In-situ synthesis composite sagger and preparation method and application thereof
By using in-situ synthetic composite scaffolds prepared from talc, kaolin and other materials in the production of lithium battery positive electrode materials, the problem of insufficient durability of scaffolds during high-temperature roasting is solved, and the effect of high recycling service life and wide application is achieved .
Patent Information
- Application Number
- CN202411334320.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-26
AI Technical Summary
In the production of existing lithium battery positive electrode materials, the scaffold is susceptible to alkaline corrosion by Li2O during the high-temperature roasting process, resulting in insufficient durability and inability to effectively resist high-temperature and alkaline corrosion.
The in-situ synthetic composite kettle consisting of the inner surface working layer and the outer substrate layer is used. The inner surface working layer contains talc, kaolin, activated α alumina, spinel and other materials, and the outer substrate layer contains kaolin, plate-shaped corundum, Electromolyte white corundum, etc., are prepared through specific ratios and sintering processes to form a cassette with excellent alkali resistance and high temperature performance.
It realizes the excellent thermal shock resistance and high circulation service life of the silhouette, significantly improves the tolerance to alkaline erosion, and has a wide range of application prospects.
Smart Images

Figure CN119019163A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of secondary batteries, and in particular to an in-situ synthetic composite sagger and a preparation method and application thereof. Background Art
[0002] The positive electrode materials of lithium batteries must be sintered in a high-temperature roller kiln at about 1000°C. The raw materials used are mainly cobalt oxide or nickel cobalt manganese oxide and lithium carbonate or lithium hydroxide as lithium sources. Therefore, the sintering process must use a sagger that can withstand high temperatures, alkaline oxidation corrosion, and cracking.
[0003] The sagger materials used in the production of lithium-ion battery positive electrode materials are mainly mullite or mullite-cordierite and corundum mullite. Li2CO3 or LiOH·H2O is used in the production of lithium battery positive electrode materials. They will decompose into Li2O during high-temperature roasting. Since Li2O has strong alkaline corrosion, Li2O will react with Al2O3 and SiO2 to produce LiAlO2 and LiAlSiO4. Therefore, the alkaline corrosion of the positive electrode raw materials on the sagger is relatively large, requiring the sagger to have high corrosion resistance.
[0004] In view of this, this application is filed. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an in-situ synthetic composite sagger and a preparation method thereof and an application thereof in the preparation of positive electrode materials. The sagger has an excellent cycle life and has broad application prospects.
[0006] To achieve the above object, the technical solution adopted by the present invention is: An in-situ synthetic composite sagger, the sagger comprising an inner surface working layer and an outer matrix layer from inside to outside; the thickness of the inner surface working layer is 1-3 mm; The inner surface working layer comprises the following raw materials in parts by weight: 5-30 parts of talc, 5-15 parts of kaolin, 0-10 parts of active α-alumina, 0-5 parts of organic binder, 10-65 parts of spinel, 0-10 parts of magnesium carbonate, 0-15 parts of zirconium oxide, 0-20 parts of yttrium-stabilized zirconium oxide, and 1-5 parts of water; The spinel includes a first spinel and a second spinel, the mass ratio of the first spinel to the second spinel is 20-100:0-80, the particle size of the first spinel is 0.5-1 mm, and the particle size of the second spinel is 1-2 mm; The outer matrix layer includes the following raw materials in parts by weight: 5-7 parts of kaolin, 0-19 parts of plate-like corundum, 15-35 parts of fused white corundum, 6-12 parts of active α-alumina, 0-8 parts of zirconium mullite, 1-4 parts of organic binder, 0-5 parts of spodumene, 0-2 parts of cordierite, 34-70 parts of magnesium-rich spinel, 0-8 parts of magnesium carbonate, 3-10 parts of zirconium oxide, 0-4 parts of zircon, 0-3 parts of yttrium oxide, 0-1.5 parts of feldspar, and 1-5 parts of water.
[0007] As a preferred embodiment of the present invention, the inner surface working layer includes the following raw materials in parts by weight: 6 to 17 parts of talc, 10 to 14 parts of kaolin, 0 to 8 parts of active α-alumina, 1 to 5 parts of organic binder, 50 to 65 parts of spinel, 0 to 6 parts of magnesium carbonate, 0 to 15 parts of zirconium oxide, 0 to 20 parts of yttrium-stabilized zirconium oxide, and 1 to 5 parts of water.
[0008] As a preferred embodiment of the present invention, the first spinel and the second spinel independently include at least one of magnesium-rich spinel, fused magnesium-rich spinel, and fused aluminum-magnesium spinel.
