Sludge unfired ceramsite as well as preparation method and application thereof

Through the combination of three-layer sandwich core-shell structure and waterproof coating, the problems of high water absorption, low strength and high preparation cost of traditional ceramics are solved, and the lightweight and high strength of sludge-free ceramics are achieved, which improves the lightweight and high strength of sludge-free ceramics. The overall performance and environmental protection of the ceramic granules.

CN119019106APending Publication Date: 2024-11-26SHANTOU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411158218.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional ceramic pellets have the disadvantages of large water absorption, low strength, and large stacking density. They have high preparation costs, and the high-temperature sintering process consumes energy and emits harmful gases, which is not conducive to the environment. The existing sludge-free ceramic pellets have limited load capacity and utilization There are problems such as low rate, high production cost, high stacking density and water absorption.

Method used

The sludge-free pottery grains with three layers of sandwich core-shell structure are composed of sludge, biochar, cement, silicon fume, fly ash, water glass, gypsum and rubber powder. The middle layer is cement and the outer shell layer is Sludge, cement, silicon fume, fly ash and water glass, and the shell layer is covered with waterproof coating. By selecting raw materials and compound design, the cost is reduced, and the lightweight, low water absorption and high ceramide are improved. Barrel pressure strength.

Benefits of technology

The lightweight, low water absorption rate and high barrel pressure strength of the ceramic granules are achieved, which reduces the raw material cost and improves the overall performance of the ceramic granules. The water absorption rate can be as low as 2.54-3.08%, and the barrel pressure strength reaches 11.68-12.46MPa. The bulk density is 845.1-886.4kg/m3, which extends the service life and improves environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019106A_ABST
    Figure CN119019106A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of building materials, and particularly discloses sludge unfired ceramsite and a preparation method and application thereof.The sludge unfired ceramsite is of a three-layer sandwich core-shell structure, an inner core layer is prepared from sludge, biochar, cement, silica fume, fly ash, water glass, gypsum, rubber powder and glass beads, a middle layer is cement slurry, and the inner core layer is made of water; the shell layer is prepared from the following raw material components: sludge, cement, silica fume, fly ash, water glass and gypsum. According to the invention, sludge and cement are used as main raw materials, and a certain amount of water glass, gypsum, glass beads and solid waste silica fume and fly ash are used as auxiliary materials; the unfired ceramic particles are prepared by fully utilizing the sludge, the fly ash and the rubber powder as well as the specific biochar and the rubber powder, optimizing and reasonably compounding the raw materials and constructing a three-layer sandwich core-shell structure, and the light weight, low water absorption and high barrel pressure strength of the ceramsite are realized on the premise of ensuring high sludge utilization rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to sludge unburned ceramsite and a preparation method and application thereof. Background Art

[0002] As a new type of building material, traditional ceramsite mainly includes eight categories: bauxite ceramsite sand, clay ceramsite, shale ceramsite, garbage ceramsite, coal gangue ceramsite, biological sludge ceramsite, riverbed mud ceramsite and fly ash ceramsite. However, most traditional ceramsites have the disadvantages of high water absorption, low strength and high bulk density.

[0003] At present, the preparation cost of building ceramsite is relatively high, mainly because the preparation process requires a large amount of cementitious materials, special admixtures and high-temperature sintering steps, which increase the cost of producing ceramsite to a certain extent. The high cost limits the application of ceramsite in some low-budget projects, and a balance needs to be struck between economic benefits and performance. At the same time, most of the ceramsite on the market is mainly sintered ceramsite, which will emit many harmful gases during the high-temperature calcination process and consume a lot of energy, which is not conducive to ecological environmental protection. At present, the raw materials for the production of ceramsite in my country are mainly natural resources such as clay and shale, while the utilization of solid waste is relatively less studied. With the reduction of natural resource stocks, the environmental resource pressure in the production process is increasing. Although relevant policies stipulate that the raw materials used by enterprises should be mixed with no less than 30% of fly ash, coal gangue, slag, sludge and other types of waste residues, the overall utilization rate is still low, most of which are only around 40%-60%. Among them: fly ash ceramsite mainly adopts roasting process, although it has the advantages of mature technology and high product strength, but it has the disadvantages of high energy consumption, large investment and complex process. Gangue ceramsite has strong adsorption capacity to water due to the existence of pores and is easy to absorb moisture; sludge ceramsite is relatively loose in composition, has low compressive strength, and is easy to deform, so its use in certain structures is limited.

