Super high-rise pump concrete and preparation method thereof
Through the cooperation of polyacrylamide, silica and ceramide, a special structure is formed, which solves the separation and water leakage problems of concrete pumping in super high-rise buildings, improves the viscosity and flowability of concrete, and achieves high strength and easy pumping The delivery effect is suitable for concrete pumping in super high-rise buildings.
Patent Information
- Application Number
- CN202411160308.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the construction of ultra-high-rise buildings, concrete pumping faces problems such as separation and water leakage, resulting in insufficient uniformity and stability. The existing high-performance concrete lacks pumpability and flowability, making it difficult to meet the needs of ultra-high-rise pumping.
The combination of polyacrylamide, silica and ceramide is used to form a special structure. Through the wrapping and adsorption of polyacrylamide, the viscosity and stability of concrete are improved, bubble generation is reduced, fluidity and strength are improved, and ultrasonic mixing is ensured. Silica is embedded in the ceramite to form nano-level agglomerates to improve the toughness of the concrete.
It effectively improves the segregation resistance, flowability and strength of pumped concrete, reduces the risk of pipeline blockage, is suitable for pumping operations in super high-rise buildings, and ensures the uniformity and stability of concrete.
Smart Images

Figure BDA0005006234010000071 
Figure BDA0005006234010000081 
Figure BDA0005006234010000091
Abstract
Description
Technical Field
[0001] The present application relates to the field of pumping concrete, and more specifically, to a super-high-rise pumping concrete and a preparation method thereof. Background Art
[0002] With the acceleration of urbanization and the continuous development of construction technology, super high-rise buildings are emerging around the world. The construction of super high-rise buildings not only reflects the economic strength and technological level of the city, but also puts forward higher requirements for building materials and construction technology. Among them, concrete is one of the most widely used materials in construction projects, and its performance and quality are directly related to the safety and durability of the building.
[0003] In the construction of super high-rise buildings, concrete pumping technology is one of the key links. Due to the height and structural characteristics of super high-rise buildings, concrete pumping faces many technical challenges. First, the height of super high-rise buildings leads to long pumping distances, and concrete is prone to segregation and bleeding during the pumping process, affecting the uniformity and stability of the concrete. Secondly, the structure of super high-rise buildings is complex, and high strength and durability requirements for concrete are high, and high-performance concrete is needed to meet the requirements. In addition, super high-rise pumped concrete also needs to have good pumpability and fluidity to ensure that the concrete can be smoothly pumped to the designated location.
[0004] Although existing high-performance concrete has high strength, it often has problems with pumpability and fluidity, making it difficult to meet the needs of super-high-rise pumping. Therefore, there is still room for improvement. Summary of the invention
[0005] In order to improve the strength of pumped concrete, the present application provides a super high-rise pumped concrete and a preparation method thereof.
[0006] In the first aspect, the present application provides a super high-rise pumping concrete, which adopts the following technical solution: A super high-rise pumping concrete comprises the following raw materials in parts by weight: 155-175 parts of cement, 140-160 parts of water, 1-10 parts of admixture, 1050-1200 parts of coarse aggregate, 700-800 parts of fine aggregate, 150-200 parts of mineral admixture, and 30-50 parts of mixture; The mixture includes ceramsite, polyacrylamide and silicon dioxide, and the weight ratio of ceramsite, polyacrylamide and silicon dioxide is 1:(0.05-0.2):(0.2-0.5).
[0007] By adopting the above technical solution, polyacrylamide, silicon dioxide and ceramsite are selected for combination. Specifically, silicon dioxide can be embedded in the holes in the ceramsite, and then polyacrylamide forms a gel in water, which wraps and adsorbs on silicon dioxide and ceramsite, and the combination of the three forms a special structure. This special structure is relatively stable because silicon dioxide is not easy to fall off the ceramsite due to the wrapping and adsorption of polyacrylamide. In addition, the wrapping of polyacrylamide also makes it difficult for lightweight ceramsite to float in concrete, reducing the generation of excess bubbles and ensuring the overall uniformity and stability of the concrete.