[0009] As a preferred embodiment of the present invention, the average particle size of the activated α-alumina is 1-2 μm.
[0010] As a preferred embodiment of the present invention, the particle size of the yttrium-stabilized zirconia is 600-1000 mesh; and / or The particle size of the zirconium oxide is 600-1000 mesh.
[0011] The iron oxide content of the kaolin used in the present invention is less than 1 part, and the particle size D50 is less than 10 μm.
[0012] Among them, the tabular corundum is 200~325 mesh.
[0013] Among them, zirconium mullite has a zirconium oxide content of more than 30% and a mesh size of 200 to 325.
[0014] Among them, spodumene is a powder with lithium oxide content greater than 6% and less than 325 mesh.
[0015] Among them, cordierite is cordierite phase>90%; 200~325 mesh.
[0016] Among them, magnesium-rich spinel has a magnesium oxide content of more than 30%.
[0017] Among them, the zirconium oxide has a zirconium oxide content of more than 99% and a mesh size of 325 to 800.
[0018] Among them, magnesium carbonate is industrial grade, magnesium oxide content>45%, powder.
[0019] Among them, zircon has a zirconium oxide content of >65%, 325~800 mesh.
[0020] Among them, feldspar is potassium feldspar or sodium feldspar, and iron oxide is less than 1%.
[0021] As a preferred embodiment of the present invention, the fused white corundum is composed of 800 mesh fused white corundum and 200-325 mesh fused white corundum in a weight ratio of 1:0.5-2.
[0022] As a preferred embodiment of the present invention, the organic binder is at least one of sodium lignin sulfonate, calcium lignin sulfonate, peach gum, yellow dextrin, white dextrin, polyvinyl alcohol, polyethylene glycol, 801 glue powder, carboxymethyl cellulose, and hydroxypropyl methyl cellulose.
[0023] The present invention also provides a method for preparing an in-situ synthetic composite sagger, comprising the following steps: (1) Weigh the raw materials of the inner surface working layer according to the ratio, mix water and organic binder evenly to obtain an organic binder solution, premix the remaining materials evenly to obtain a premix, mix the premix with the organic binder evenly, age, and pass through a 2-3 mesh sieve to obtain a material body of the inner surface working layer; (2) Weigh the raw materials of the outer matrix layer according to the ratio, mix water and organic binder evenly to obtain a binder solution, premix the remaining materials evenly, and then mix them evenly with the organic binder solution, age them, and pass them through a 2-3 mesh sieve to obtain the outer matrix layer material; (3) Adding the inner surface working layer material and the outer matrix layer material into the mold respectively, pressing, drying, and sintering to obtain an in-situ synthesized composite sagger; wherein the sintering temperature is 1300-1400°C, and the sintering time is 1-10 hours.
[0024] The present invention also provides an application of an in-situ synthetic composite sagger in preparing positive electrode materials.
[0025] The beneficial effects of the present invention are as follows: the present invention uses the outer substrate layer as the outer layer, the inner layer is resistant to alkali corrosion, the outer layer is resistant to high temperature, the sagger has excellent thermal shock resistance, the sagger has a high cycle service life, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the XRD pattern of the sagger of the present invention.
[0027] Figure 2 This is a diagram for evaluating the thermal shock resistance of saggers. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0029] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0030] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0031] In the present application, there is no particular limitation on the specific dispersion and stirring treatment methods.
[0032] Unless otherwise specified, the components, raw materials or instruments used in the embodiments and comparative examples of the present invention are all commercially available raw materials or instruments, and the components and raw materials used in each parallel experiment are all of the same kind.
[0033] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.