[0004] With the development of national infrastructure construction and river sludge cleaning, a large amount of construction waste and river sludge have accumulated, forming sludge with complex components. Compared with landfill treatment, preparing sludge into expanded clay is more economical and environmentally friendly. At present, the unburned expanded clay prepared from common sludge has the disadvantages of limited load-bearing capacity, low utilization rate, high production cost, high bulk density and water absorption rate, and it is difficult to meet the performance requirements of high-strength and high-durability building materials. At the same time, most of the unburned expanded clay prepared with sludge as raw material uses foaming agents to reduce the bulk density, but the effect is not good and the process is complicated, resulting in a generally high bulk density of more than 1000kg / m 3 , and the barrel pressure strength is low. In addition, there are many pores on the surface of unburned ceramsite, which has high hydrophilicity. However, the surface of unburned ceramsite prepared with sludge is easy to soften, resulting in the influence of water absorption rate and strength.

[0005] Therefore, there is an urgent need to develop an unfired expanded clay prepared with sludge as the main raw material, which can simultaneously have the characteristics of light weight, low water absorption and high barrel pressure strength. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a sludge unburned ceramsite and a preparation method and application thereof, wherein the unburned ceramsite utilizes solid waste sludge, silica ash, fly ash and rubber powder, and can simultaneously achieve light weight, low water absorption rate and high barrel pressure strength.

[0007] In order to solve the above technical problems, the first aspect of the present invention provides a sludge unburned ceramsite, which has a three-layer sandwich core-shell structure, wherein: the raw material components of the inner core layer include sludge, biochar, cement, silica fume, fly ash, water glass, gypsum, rubber powder and glass beads, the middle layer is cement, and the raw material components of the outer shell layer include sludge, cement, silica fume, fly ash, water glass and gypsum.

[0008] Specifically, the present invention uses sludge and cement as main raw materials, and is mixed with a certain amount of water glass, gypsum, glass beads and solid waste silica fume, fly ash; as well as specific biochar and rubber powder. By optimizing and reasonably compounding the raw materials and designing a three-layer sandwich core-shell structure, unfired ceramsite is prepared. While greatly reducing the cost of raw materials, the quality of the product is effectively guaranteed, and the lightweight, low water absorption and high barrel pressure strength of the ceramsite are achieved.

[0009] Among them: the inner core layer is mainly prepared with sludge, biochar, cement, silica fume, fly ash, water glass, gypsum, rubber powder and glass beads as raw materials. On the one hand, biochar is used to modify the sludge, which can not only significantly improve the dewatering performance of the sludge, but also adsorb heavy metal ions in the sludge, improve the stability of the sludge, and reduce its influence on the strength of building materials; on the other hand, the light weight of biochar, rubber powder, glass beads and silica fume is used to reduce the weight of ceramsite. The cement interlayer serves as an intermediate bridge to tightly bond the inner core layer and the outer shell together. While enhancing the overall strength and stability of the ceramsite, it helps to prevent the ceramsite from breaking and damaging during use, prolonging its service life and improving the wear resistance and impact resistance of the ceramsite. The outer shell of the unfired ceramsite is prepared with cement, silica fume, fly ash, water glass, gypsum and other cementitious materials. It is different from the raw material components of the inner core layer, reducing the lightweight rubber powder, biochar and glass beads, and using the high bonding property of the cementitious materials to provide a higher strength skeleton, thereby further improving the barrel pressure strength of the ceramsite. Therefore, the three-layer sandwich core-shell structure design of the present invention can effectively improve the overall performance of ceramsite.

[0010] As a further improvement of the above solution, the surface of the outer shell layer is coated with a waterproof layer, and the waterproof layer is formed by curing a waterproof coating.

[0011] Specifically, the waterproof coating, as a protective film, not only fills the tiny pores on the surface of the ceramsite, reduces the water absorption rate of the ceramsite, but also helps to improve the mechanical properties and stability of the ceramic. At the same time, the waterproof coating helps to improve the softening and waterproof properties of the ceramsite and improve its waterproof effect.

[0012] Preferably, the waterproof coating comprises organosilicon-modified polyurethane resin, organofluorine coating, organosilicon coating and epoxy resin. Compared with other waterproof coatings, the composite use of these coatings not only has excellent waterproof performance but also has strong adhesion to expanded clay.