[0008] During the pumping process, the above special structure also plays a significant role. The polyacrylamide wrapped structure is used in pumped concrete, which can effectively increase the viscosity of pumped concrete and reduce the segregation phenomenon during pumping. It not only improves the pumping effect, but also reduces the risk of pipeline blockage, making it more suitable for super-high-rise pumping operations.
[0009] As the preparation and curing reaction of pumped concrete proceeds, due to the negative charge of polyacrylamide, the special structure of the outermost polyacrylamide will attract the positive charge in the concrete system, and the silicon dioxide it encapsulates will be more thoroughly exposed in the concrete system. The calcium ions in the cement paste can effectively promote the formation of aggregates of some silicon dioxide, which play a role similar to fibers inside the cement, thereby effectively improving the strength and toughness of the concrete.
[0010] In addition, the combination of expanded clay with silica and polyacrylamide in the mixture can effectively improve the problem that expanded clay easily absorbs water inside the concrete, effectively alleviates the impact on the fluidity of the concrete, and makes the pumped concrete have the properties of high ease, high resistance to segregation, and high strength.
[0011] Preferably, the weight ratio of the ceramsite, polyacrylamide and silicon dioxide is 1:(0.1-0.15):(0.35-0.45).
[0012] By adopting the above technical solution, the dosage relationship between expanded clay, polyacrylamide and silica is further limited, forming a special structure with more stable performance, which can better play a special effect in pumped concrete.
[0013] Preferably, the particle size of the ceramsite is 5-10 mm.
[0014] By adopting the above technical solution, the particle size of ceramsite is further limited. The ceramsite under this particle size has a better matching effect with silicon dioxide and polyacrylamide, which can effectively support the structure of pumped concrete and improve its strength. Moreover, ceramsite with appropriate particle size can be more evenly distributed in pumped concrete, which helps to reduce friction resistance, improve the fluidity of pumped concrete, and make it easier to transport through pipelines.
[0015] Preferably, the particle size of the silicon dioxide is 200-300 nm.
[0016] By adopting the above technical solution, the particle size of silica is further limited. Nano-scale silica is easier to embed into the expanded clay structure and has a larger specific surface area. The subsequent reaction with cement paste is easier to carry out, so that a fiber-like effect extends throughout the entire concrete system, effectively improving the performance of pumped concrete.
[0017] Preferably, the mineral admixture includes a mixture of one or more of fly ash, mineral powder and silicon powder.
[0018] Preferably, the mineral admixtures are fly ash, mineral powder and silica powder. Based on the weight of the super high-rise pumped concrete, the fly ash is 60-80 parts, the mineral powder is 80-90 parts, and the silica powder is 10-30 parts.
[0019] By adopting the above technical solution and selecting specific types of mineral admixtures, cement and fine aggregate can be effectively saved, the amount of cement in concrete can be reduced, the pores between cement particles can be filled, the density of subsequently formed concrete can be increased, and the working performance of pumped concrete can be improved.
[0020] In a second aspect, the present application provides a method for preparing super high-rise pumping concrete, which adopts the following technical scheme: A method for preparing super high-rise pumping concrete, comprising the following steps: Step 1: preparing an aqueous solution of the mixture: taking a portion of water and mixing it with ceramsite, polyacrylamide and silicon dioxide under ultrasonic conditions to obtain an aqueous solution of the mixture; Step 2: Mix cement, mineral admixture and remaining water until uniform to obtain a first mixture; Step 3: Mixing the first mixture with the aqueous solution of the mixture until uniform, to obtain a second mixture; Step 4: Mix the second mixture with the coarse aggregate and the fine aggregate until they are uniform to obtain the third mixture; Step 5: Mix the third mixture with the admixture until uniform to obtain the finished product.
[0021] Preferably, the specific steps of step 1 are as follows: Step 1a: Mix ceramsite, silicon dioxide and water, and ultrasonically mix for 10-20 minutes at an ultrasonic frequency of 30-35 kHz and an ultrasonic power of 200-250 W to obtain a primary mixture; Step 1b: Add polyacrylamide to the initial mixture and mix under ultrasonic conditions for 5-10 minutes to obtain an aqueous solution of the mixture.