[0034] Example 1 A method for preparing an in-situ synthetic composite sagger comprises the following steps: (1) Weigh the raw materials of the inner surface working layer according to the following ratio: 15.1 parts of talc, 14 parts of kaolin, 6 parts of active α-alumina, 2 parts of carboxymethyl cellulose, 65 parts of fused magnesia alumina spinel, and 2 parts of water; the fused magnesia alumina spinel includes a first fused magnesia alumina spinel and a second fused magnesia alumina spinel, the mass ratio of the first fused magnesia alumina spinel to the second fused magnesia alumina spinel is 31:69, the particle size of the first fused magnesia alumina spinel is 0.5-1 mm, and the particle size of the second fused magnesia alumina spinel is 1-2 mm; the average particle size of the active α-alumina is 1-2 μm; Mix water and carboxymethyl cellulose evenly to obtain a carboxymethyl cellulose solution, premix the remaining materials evenly to obtain a premix, mix the premix with the carboxymethyl cellulose solution evenly, age (also known as trapped material) for 24 hours, and pass through a 2-3 mesh sieve to obtain an inner surface working layer material body; (2) Weigh the raw materials of the outer matrix layer according to the following ratio: 7 parts of kaolin, 17.5 parts of 800 mesh fused white corundum, 17.5 parts of 200-325 mesh fused white corundum, 8 parts of activated α-alumina, 5 parts of spodumene, 34 parts of magnesium-rich spinel, 8 parts of magnesium carbonate, 3 parts of zirconium oxide, 0.3 parts of yttrium oxide, 2 parts of carboxymethyl cellulose, and 2.5 parts of water; Mix water and carboxymethyl cellulose evenly to obtain a carboxymethyl cellulose solution, premix the remaining materials evenly, then mix them evenly with the carboxymethyl cellulose solution, age them for 24 hours, and pass them through a 2-3 mesh sieve to obtain an outer matrix layer material; (3) The inner surface working layer material and the outer matrix layer material are added into the mold respectively, and the semi-finished product is obtained by pressing with a bidirectional 1500T hydraulic press, which is then dried at 80°C for 4h and sintered at 1350°C for 5h to obtain an in-situ synthesized composite sagger.
[0035] Among them, the XRD pattern of this embodiment is as follows Figure 1 shown.
[0036] Example 2 A method for preparing an in-situ synthetic composite sagger comprises the following steps: (1) Weigh the raw materials of the inner surface working layer according to the following ratio: 17 parts of talc, 12 parts of kaolin, 3 parts of activated α-alumina, 2 parts of carboxymethyl cellulose, 8 parts of zirconium oxide, 60 parts of magnesium-rich spinel, and 3.5 parts of water; the particle size of the magnesium-rich spinel is 0.5-1 mm; the average particle size of the activated α-alumina is 1-2 μm; the particle size of the zirconium oxide is 800 mesh; Mix water and carboxymethyl cellulose evenly to obtain a carboxymethyl cellulose solution, premix the remaining materials evenly to obtain a premix, mix the premix with the carboxymethyl cellulose solution evenly, age (also known as trapped material) for 24 hours, and pass through a 2-3 mesh sieve to obtain an inner surface working layer material body; (2) Weigh the raw materials of the outer matrix layer according to the following ratio: 5 parts of kaolin, 10 parts of plate-like corundum, 7.5 parts of 800 mesh fused white corundum, 7.5 parts of 200-325 mesh fused white corundum, 8 parts of activated α-alumina, 5 parts of zirconium mullite, 2 parts of cordierite, 45 parts of magnesium-rich spinel, 6 parts of zirconium oxide, 4 parts of zircon, 2 parts of carboxymethyl cellulose, and 2.5 parts of water; Mix water and carboxymethyl cellulose evenly to obtain a carboxymethyl cellulose solution, premix the remaining materials evenly, then mix them evenly with the carboxymethyl cellulose solution, age them for 24 hours, and pass them through a 2-3 mesh sieve to obtain an outer matrix layer material; (3) The inner surface working layer material and the outer matrix layer material are added into the mold respectively, and the semi-finished product is obtained by pressing with a bidirectional 1500T hydraulic press, which is then dried at 80°C for 4h and sintered at 1350°C for 5h to obtain an in-situ synthesized composite sagger.
[0037] Example 3 A method for preparing an in-situ synthetic composite sagger comprises the following steps: (1) Weigh the raw materials of the inner surface working layer according to the following ratio: 17 parts of talc, 12 parts of kaolin, 2 parts of carboxymethyl cellulose, 15 parts of zirconium oxide, 50 parts of magnesium-rich spinel, and 3.5 parts of water; the particle size of the magnesium-rich spinel is 0.5-1 mm; the particle size of the zirconium oxide is 800 mesh; Mix water and carboxymethyl cellulose evenly to obtain a carboxymethyl cellulose solution, premix the remaining materials evenly to obtain a premix, mix the premix with the carboxymethyl cellulose solution evenly, age (also known as trapped material) for 24 hours, and pass through a 2-3 mesh sieve to obtain an inner surface working layer material body; (2) Weigh the raw materials of the outer matrix layer according to the following ratio: 7 parts of kaolin, 19 parts of plate-like corundum, 12 parts of activated α-alumina, 5 parts of zirconium mullite, 2 parts of cordierite, 49 parts of magnesium-rich spinel, 6 parts of zirconium oxide, 2 parts of carboxymethyl cellulose, and 2.5 parts of water; Mix water and carboxymethyl cellulose evenly to obtain a carboxymethyl cellulose solution, premix the remaining materials evenly, then mix them evenly with the carboxymethyl cellulose solution, age them for 24 hours, and pass them through a 2-3 mesh sieve to obtain an outer matrix layer material; (3) The inner surface working layer material and the outer matrix layer material are added into the mold respectively, and the semi-finished product is obtained by pressing with a bidirectional 1500T hydraulic press, which is then dried at 80°C for 4h and sintered at 1350°C for 5h to obtain an in-situ synthesized composite sagger.
