, and obtain lithium aluminum silicate glass with excellent anti-drop performance.
[0010] Preferably, in the step (1), the preheating temperature is 310°C and the time is 15 minutes. When the preheating temperature of the lithium aluminosilicate glass is too high, the ionic bonds formed by the bridging oxygen bonds inside will become loose, and the internal ion distribution will be relocated, and the sodium-lithium replacement will be uneven, which will lead to unstable compressive stress. The present invention can improve the problems of internal ion displacement, poor distribution uniformity, uneven distribution of large sodium ions and potassium ions at different positions, uneven compressive stress, uneven force diffusion and poor anti-fading performance caused by high preheating temperature and long time by adopting low temperature and short time preheating.
[0011] Preferably, in step (1), the mass ratio of sodium nitrate to potassium nitrate is 85%-95%:5%-15%. More preferably, in step (1), the mass ratio of sodium nitrate to potassium nitrate is 90%:10%. By strictly controlling the mass ratio of sodium salt to potassium salt, the drop resistance of lithium aluminosilicate glass can be significantly improved.
[0012] Preferably, in step (1), the strengthening temperature is 400°C and the time is 6 hours. By adopting low-temperature and long-term salt bath strengthening, the replacement of Na ions and Li ions is evenly and stably promoted from the outside to the inside, the deep stress is deeper, and the sodium stress curve is flatter.
[0013] Preferably, in the step (2), the preheating temperature is 320°C and the time is 15 minutes. When the preheating temperature of the lithium aluminosilicate glass is too high, the ionic bonds formed by the bridging oxygen bonds inside will become loose, and the internal ion distribution will be relocated, and the sodium-lithium replacement will be uneven, which will lead to unstable compressive stress. The present invention can improve the problems of internal ion displacement, poor distribution uniformity, uneven distribution of large sodium ions and potassium ions at different positions, uneven compressive stress, uneven force diffusion and poor anti-fading performance caused by high preheating temperature and long time by adopting low temperature and short time preheating.
[0014] Preferably, in step (2), the strengthening temperature is 395°C and the time is 60 minutes. By adopting low-temperature and long-term salt bath strengthening, the replacement of Na ions and Li ions is evenly and stably promoted from the outside to the inside, the deep stress is deeper, and the sodium stress curve is flatter.
[0015] Another object of the present invention is achieved through the following technical solution: a lithium aluminosilicate glass with excellent anti-drop performance, wherein the lithium aluminosilicate glass is produced according to the production process described above.
[0016] The beneficial effects of the present invention are as follows: the production process of the present invention can improve the problems of internal ion displacement, poor distribution uniformity, uneven distribution of large sodium ions and potassium ions at different positions, uneven compressive stress, uneven force diffusion and poor anti-fading performance caused by high preheating temperature and long preheating time by adopting low-temperature short-time preheating; by adopting low-temperature long-time salt bath strengthening, the replacement of Na ions and Li ions is promoted uniformly and stably from the outside to the inside, the deep stress is deeper, and the sodium stress curve is flatter, and the problem of uneven compressive stress caused by a series of ionic bonds and covalent bonds such as SI-O bonds in the product during high-temperature salt bath tempering due to different bond energies, different bond lengths, disordered opening of internal structure replacement channels, and disordered ion replacement can be avoided, thereby improving the anti-drop performance of lithium aluminum silicon glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 3 is a relationship diagram between the surface compressive stress CS and the stress layer depth DOL of the lithium aluminosilicate glass of the present invention, wherein curve A is the lithium aluminosilicate glass prepared in Example 2, curve B is the lithium aluminosilicate glass prepared in Comparative Example 1, the X-axis curve is the sodium stress curve, and the Y-axis oblique line is the potassium stress curve. DETAILED DESCRIPTION
[0018] In order to facilitate the understanding of those skilled in the art, the following embodiments and attached Figure 1 The present invention is further described, and the contents mentioned in the implementation modes are not intended to limit the present invention.