[0022] By adopting the above technical solution, the feeding sequence and specific ultrasonic conditions when preparing the mixture are further limited, so that as much silicon dioxide as possible can be firmly embedded in the expanded clay structure, and then the polyacrylamide can more fully wrap the silicon dioxide and expanded clay, so that the special structure is stably formed, and the role of the special structure can be more fully exerted later.
[0023] In summary, this application has the following beneficial effects: 1. The present application prepares a mixture by combining polyacrylamide, silicon dioxide and ceramsite to form a special structure in which silicon dioxide is embedded in ceramsite and polyacrylamide is interspersed and wrapped, thereby alleviating the problem that ceramsite is easy to float in the pumping concrete system due to its light weight, so that the ceramsite can fully play the effect of improving the strength of the pumping concrete; and, the special structure also solves the problem that ceramsite is easy to excessively absorb water inside the pumping concrete system, thereby ensuring the good fluidity of the pumping concrete.
[0024] 2. The special structure of the present application is applied in pumped concrete to enhance the viscosity of the pumped concrete and improve the anti-segregation property of the pumped concrete.
[0025] 3. The special structure of the present application is that during the preparation and curing period of pumped concrete, part of the polyacrylamide cooperates with the concrete system to expose the coated silica. This part of the silica forms aggregates and plays a role similar to fiber inside the system, greatly improving the strength and toughness of the pumped concrete. DETAILED DESCRIPTION
[0026] The present application is further described in detail below with reference to the embodiments.
[0027] The raw materials used in the following examples and comparative examples are all commercially available products. Example
[0028] Example 1 A super high-rise pumping concrete comprises the following raw materials: cement, water, admixture, coarse aggregate, fine aggregate, mineral admixture and mixture.
[0029] The cement is P.042.5 silicate cement, the admixture is polycarboxylic acid water reducer (slow-setting type), the coarse aggregate is 5-25mm crushed stone, the fine aggregate is 0.5-0.35mm machine-made sand, and the mineral admixtures are fly ash, mineral powder and silica powder.
[0030] The mixture includes ceramsite, polyacrylamide and silicon dioxide, and the weight ratio of ceramsite, polyacrylamide and silicon dioxide is 1:0.1:0.4.
[0031] The particle size of ceramsite is 5-10 mm, and the particle size of silicon dioxide is 250 nm. Polyacrylamide is anionic, commercially available, and purchased from Henan Baiyuan Environmental Protection Technology Co., Ltd. in this embodiment.
[0032] The specific amount of each raw material is shown in Table 1.
[0033] The present application also provides a method for preparing super high-rise pumped concrete, comprising the following steps: Step 1: Prepare an aqueous solution of the mixture: Step 1a: Weigh water according to the weight ratio of ceramsite to water of 1:1, and this part of water is defined as water A.
[0034] The ceramsite, silicon dioxide and water A were ultrasonically mixed for 15 minutes at an ultrasonic frequency of 32 kHz and an ultrasonic power of 220 W to obtain a primary mixture.
[0035] Step 1b: Add polyacrylamide to the primary mixture, and mix for 8 minutes under ultrasonic conditions of maintaining an ultrasonic frequency of 32 kHz and an ultrasonic power of 220 W to obtain an aqueous solution of the mixture.
[0036] Step 2: Mix cement, mineral admixtures and remaining water (this part is defined as water B, the sum of water A and water B is 150, and the water recorded in Table 1 is also the sum), and stir until uniform to obtain the first mixture.
[0037] Step 3: Mix the first mixture with the mixture and stir until uniform to obtain a second mixture.
[0038] Step 4: Mix the second mixture with coarse aggregate and fine aggregate, and stir until uniform to obtain the third mixture.
[0039] Step 5: Mix the third mixture with the admixture, stir until uniform, and obtain the finished product.
[0040] Example 2 A super high-rise pumping concrete comprises the following raw materials: cement, water, admixture, coarse aggregate, fine aggregate, mineral admixture and mixture.