[0013] Preferably, the mass ratio of the organosilicon-modified polyurethane resin, the organofluorine coating, the organosilicon coating and the epoxy resin is (3-5): (2-4): (1-3): 1

[0014] Preferably, the biochar is straw biochar.

[0015] As a further improvement of the above scheme, the raw material components of the inner core layer include, by weight: 50-70 parts of sludge, 2-4 parts of biochar, 15-30 parts of cement, 1-3 parts of silica fume, 3-10 parts of fly ash, 1-6 parts of water glass, 1-5 parts of gypsum, 2-6 parts of rubber powder, and 1-4 parts of glass beads.

[0016] As a further improvement of the above scheme, the raw material components of the outer shell layer include, by weight: 30-50 parts of sludge, 30-50 parts of cement, 1-3 parts of silica fume, 5-15 parts of fly ash, 3-7 parts of water glass, and 1-5 parts of gypsum.

[0017] As a further improvement of the above scheme, the cement slurry includes 40-60 parts of cement, 5-15 parts of water, and 0.05-0.15 parts of polycarboxylic acid water reducer by weight. Polycarboxylic acid has a high efficiency water reducer, which can effectively reduce the amount of cement water and improve the bonding strength of the transition layer.

[0018] As a further improvement of the above solution, the diameter of the inner core layer is 2-4 mm.

[0019] As a further improvement of the above solution, the thickness of the intermediate layer is 0.5-1 mm.

[0020] As a further improvement of the above solution, the diameter of the ceramsite is 6-10 mm.

[0021] The second aspect of the present invention provides a method for preparing the above-mentioned sludge unburned ceramsite, comprising the following steps:

[0022] (1) Mixing the sludge with biochar, and then adding cement, silica fume, fly ash, water glass, gypsum, rubber powder and glass beads to granulate and form an inner core layer;

[0023] (2) placing the inner core layer formed in step (1) in cement slurry, taking it out, and forming an intermediate layer;

[0024] (3) Mixing the raw materials for preparing the outer shell layer, adding the ceramsite coated with the middle layer in step (2), and granulating the ceramsite so that the surface of the ceramsite is coated with the raw materials of the outer shell layer, and curing to obtain the sludge unburned ceramsite.

[0025] Preferably, in step (3), the curing is natural curing at room temperature for 25-30 days.

[0026] As a further improvement of the above scheme, the preparation method also includes the steps of coating a waterproof coating on the surface of the cured ceramsite and curing it.

[0027] Preferably, the curing condition is natural drying at room temperature.

[0028] A third aspect of the present invention provides a building material, which includes the above-mentioned sludge unburned ceramsite.

[0029] Compared with the prior art, the above technical solution of the present invention has at least the following technical effects or advantages:

[0030] (1) The present invention uses sludge and cement as main raw materials, and is mixed with a certain amount of water glass, gypsum, glass beads and solid waste silica fume, fly ash; as well as specific biochar and rubber powder, to make full use of solid waste sludge, fly ash and rubber powder, and prepares unfired ceramic particles by optimizing and reasonably compounding the raw materials and constructing a three-layer sandwich core-shell structure. Under the premise of ensuring a high sludge utilization rate, the lightweight, low water absorption and high barrel pressure strength of the ceramsite are achieved.

[0031] (2) The inner core layer of the present invention utilizes biochar to modify the sludge to improve the dewatering performance of the sludge and adsorb heavy metals, thereby improving the stability of the sludge; and a certain amount of light biochar, rubber powder, glass beads and silica fume are added to the inner core layer to reduce the weight of the ceramsite. At the same time, the inner core layer and the outer shell layer are tightly bonded by the cement interlayer to improve the overall strength and stability of the ceramsite. The outer shell layer uses a raw material component different from that in the inner core layer, and utilizes the high bonding property of the cementitious material to provide a high-strength skeleton, thereby further improving the mechanical properties of the ceramsite. Therefore, the three-layer sandwich core-shell structure design of the present invention with specific raw material components effectively improves the overall performance of the ceramsite, achieving a water absorption rate of the ceramsite as low as 2.54-3.08%, a barrel pressure strength of 11.68-12.46MPa, and a bulk density of 845.1-886.4kg / m 3 . BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The present invention is a process flow chart for preparing unfired ceramsite. DETAILED DESCRIPTION

[0033] The present invention is described in detail below in conjunction with the examples, so that the technical personnel of the relevant technical field can understand the present invention. It is necessary to point out here that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. The non-essential improvements and adjustments made to the present invention by the skilled person in the relevant field according to the above invention content should still belong to the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods that are not mentioned in detail are all process steps or preparation methods known to those skilled in the art.