[0038] Example 4 A method for preparing an in-situ synthetic composite sagger comprises the following steps: (1) Weigh the raw materials of the inner surface working layer according to the following ratio: 17 parts of talc, 12 parts of kaolin, 2 parts of carboxymethyl cellulose, 3 parts of active α-alumina, 8 parts of zirconia, 60 parts of fused magnesium-rich spinel, and 3.5 parts of water; the particle size of the magnesium-rich spinel is 0.5-1 mm; the average particle size of the active α-alumina is 1-2 μm; the particle size of the zirconium oxide is 800 mesh; Mix water and carboxymethyl cellulose evenly to obtain a carboxymethyl cellulose solution, premix the remaining materials evenly to obtain a premix, mix the premix with the carboxymethyl cellulose solution evenly, age (also known as trapped material) for 24 hours, and pass through a 2-3 mesh sieve to obtain an inner surface working layer material body; (2) Weigh the raw materials of the outer matrix layer according to the following ratio: 5 parts of kaolin, 6 parts of plate-like corundum, 9 parts of activated α-alumina, 8 parts of zirconium mullite, 2 parts of cordierite, 60 parts of magnesium-rich spinel, 10 parts of zirconium oxide, 1.5 parts of albite, 2 parts of carboxymethyl cellulose, and 2.5 parts of water; Mix water and carboxymethyl cellulose evenly to obtain a carboxymethyl cellulose solution, premix the remaining materials evenly, then mix them evenly with the carboxymethyl cellulose solution, age them for 24 hours, and pass them through a 2-3 mesh sieve to obtain an outer matrix layer material; (3) The inner surface working layer material and the outer matrix layer material are added into the mold respectively, and the semi-finished product is obtained by pressing with a bidirectional 1500T hydraulic press, which is then dried at 80°C for 4h and sintered at 1350°C for 5h to obtain an in-situ synthesized composite sagger.
[0039] Example 5 A method for preparing an in-situ synthetic composite sagger comprises the following steps: (1) Weigh the raw materials of the inner surface working layer according to the following ratio: 6 parts of talc, 10 parts of kaolin, 2 parts of carboxymethyl cellulose, 8 parts of active α-alumina, 5 parts of zirconium oxide, 65 parts of magnesium-rich spinel, 6 parts of magnesium carbonate, and 3.5 parts of water; the particle size of the magnesium-rich spinel is 0.5-1 mm; the average particle size of the active α-alumina is 1-2 μm; the particle size of the zirconium oxide is 800 mesh; Mix water and carboxymethyl cellulose evenly to obtain a carboxymethyl cellulose solution, premix the remaining materials evenly to obtain a premix, mix the premix with the carboxymethyl cellulose solution evenly, age (also known as trapped material) for 24 hours, and pass through a 2-3 mesh sieve to obtain an inner surface working layer material body; (2) Weigh the raw materials of the outer matrix layer according to the following ratio: 5 parts of kaolin, 6 parts of activated α-alumina, 5 parts of zirconium mullite, 2 parts of spodumene, 2 parts of cordierite, 70 parts of magnesium-rich spinel, 10 parts of zirconium oxide, 1.5 parts of albite, 2 parts of carboxymethyl cellulose, and 2.5 parts of water; Mix water and carboxymethyl cellulose evenly to obtain a carboxymethyl cellulose solution, premix the remaining materials evenly, then mix them evenly with the carboxymethyl cellulose solution, age them for 24 hours, and pass them through a 2-3 mesh sieve to obtain an outer matrix layer material; (3) The inner surface working layer material and the outer matrix layer material are added into the mold respectively, and the semi-finished product is obtained by pressing with a bidirectional 1500T hydraulic press, which is then dried at 80°C for 4h and sintered at 1350°C for 5h to obtain an in-situ synthesized composite sagger.
[0040] Among them, the performance test of the embodiment is as follows Figure 2 shown.
[0041] Table 1 The sagger described in the present invention has excellent thermal shock resistance, a high cycle service life and a wide range of application prospects.