[0019] Example 1
[0020] A production process for improving the drop resistance of lithium aluminosilicate glass comprises the following steps:
[0021] (1) Primary strengthening: preheat the lithium aluminosilicate glass at 300°C for 10 min, then place it in a mixed molten salt of sodium nitrate and potassium nitrate at 385°C for 5 h, drip the strengthened glass with salt for 4 min, and then transfer it to room temperature for cooling;
[0022] (2) Secondary strengthening: The lithium aluminosilicate glass is preheated at 300°C for 10 minutes, then placed in a molten salt of potassium nitrate and strengthened at 380°C for 60 minutes. The strengthened glass is dripped with salt for 4 minutes and then transferred to room temperature for cooling to obtain lithium aluminosilicate glass with excellent drop resistance.
[0023] A lithium aluminosilicate glass with excellent anti-drop performance, wherein the lithium aluminosilicate glass is produced according to the above-mentioned production process.
[0024] Example 2
[0025] A production process for improving the drop resistance of lithium aluminosilicate glass comprises the following steps:
[0026] (1) Primary strengthening: preheat the lithium aluminosilicate glass at 310°C for 15 min, then place it in a mixed molten salt of sodium nitrate and potassium nitrate at 400°C for strengthening for 6 h, drip salt on the strengthened glass for 5 min, and then transfer it to room temperature for cooling;
[0027] (2) Secondary strengthening: The lithium aluminosilicate glass is preheated at 310°C for 15 minutes, and then placed in a molten salt of potassium nitrate and strengthened at 385°C for 75 minutes. The strengthened glass is dripped with salt for 5 minutes and then transferred to room temperature for cooling to obtain lithium aluminosilicate glass with excellent drop resistance.
[0028] A lithium aluminosilicate glass with excellent anti-drop performance, wherein the lithium aluminosilicate glass is produced according to the above-mentioned production process.
[0029] Example 3
[0030] A production process for improving the drop resistance of lithium aluminosilicate glass comprises the following steps:
[0031] (1) Primary strengthening: preheat the lithium aluminosilicate glass at 320°C for 20 min, then place it in a mixed molten salt of sodium nitrate and potassium nitrate at 410°C for 7 h, drip the strengthened glass with salt for 6 min, and then transfer it to room temperature for cooling;
[0032] (2) Secondary strengthening: The lithium aluminosilicate glass is preheated at 320°C for 20 minutes, then placed in a molten salt of potassium nitrate and strengthened at 390°C for 90 minutes. The strengthened glass is dripped with salt for 6 minutes and then transferred to room temperature for cooling to obtain lithium aluminosilicate glass with excellent drop resistance.
[0033] A lithium aluminosilicate glass with excellent anti-drop performance, wherein the lithium aluminosilicate glass is produced according to the production process described above.
[0034] Comparative Example 1
[0035] The difference between this comparative example and Example 2 is that the preheating temperature of the primary and secondary strengthening is 350°C, and the time is 15 minutes; the temperature of the primary strengthening is 410°C, and the time is 2 hours; the temperature of the secondary strengthening is 390°C, and the time is 50 minutes.
[0036] Comparative Example 2
[0037] The difference between this comparative example and Example 2 is that the preheating temperature of the primary strengthening and the secondary strengthening is 350° C. and the time is 15 minutes.
[0038] Comparative Example 3
[0039] The difference between this comparative example and Example 2 is that the temperature of the first strengthening is 410° C. and the time is 2 h, and the temperature of the second strengthening is 390° C. and the time is 50 min.
[0040] The lithium aluminum silicate glass produced by the production process of Examples 1-3 of the present invention and Comparative Examples 1-3 was tested for its anti-drop performance. The test conditions are as follows: the strengthened 0.7mm thick 2.5D lithium aluminum silicate glass (the raw material is Asahi Glass AGC-DTSTAR-PLUS white glass sheet) is glued to a 180g counterweight block with a 0.8mm thick backing adhesive, and dropped from 30cm in a directional manner, and the height is increased every 10cm. Ten pieces are tested at each height, and the lowest crack height is recorded. The test results are shown in the following table.