[0041] The cement is P.042.5 silicate cement, the admixture is polycarboxylic acid water reducer (slow-setting type), the coarse aggregate is 5-25mm crushed stone, the fine aggregate is 0.5-0.35mm machine-made sand, and the mineral admixtures are fly ash, mineral powder and silica powder.
[0042] The mixture includes ceramsite, polyacrylamide and silicon dioxide. The weight ratio of ceramsite, polyacrylamide and silicon dioxide is 1:0.05:0.2.
[0043] The particle size of ceramsite is 5-10 mm, and the particle size of silicon dioxide is 200 nm. Polyacrylamide is anionic, commercially available, and purchased from Henan Baiyuan Environmental Protection Technology Co., Ltd. in this embodiment.
[0044] The specific amount of each raw material is shown in Table 1.
[0045] The present application also provides a method for preparing super high-rise pumped concrete, comprising the following steps: Step 1: Prepare an aqueous solution of the mixture: Step 1a: Weigh water according to the weight ratio of ceramsite to water of 1:1, and this part of water is defined as water A.
[0046] The ceramsite, silicon dioxide and water A were ultrasonically mixed for 20 minutes at an ultrasonic frequency of 30 KHz and an ultrasonic power of 200 W to obtain a primary mixture.
[0047] Step 1b: Add polyacrylamide to the primary mixture, and mix for 10 minutes under ultrasonic conditions of maintaining an ultrasonic frequency of 30 KHz and an ultrasonic power of 200 W to obtain an aqueous solution of the mixture.
[0048] Step 2: Mix cement, mineral admixtures and remaining water (this part is defined as water B, the sum of water A and water B is 140, and the water recorded in Table 1 is also the sum) and stir until uniform to obtain the first mixture.
[0049] Step 3: Mix the first mixture with the mixture and stir until uniform to obtain a second mixture.
[0050] Step 4: Mix the second mixture with coarse aggregate and fine aggregate, and stir until uniform to obtain the third mixture.
[0051] Step 5: Mix the third mixture with the admixture, stir until uniform, and obtain the finished product.
[0052] Example 3 A super high-rise pumping concrete comprises the following raw materials: cement, water, admixture, coarse aggregate, fine aggregate, mineral admixture and mixture.
[0053] The cement is P.042.5 silicate cement, the admixture is polycarboxylic acid water reducer (slow-setting type), the coarse aggregate is 5-25mm crushed stone, the fine aggregate is 0.5-0.35mm machine-made sand, and the mineral admixtures are fly ash, mineral powder and silica powder.
[0054] The mixture includes ceramsite, polyacrylamide and silicon dioxide. The weight ratio of ceramsite, polyacrylamide and silicon dioxide is 1:0.2:0.5.
[0055] The particle size of ceramsite is 5-10 mm, and the particle size of silicon dioxide is 300 nm. Polyacrylamide is anionic, commercially available, and purchased from Henan Baiyuan Environmental Protection Technology Co., Ltd. in this embodiment.
[0056] The specific amount of each raw material is shown in Table 1.
[0057] The present application also provides a method for preparing super high-rise pumped concrete, comprising the following steps: Step 1: Prepare an aqueous solution of the mixture: Step 1a: Weigh water according to the weight ratio of ceramsite to water of 1:1, and this part of water is defined as water A.
[0058] The ceramsite, silicon dioxide and water A were ultrasonically mixed for 10 min at an ultrasonic frequency of 35 KHz and an ultrasonic power of 250 W to obtain a primary mixture.
[0059] Step 1b: Add polyacrylamide to the primary mixture, and mix for 5 minutes under ultrasonic conditions of 35 kHz and 250 W to obtain an aqueous solution of the mixture.
[0060] Step 2: Mix cement, mineral admixtures, and remaining water (this portion is defined as water B, the sum of water A and water B is 160, and the water recorded in Table 1 is also the sum), and stir until uniform to obtain the first mixture.
[0061] Step 3: Mix the first mixture with the mixture and stir until uniform to obtain a second mixture.