[0034] The manufacturers and models of the waterproof coatings and water reducing agents used in the following examples and comparative examples are as follows:

[0035] Silicone-modified polyurethane resin: Dolphin-1089R3 water-based silicone-modified polyurethane resin produced by Sansheng Chemical;

[0036] Organic fluorine coating: FC2200 fluorocarbon topcoat produced by Shuangshi Company;

[0037] Silicone coating: 231030 silicone high temperature resistant paint produced by Hanbot Company;

[0038] Epoxy resin: ST-0011 epoxy resin produced by Hebei Zhongxin Anticorrosion Materials Co., Ltd.;

[0039] Polycarboxylate water reducer: Polycarboxylate water reducer produced by Guangdong Shantou Huiqiang Admixture Co., Ltd., with a mother liquor solid content of 40%.

[0040] Example 1

[0041] A sludge unburned ceramsite, which has a three-layer sandwich core-shell structure, wherein: the raw material components of the inner core layer include, by weight, 59 parts of sludge, 3 parts of straw biochar, 20 parts of cement, 2 parts of silica fume, 5 parts of fly ash, 2 parts of water glass, 2 parts of gypsum, 3 parts of rubber powder, and 2 parts of glass microbeads; the cement slurry of the middle layer includes, by weight, 50 parts of cement, 10 parts of water and 0.1 parts of polycarboxylic acid water reducer; the raw material components of the outer shell layer include, by weight, 44 parts of sludge, 44 parts of cement, 2 parts of silica fume, 5 parts of fly ash, 2 parts of water glass, and 3 parts of gypsum; and the outer shell layer is coated with a waterproof layer formed by curing a waterproof coating, and the waterproof coating includes, by weight, 4 parts of organosilicon-modified polyurethane resin, 3 parts of organofluorine coating, 2 parts of organosilicon coating, and 1 part of epoxy resin.

[0042] A method for preparing sludge unburned ceramsite, the process flow is as follows Figure 1 As shown, the following steps are included:

[0043] (1) drying the sludge after impurity removal at 105°C, crushing it with a wall-breaking machine, sieving it, and then mixing it evenly with straw biochar to obtain modified sludge; then adding cement, silica fume, fly ash, water glass, gypsum, rubber powder, and glass beads according to the mass ratio, mixing evenly, and obtaining the inner core layer raw material; then pouring it into the rotating basin of the granulator, adjusting the angle and speed of the granulator, starting the turntable, spraying water to granulate it, rolling it into spherical ceramsite of 2-4 mm, sieving it, and obtaining the inner core layer;

[0044] (2) slowly placing the inner core layer prepared in step (1) into the cement slurry using a colander, and scooping it out to form a cement middle layer with a thickness of 0.5-1 mm;

[0045] (3) Weighing the raw materials for preparing the outer shell layer according to the mass ratio, mixing them evenly, adding the ceramsite for wrapping the middle layer prepared in step (2), pouring them into the rotating bowl of the granulator, adjusting the angle and speed of the granulator, starting the turntable, and granulating, so that the raw materials for the outer shell layer on the surface of the ceramsite are wrapped, rolling them into spherical ceramsite with a diameter of 6-10 mm, sieving them, and forming the outer shell layer; aging them indoors for 2 hours, and then transferring them to a room temperature curing box for natural curing for 28 days;

[0046] (4) spraying the waterproof coating on the surface of the ceramsite prepared in step (3) and letting it dry naturally to obtain the sludge unburned ceramsite of this embodiment.