[0041] Test items Preheat One-time reinforcement Secondary reinforcement Minimum rupture height / cm Example 1 300℃,10min 385℃,5h 380℃,60min 120cm Example 2 310℃,15min 400℃,6h 385℃,75min 130cm Example 3 320℃,20min 410℃,7h 390℃,90min 120cm Comparative Example 1 350℃,15min 410℃,2h 390℃,50min 60cm Comparative Example 2 350℃,15min 400℃,6h 385℃,75min 90cm Comparative Example 3 310℃,15min 410℃,2h 390℃,50min 80cm
[0042] It can be seen from the above table that the production process of the present invention can improve the anti-drop performance of the lithium aluminum silicate glass by more than 100% through low-temperature short-time preheating and low-temperature long-time salt bath strengthening.
[0043] The relationship between the surface compressive stress CS and the stress layer depth DOL of the lithium aluminosilicate glass prepared in Example 2 of the present invention and Comparative Example 1 is shown in the figure below: Figure 1 As shown, the curves are curve A and curve B respectively. It can be seen that the production process of the present invention is strengthened by low-temperature short-time preheating and low-temperature long-time salt bath. The corresponding curve A is flatter than curve B, the deeper the sodium stress depth, and the stronger the sodium stress at the same depth position, so that the lithium aluminum silicon glass has excellent anti-drop performance.
[0044] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. A production process for improving the drop resistance of lithium aluminosilicate glass, characterized in that: The steps include: (1) Primary strengthening: preheat the lithium aluminosilicate glass at 300-320°C for 10-20 min, then place it in a mixed molten salt of sodium nitrate and potassium nitrate at 385-410°C for strengthening for 5-7 h, drip the strengthened glass with salt for 4-6 min, and then transfer it to room temperature for cooling; (2) Secondary strengthening: preheat the lithium aluminum silicate glass at 300-320°C for 10-20 minutes, then place it in a molten salt of potassium nitrate and strengthen it at 380-390°C for 60-90 minutes. After dripping salt on the strengthened glass for 4-6 minutes, transfer it to room temperature for cooling, and obtain lithium aluminum silicate glass with excellent anti-drop performance.
2. A production process for improving the anti-drop performance of lithium aluminosilicate glass according to claim 1, characterized in that: In the step (1), the preheating temperature is 310° C. and the time is 15 minutes.
3. The production process for improving the anti-drop performance of lithium aluminosilicate glass according to claim 1, characterized in that: In the step (1), the mass ratio of sodium nitrate to potassium nitrate is 85%-95%:5%-15%.
4. The production process for improving the anti-drop performance of lithium aluminosilicate glass according to claim 1, characterized in that: In the step (1), the mass ratio of sodium nitrate to potassium nitrate is 90%:10%.
5. The production process for improving the anti-drop performance of lithium aluminosilicate glass according to claim 1, characterized in that: In the step (1), the strengthening temperature is 400° C. and the time is 6 hours.
6. The production process for improving the anti-drop performance of lithium aluminosilicate glass according to claim 1, characterized in that: In the step (2), the preheating temperature is 320° C. and the time is 15 minutes.
7. The production process for improving the drop resistance of lithium aluminosilicate glass according to claim 1, characterized in that: In the step (2), the strengthening temperature is 395° C. and the time is 60 minutes.
8. A lithium aluminosilicate glass with excellent drop resistance, characterized in that: The lithium aluminosilicate glass is produced according to the production process described in any one of claims 1-7.
Citation Information
Patent Citations
Novel strengthening process for lithium-aluminum-silicon glass
CN113387598A
Chemical strengthening method for anti-breaking lithium aluminum silicon glass
CN114292034A
Chemical strengthening method, chemically strengthened glass, glass-containing product and preparation method and application thereof
CN116023044A
Tempered glass having high compressive stress and high safety, and processing method therefor
WO2022037334A1
Lithium aluminosilicate glass, tempered glass, preparation method therefor and electronic product
WO2022141273A1