[0062] Step 4: Mix the second mixture with coarse aggregate and fine aggregate, and stir until uniform to obtain the third mixture.
[0063] Step 5: Mix the third mixture with the admixture, stir until uniform, and obtain the finished product.
[0064] Example 4 A super high-rise pumping concrete comprises the following raw materials: cement, water, admixture, coarse aggregate, fine aggregate, mineral admixture and mixture.
[0065] The cement is P.042.5 silicate cement, the admixture is polycarboxylic acid water reducer (slow-setting type), the coarse aggregate is 5-25mm crushed stone, the fine aggregate is 0.5-0.35mm machine-made sand, and the mineral admixtures are fly ash, mineral powder and silica powder.
[0066] The mixture includes ceramsite, polyacrylamide and silicon dioxide. The weight ratio of ceramsite, polyacrylamide and silicon dioxide is 1:0.1:0.35.
[0067] The particle size of ceramsite is 5-10 mm, and the particle size of silicon dioxide is 250 nm. Polyacrylamide is anionic, commercially available, and purchased from Henan Baiyuan Environmental Protection Technology Co., Ltd. in this embodiment.
[0068] The specific amount of each raw material is shown in Table 1.
[0069] The present application also provides a method for preparing super high-rise pumped concrete, comprising the following steps: Step 1: Prepare an aqueous solution of the mixture: Step 1a: Weigh water according to the weight ratio of ceramsite to water of 1:1, and this part of water is defined as water A.
[0070] The ceramsite, silicon dioxide and water A were ultrasonically mixed for 15 minutes at an ultrasonic frequency of 32 kHz and an ultrasonic power of 220 W to obtain a primary mixture.
[0071] Step 1b: Add polyacrylamide to the primary mixture, and mix for 8 minutes under ultrasonic conditions of maintaining an ultrasonic frequency of 32 kHz and an ultrasonic power of 220 W to obtain an aqueous solution of the mixture.
[0072] Step 2: Mix cement, mineral admixtures and remaining water (this part is defined as water B, the sum of water A and water B is 150, and the water recorded in Table 1 is also the sum), and stir until uniform to obtain the first mixture.
[0073] Step 3: Mix the first mixture with the mixture and stir until uniform to obtain a second mixture.
[0074] Step 4: Mix the second mixture with coarse aggregate and fine aggregate, and stir until uniform to obtain the third mixture.
[0075] Step 5: Mix the third mixture with the admixture, stir until uniform, and obtain the finished product.
[0076] Example 5 A super high-rise pumping concrete comprises the following raw materials: cement, water, admixture, coarse aggregate, fine aggregate, mineral admixture and mixture.
[0077] The cement is P.042.5 silicate cement, the admixture is polycarboxylic acid water reducer (slow-setting type), the coarse aggregate is 5-25mm crushed stone, the fine aggregate is 0.5-0.35mm machine-made sand, and the mineral admixtures are fly ash, mineral powder and silica powder.
[0078] The mixture includes ceramsite, polyacrylamide and silicon dioxide. The weight ratio of ceramsite, polyacrylamide and silicon dioxide is 1:0.15:0.45.
[0079] The particle size of ceramsite is 5-10 mm, and the particle size of silicon dioxide is 250 nm. Polyacrylamide is anionic, commercially available, and purchased from Henan Baiyuan Environmental Protection Technology Co., Ltd. in this embodiment.
[0080] The specific amount of each raw material is shown in Table 1.
[0081] The present application also provides a method for preparing super high-rise pumped concrete, comprising the following steps: Step 1: Prepare an aqueous solution of the mixture: Step 1a: Weigh water according to the weight ratio of ceramsite to water of 1:1, and this part of water is defined as water A.
[0082] The ceramsite, silicon dioxide and water A were ultrasonically mixed for 15 minutes at an ultrasonic frequency of 32 kHz and an ultrasonic power of 220 W to obtain a primary mixture.