[0047] Example 2

[0048] A sludge unburned ceramsite, which has a three-layer sandwich core-shell structure, wherein: the raw material components of the inner core layer include, by weight, 54 parts of sludge, 3 parts of straw biochar, 21 parts of cement, 3 parts of silica fume, 8 parts of fly ash, 4 parts of water glass, 2 parts of gypsum, 4 parts of rubber powder, and 1 part of glass microbeads; the cement slurry of the middle layer includes, by weight, 50 parts of cement, 10 parts of water and 0.1 parts of polycarboxylic acid water reducer; the raw material components of the outer shell layer include, by weight, 41 parts of sludge, 41 parts of cement, 2 parts of silica fume, 10 parts of fly ash, 3 parts of water glass, and 3 parts of gypsum; and the outer shell layer is coated with a waterproof layer formed by curing a waterproof coating, and the waterproof coating includes, by weight, 4 parts of organosilicon-modified polyurethane resin, 3 parts of organofluorine coating, 2 parts of organosilicon coating, and 1 part of epoxy resin.

[0049] The preparation method of the sludge unburned ceramsite in Example 2 is the same as that in Example 1.

[0050] Example 3

[0051] A sludge unburned ceramsite, which has a three-layer sandwich core-shell structure, wherein: the raw material components of the inner core layer include, by weight, 56 parts of sludge, 3 parts of straw biochar, 22 parts of cement, 2 parts of silica fume, 6 parts of fly ash, 3 parts of water glass, 2 parts of gypsum, 4 parts of rubber powder, and 2 parts of glass microbeads; the cement slurry of the middle layer includes, by weight, 50 parts of cement, 10 parts of water and 0.1 parts of polycarboxylic acid water reducer; the raw material components of the outer shell layer include, by weight, 43 parts of sludge, 43 parts of cement, 2 parts of silica fume, 7 parts of fly ash, 3 parts of water glass, and 2 parts of gypsum; and the outer shell layer is coated with a waterproof layer formed by curing a waterproof coating, and the waterproof coating includes, by weight, 4 parts of organosilicon-modified polyurethane resin, 3 parts of organofluorine coating, 2 parts of organosilicon coating, and 1 part of epoxy resin.

[0052] The preparation method of the sludge unburned ceramsite in Example 3 is the same as that in Example 1.

[0053] Comparative Example 1

[0054] The only difference between Comparative Example 1 and Example 1 is that the structure of the sludge unburned expanded clay is different. The sludge unburned expanded clay in Comparative Example 1 does not contain an intermediate layer and an outer shell layer, and is prepared only from the raw materials of the inner core layer, and the same waterproof coating as that in Example 1 is sprayed on its surface.

[0055] Comparative Example 2

[0056] The only difference between Comparative Example 2 and Example 1 is that the structure of the sludge unburned expanded clay is different. The sludge unburned expanded clay in Comparative Example 2 has a double-layer core-shell structure, does not contain a cement intermediate layer, and the same waterproof coating as in Example 1 is sprayed on its surface.

[0057] Comparative Example 3

[0058] The only difference between Comparative Example 3 and Example 1 is that the structure of the sludge unburned expanded clay is different. The sludge unburned expanded clay of Comparative Example 3 does not contain an inner core layer and an intermediate layer, and is prepared only from the raw materials of the outer shell layer, and the same waterproof coating as that of Example 1 is sprayed on its surface.

[0059] Comparative Example 4

[0060] The difference between Comparative Example 4 and Example 1 is only that the structure of the sludge unburned ceramsite is different. The surface of the outer shell layer of the sludge unburned ceramsite in Comparative Example 4 is not sprayed with waterproof coating, that is, it does not contain a waterproof layer.

[0061] Comparative Example 5

[0062] The only difference between Comparative Example 5 and Example 1 is that the raw material components of the inner core layer of the sludge-free expanded clay are different. The raw material components of the inner core layer of Comparative Example 1 do not include straw biochar, and include, by weight: 59 parts of sludge, 20 parts of cement, 2 parts of silica fume, 5 parts of fly ash, 2 parts of water glass, 2 parts of gypsum, 6 parts of rubber powder, and 2 parts of glass beads.

[0063] Comparative Example 6

[0064] The only difference between Comparative Example 6 and Example 1 is that the raw material components of the inner core layer of the sludge-free expanded clay are different. The raw material components of the inner core layer of Comparative Example 6 do not include straw biochar, and include, by weight: 59 parts of sludge, 3 parts of ammonium bicarbonate, 20 parts of cement, 2 parts of silica fume, 5 parts of fly ash, 2 parts of water glass, 2 parts of gypsum, 3 parts of rubber powder, and 2 parts of glass beads.