[0042] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. An in-situ synthetic composite sagger, It is characterized in that The sagger comprises an inner surface working layer and an outer matrix layer from inside to outside; the thickness of the inner surface working layer is 1-3 mm; The inner surface working layer comprises the following raw materials in parts by weight: 5-30 parts of talc, 5-15 parts of kaolin, 0-10 parts of active α-alumina, 0-5 parts of organic binder, 10-65 parts of spinel, 0-10 parts of magnesium carbonate, 0-15 parts of zirconium oxide, 0-20 parts of yttrium-stabilized zirconium oxide, and 1-5 parts of water; the spinel comprises a first spinel and a second spinel, the mass ratio of the first spinel to the second spinel is 20-100:0-80, the particle size of the first spinel is 0.5-1 mm, and the particle size of the second spinel is 1-2 mm; The outer matrix layer includes the following raw materials in parts by weight: 5-7 parts of kaolin, 0-19 parts of plate-like corundum, 15-35 parts of fused white corundum, 6-12 parts of active α-alumina, 0-8 parts of zirconium mullite, 1-4 parts of organic binder, 0-5 parts of spodumene, 0-2 parts of cordierite, 34-70 parts of magnesium-rich spinel, 0-8 parts of magnesium carbonate, 3-10 parts of zirconium oxide, 0-4 parts of zircon, 0-3 parts of yttrium oxide, 0-1.5 parts of feldspar, and 1-5 parts of water.
2. The in-situ synthetic composite sagger according to claim 1, It is characterized in that The inner surface working layer includes the following raw materials in parts by weight: 6-17 parts of talc, 10-14 parts of kaolin, 0-8 parts of active α-alumina, 1-5 parts of organic binder, 50-65 parts of spinel, 0-6 parts of magnesium carbonate, 0-15 parts of zirconium oxide, 0-20 parts of yttrium-stabilized zirconium oxide, and 1-5 parts of water.
3. The in-situ synthetic composite sagger according to claim 1, It is characterized in that The first spinel and the second spinel independently include at least one of magnesium-rich spinel, fused magnesium-rich spinel, and fused aluminum-magnesium spinel.
4. The in-situ synthetic composite sagger according to claim 1, It is characterized in that The average particle size of the activated α-alumina is 1-2 μm.
5. The in-situ synthetic composite sagger according to claim 1, It is characterized in that The particle size of the yttrium stabilized zirconia is 600-1000 mesh; and / or The particle size of the zirconium oxide is 600-1000 mesh.
6. The in-situ synthetic composite sagger according to claim 1, It is characterized in that The fused white corundum is composed of 800 mesh fused white corundum and 200-325 mesh fused white corundum in a weight ratio of 1:0.5-2.
7. The in-situ synthetic composite sagger according to any one of claims 1 to 6, It is characterized in that The organic binder is at least one of sodium lignin sulfonate, calcium lignin sulfonate, peach gum, yellow dextrin, white dextrin, polyvinyl alcohol, polyethylene glycol, 801 glue powder, carboxymethyl cellulose, and hydroxypropyl methyl cellulose.
8. The method for preparing the in-situ synthetic composite sagger according to any one of claims 1 to 6, It is characterized in that The following steps are involved: (1) Weigh the raw materials of the inner surface working layer according to the ratio, mix water and organic binder evenly to obtain an organic binder solution, premix the remaining materials evenly to obtain a premix, mix the premix with the organic binder evenly, age, and pass through a 2-3 mesh sieve to obtain a material body of the inner surface working layer; (2) Weigh the raw materials of the outer matrix layer according to the ratio, mix water and organic binder evenly to obtain a binder solution, premix the remaining materials evenly, and then mix them evenly with the organic binder solution, age them, and pass them through a 2-3 mesh sieve to obtain the outer matrix layer material; (3) Adding the inner surface working layer material and the outer matrix layer material into the mold respectively, pressing, drying, and sintering to obtain an in-situ synthesized composite sagger; wherein the sintering temperature is 1300-1400°C, and the sintering time is 1-10 hours.
9. Use of the in-situ synthesis composite sagger according to any one of claims 1 to 7 in the preparation of positive electrode materials.
Citation Information
Patent Citations
Combination saggar and production method and application thereof
CN107963900A
Special sagger for sintering lithium battery positive electrode material and preparation method of sagger
CN110540418A
Sagger for positive electrode material of lithium battery and preparation method of sagger
CN112010661A
Double-layer structure sagger for lithium battery positive electrode material and preparation method of double-layer structure sagger
CN116655394A
Sagger for producing positive electrode active material of lithium ion battery
JP2009292704A
Cited By
Lithium aluminate composite sagger and preparation method and application thereof
CN120829303A