[0083] Step 1b: Add polyacrylamide to the primary mixture, and mix for 8 minutes under ultrasonic conditions of maintaining an ultrasonic frequency of 32 kHz and an ultrasonic power of 220 W to obtain an aqueous solution of the mixture.
[0084] Step 2: Mix cement, mineral admixtures and remaining water (this part is defined as water B, the sum of water A and water B is 150, and the water recorded in Table 1 is also the sum), and stir until uniform to obtain the first mixture.
[0085] Step 3: Mix the first mixture with the mixture and stir until uniform to obtain a second mixture.
[0086] Step 4: Mix the second mixture with coarse aggregate and fine aggregate, and stir until uniform to obtain the third mixture.
[0087] Step 5: Mix the third mixture with the admixture, stir until uniform, and obtain the finished product.
[0088] Table 1 Example 6 A super high-rise pumping concrete, which is different from Example 1 in that the particle size of the ceramsite is 20-25 mm.
[0089] Example 7 A super high-rise pumping concrete, which is different from Example 1 in that the particle size of silicon dioxide is 200 μm.
[0090] Example 8 A method for preparing super high-rise pumping concrete, which is different from Example 1 in that: the ultrasonic conditions in step 1 are: ultrasonic frequency 10KHz, ultrasonic power 100W.
[0091] Example 9 A method for preparing super high-rise pumping concrete, which is different from Example 1 in that: the ultrasonic conditions in step 1 are: ultrasonic frequency 50KHz, ultrasonic power 500W.
[0092] Example 10 A method for preparing super high-rise pumping concrete, which is different from Example 1 in that: the specific steps of step 1 are as follows: ceramsite, silicon dioxide, polyacrylamide and water are mixed, and ultrasonic mixing is performed for 23 minutes under the conditions of ultrasonic frequency of 32KHz and ultrasonic power of 220W to obtain an aqueous solution of the mixture.
[0093] Comparative Example Comparative Example 1 A super high-rise pumping concrete, which is different from Example 1 in that the polyacrylamide in the mixture is replaced by xanthan gum.
[0094] Comparative Example 2 A super high-rise pumping concrete, which is different from Example 1 in that the silicon dioxide in the mixture is replaced by fly ash.
[0095] Comparative Example 3 A super high-rise pumping concrete, which is different from Example 1 in that the ceramsite in the mixture is replaced by perlite.
[0096] Comparative Example 4 A super high-rise pumping concrete, which is different from Example 1 in that the weight ratio of ceramsite, polyacrylamide and silicon dioxide is 1:0.4:0.1.
[0097] Performance testing 1. Pumping performance: According to GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures", the super-high-rise pumping concrete of Examples 1-10 and Comparative Examples 1-4 was tested, and the expansion degree out of the machine and the expansion degree 3 hours after pumping were recorded in Table 2.
[0098] 2. Segregation resistance: With reference to JGJ / T 283-2012 "Technical Specification for Application of Self-compacting Concrete", the super-high-rise pumping concrete of Examples 1-10 and Comparative Examples 1-4 was tested by sieve analysis, and the segregation rates were recorded in Table 2.
[0099] 3. Compressive strength: Referring to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the super-high-rise pumped concrete of Examples 1-10 and Comparative Examples 1-4 was tested for 28d compressive strength, and the results are recorded in Table 2.
[0100] 4. Splitting tensile strength: With reference to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the splitting tensile strength of the super-high-rise pumped concrete of Examples 1-10 and Comparative Examples 1-4 was tested, and the results are recorded in Table 2.
[0101] Loading speed is 0.4kN / s Table 2 According to the test data in Table 2, the super-high-rise pumped concrete of Examples 1-10 maintains a high degree of expansion when leaving the machine and 3 hours after pumping, indicating that it has good pumping performance. Compared with the super-high-rise pumped concrete of Comparative Examples 1-4, the degree of expansion of Examples 1-10 when leaving the machine and 3 hours after pumping is slightly different, indicating that it still maintains good workability. Not only that, the super-high-rise pumped concrete of Examples 1-10 is significantly better than that of Comparative Examples 1-4 in terms of anti-segregation, compressive strength, and splitting tensile strength. This shows that the specifically prepared mixture is used in super-high-rise pumped concrete, which can ensure the pumpability and fluidity of the super-high-rise pumped concrete, while making it have high performance and can adapt to more needs and scenarios.