[0065] Performance Testing

[0066] The bulk density, barrel pressure strength and 1-hour water absorption rate of the ceramsite samples prepared in each embodiment and comparative example were measured with reference to the national standard GBT17431.2-2010 "Light aggregate and its test method Part 2: Light aggregate test method", and the results are shown in Table 1.

[0067] Table 1:

[0068]

[0069]

[0070] As shown in Table 1, the embodiment utilizes the technology of straw biochar modified sludge and three-layer sandwich core-shell structure to stimulate the bonding performance of straw biochar, cement, water glass, silica fume and fly ash in ceramsite, so that the stacking density of embodiment 1, embodiment 2 and embodiment 3 is similar to that of the comparative example, and the barrel pressure strength of the embodiment is higher than that of the comparative example, which shows that the embodiment has higher compressive strength when subjected to external pressure, and at the same time, with better structural strength, more waste materials can be mixed in the same volume to improve environmental protection. Secondly, the water absorption rate of the embodiment is much lower than the water absorption rate of 12.81% in comparative example 4 without a waterproof layer. The low water absorption rate shows that the waterproof coating sprayed on the surface of ceramsite has good waterproof performance, which can effectively reduce the damage of water penetration to the material structure, extend the service life of the material, and reduce maintenance costs.

[0071] For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, without having to go through creative labor. Therefore, simple improvements made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the protection scope of the present invention. The above embodiments are preferred embodiments of the present invention, and all processes similar to the present invention and equivalent changes made should belong to the protection scope of the present invention.

Claims

1. A sludge unburned ceramsite, characterized in that: The sludge unburned ceramsite has a three-layer sandwich core-shell structure, wherein the raw material components of the inner core layer include sludge, biochar, cement, silica fume, fly ash, water glass, gypsum, rubber powder and glass beads, the middle layer is cement slurry, and the raw material components of the outer shell layer include sludge, cement, silica fume, fly ash, water glass and gypsum.

2. The sludge unburned ceramsite according to claim 1, characterized in that: The surface of the outer shell layer is covered with a waterproof layer, and the waterproof layer is formed by curing waterproof coating.

3. The sludge unburned ceramsite according to claim 1, characterized in that: The biochar is straw biochar.

4. The sludge unburned ceramsite according to claim 1, characterized in that: The raw material components of the inner core layer include, by weight: 50-70 parts of sludge, 2-4 parts of biochar, 15-30 parts of cement, 1-3 parts of silica fume, 3-10 parts of fly ash, 1-6 parts of water glass, 1-5 parts of gypsum, 2-6 parts of rubber powder, and 1-4 parts of glass beads.

5. The sludge unburned ceramsite according to claim 1, characterized in that: The raw material components of the outer shell layer include, by weight: 30-50 parts of sludge, 30-50 parts of cement, 1-3 parts of silica fume, 5-15 parts of fly ash, 3-7 parts of water glass, and 1-5 parts of gypsum.

6. The sludge unburned ceramsite according to claim 1, characterized in that: The cement slurry comprises 40-60 parts of cement, 5-15 parts of water and 0.05-0.15 parts of polycarboxylate water reducer by weight.

7. The sludge unburned ceramsite according to any one of claims 1 to 6, characterized in that: The diameter of the inner core layer is 2-4 mm; and / or the diameter of the ceramsite is 6-10 mm.

8. A method for preparing sludge unburned ceramsite according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Mixing the sludge with biochar, and then adding cement, silica fume, fly ash, water glass, gypsum, rubber powder and glass beads to granulate and form an inner core layer; (2) placing the inner core layer formed in step (1) in cement slurry, taking it out, and forming an intermediate layer; (3) Mixing the raw materials for preparing the outer shell layer, adding the ceramsite coated with the middle layer in step (2), and granulating the ceramsite so that the surface of the ceramsite is coated with the raw materials of the outer shell layer, and curing to obtain the sludge unburned ceramsite.

9. The method for preparing sludge unburned ceramsite according to claim 8, characterized in that: The preparation method also includes the steps of coating a waterproof coating on the surface of the cured ceramsite and curing the coating.

10. A building material, characterized in that: The building material comprises the sludge unburned ceramsite according to any one of claims 1-7.

Citation Information

Cited By

  • Lightweight ceramsite as well as preparation method and application thereof

    CN120965364A