[0102] The data also show that the special combination of the mixture is an organic whole. Any replacement or split will have a great impact on the performance of the mixture, resulting in its inability to perform excellent performance in super-high-rise pumped concrete.
[0103] Example 6 is based on Example 1, but the particle size of ceramsite is changed; Example 7 is based on Example 1, but the particle size of silicon dioxide is changed; Examples 8-9 are based on Example 1, but the ultrasonic conditions when preparing the mixture are changed; Example 10 is based on Example 1, but the mixing method of the raw materials of the mixture is changed. According to the data in Table 2, in all tests of Examples 6-10, there is a more or less downward trend compared with Example 1, indicating that further limiting the specifications of ceramsite and silicon dioxide and the ultrasonic conditions and feeding method when preparing the mixture can contribute to the formation of special structures.
[0104] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A super high-rise pumping concrete, characterized in that: According to weight parts, it includes the following raw materials: 155-175 parts of cement, 140-160 parts of water, 1-10 parts of admixture, 1050-1200 parts of coarse aggregate, 700-800 parts of fine aggregate, 150-200 parts of mineral admixture, and 30-50 parts of mixture; The mixture includes ceramsite, polyacrylamide and silicon dioxide, and the weight ratio of ceramsite, polyacrylamide and silicon dioxide is 1: (0.05-0.2): (0.2-0.5).
2. The super high-rise pumped concrete according to claim 1 is characterized in that: The weight ratio of the ceramsite, polyacrylamide and silicon dioxide is 1: (0.1-0.15): (0.35-0.45).
3. The super high-rise pumped concrete according to claim 1 is characterized in that: The particle size of the ceramsite is 5-10 mm.
4. The super high-rise pumped concrete according to claim 1 is characterized in that: The particle size of the silicon dioxide is 200-300 nm.
5. The super high-rise pumped concrete according to claim 1 is characterized in that: The mineral admixture includes a mixture of one or more of fly ash, mineral powder and silicon powder.
6. The super high-rise pumped concrete according to claim 5, characterized in that: The mineral admixtures are fly ash, mineral powder and silica powder. Calculated by weight of the super high-rise pumping concrete, the fly ash is 60-80 parts, the mineral powder is 80-90 parts, and the silica powder is 10-30 parts.
7. A method for preparing super high-rise pumped concrete according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: preparing an aqueous solution of the mixture: taking a portion of water and mixing it with ceramsite, polyacrylamide and silicon dioxide under ultrasonic conditions to obtain an aqueous solution of the mixture; Step 2: Mix cement, mineral admixture and remaining water until uniform to obtain a first mixture; Step 3: Mixing the first mixture with the aqueous solution of the mixture until uniform, to obtain a second mixture; Step 4: Mix the second mixture with the coarse aggregate and the fine aggregate until they are uniform to obtain the third mixture; Step 5: Mix the third mixture with the admixture until uniform to obtain the finished product.
8. The method for preparing super high-rise pumped concrete according to claim 7, characterized in that: The specific steps of step 1 are as follows: Step 1a: Mix ceramsite, silicon dioxide and water, and ultrasonically mix for 10-20 minutes at an ultrasonic frequency of 30-35 kHz and an ultrasonic power of 200-250 W to obtain a primary mixture; Step 1b: Add polyacrylamide to the initial mixture and mix under ultrasonic conditions for 5-10 minutes to obtain an aqueous solution of the mixture.
Citation Information
Patent Citations
C60 pumping concrete and preparation method thereof
CN111153655A
Large-flow-state circumferential inverted arch thin-wall anti-crack concrete and preparation method thereof
CN112851257A
Premixed pumping light-weight high-strength concrete mixture and preparation method thereof
CN114315287A
METHOD FOR PRODUCING CONSTRUCTION PRODUCTS BASED ON A SILICA-CONTAINING BINDER