LiVO2-Li2TiO3 binary system microwave dielectric ceramic with adjustable temperature coefficient of resonance frequency and preparation method of LiVO2-Li2TiO3 binary system microwave dielectric ceramic

Through the solid phase sintering method of LiVO2-Li2TiO3 binary system microwave dielectric ceramics, the chemical formula and sintering temperature of the ceramics are regulated, and the resonance frequency temperature coefficient and high dielectric loss problems of ceramic materials in microwave communication are solved, and the problem of instability of the resonance frequency temperature coefficient and high dielectric loss of ceramic materials in microwave communication is achieved. The τf value of zero and the high Q×f value meet the temperature stability and low dielectric loss requirements of microwave communication.

CN119019165APending Publication Date: 2024-11-26SOUTHWEST PETROLEUM UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411121265.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

Smart Images

  • Figure BDA0004995172470000031
    Figure BDA0004995172470000031
  • Figure BDA0004995172470000032
    Figure BDA0004995172470000032
  • Figure BDA0004995172470000041
    Figure BDA0004995172470000041
Patent Text Reader

Abstract

The invention belongs to the field of electronic ceramics and manufacturing thereof, and relates to a LiVO2-Li2TiO3 binary system microwave dielectric ceramic with an adjustable temperature coefficient of resonance frequency and a preparation method of the LiVO2-Li2TiO3 binary system microwave dielectric ceramic. The sintering temperature of the microwave dielectric ceramic material provided by the invention is 825-900 DEG C, the dielectric constant is 17-25, the Q * f value can be up to 13788GHz, and the temperature coefficient of resonance frequency can be up to-4ppm / DEG C. The raw materials Li2CO3, V2O5 and TiO2 need to be blended according to the chemical general formula xLiVO2-(1-x) Li2TiO3, wherein x ranges from 0.025 to 0.5. The temperature-stable microwave dielectric ceramic material can be prepared through a solid-phase reaction sintering method, the preparation method is simple, industrial production is easy, and the temperature-stable microwave dielectric ceramic material is a novel layered structure microwave dielectric ceramic system with potential application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electronic ceramics and their manufacture, and relates to a LiVO2-Li2TiO3 binary system microwave dielectric ceramic with adjustable resonant frequency temperature coefficient and a preparation method thereof, which is mainly used in the communication field. Background Art

[0002] Microwave dielectric ceramics are new ceramic materials used as dielectric materials in microwave frequency band circuits to perform one or more functions. They are widely used in electronic components such as dielectric resonators, dielectric filters, dielectric antennas, and duplexers. For the application of dielectric ceramics in the field of microwave communications, it is required that the dielectric ceramic materials have high temperature stability, that is, the ceramic materials have a resonant frequency temperature coefficient (τ f ); At the same time, the ceramic material is required to exhibit low dielectric loss. An important indicator requirement of the filter is low insertion loss.

[0003] Among many microwave dielectric ceramics, Li2TiO3 ceramics have been widely used due to their good microwave dielectric properties and have played an important role in the field of electronic components. The best sintering temperature of pure Li2TiO3 ceramics is 1200℃, and the best microwave dielectric property it exhibits is ε r =23.29, Q×f=15525GHz, τ f =35.05ppm / ℃. At present, the τ of Li2TiO3 ceramics f The value control mainly adopts ion doping and preparation that can "compensate" for each other τ f The LiVO2 and Li2TiO3 ceramics are both layered crystal structures. + The octahedron formed with V 3+ The coordination polyhedron formed by O 2+ The tops of the Li2TiO3 are connected together and extend in layers along the c-axis to form a three-dimensional ordered crystal structure. + The octahedron formed with Ti 4+ The coordination polyhedrons share the same edges and vertices to form an orderly arrangement. At the same time, in the c-axis direction, the individual Li + The octahedral layer formed with Ti 4+ and Li + The co-arranged coordination polyhedron layers extend in sequence to form a crystal. According to the layered crystal structure of Li2TiO3 and LiVO2 ceramics, the interlayer spacing of the layered crystal structure and the degree of distortion of the oxygen polyhedrons between the layers can be controlled in order to obtain τ fThe novel microwave dielectric ceramic material system with a near-zero value can be used as a light-weight, temperature-stable material system with potential application value. The invention mainly discloses the preparation process and microwave dielectric properties of LiVO2-Li2TiO3 binary system microwave dielectric ceramics, and relates to a temperature-stable microwave dielectric ceramic material. Summary of the invention

[0004] The purpose of the present invention is to provide a LiVO2-Li2TiO3 binary system microwave dielectric ceramic with adjustable resonant frequency temperature coefficient and a preparation method thereof. The chemical formula of the material is xLiVO2-(1-x)Li2TiO3, wherein the range of x is between 0.025 and 0.5, and the raw materials used are Li2CO3, V2O5, and TiO2, and the material is prepared by solid phase sintering. Among them, when x=0.025 and the sintering temperature is 875°C, the prepared 0.025LiVO2-0.975Li2TiO3 has a Q×f value of up to 13788GHz and a dielectric constant of between 20 and 23; when x=0.05 and the sintering temperature is 825°C, the prepared 0.025LiVO2-0.975Li2TiO3 has a τ f =-4ppm / ℃, that is, a near-zero resonant frequency temperature coefficient is obtained. At this time, the Q×f value is 11939GHz and the dielectric constant is between 22 and 24.

[0005] The preparation method of the above microwave dielectric ceramic is as follows:

[0006] Step 1: According to the chemical formula of xLiVO2-(1-x)Li2TiO3, accurately weigh the oxide raw materials according to the stoichiometric ratio for mixing.

[0007] Step 2: Put the prepared powder into a nylon ball mill. The ball milling media are zirconium balls and anhydrous ethanol. The mass ratio of powder, zirconium balls and anhydrous ethanol is 1:5:1 to 1:5:2. Use a planetary ball mill to mill for 4 to 8 hours. Dry the milled slurry in an oven at 100°C and sieve it with a 100-mesh screen.

[0008] Step 3: Pre-sinter the LiVO2 and Li2TiO3 powders at a heating rate of 3°C / min to 500°C and 800°C, respectively.

[0009] Step 4: ball-mill the powder fired in step 3 for a second time, keep the ratio of powder, zirconium ball and deionized water at 1:5:1 to 1:5:2, mix and ball-mill for 4 to 8 hours, take out and dry in an oven at 100°C, granulate the powder with 13wt% PVA solution as a binder, and press into shape.

[0010] Step 5: First, increase the temperature to 600°C at a rate of 3°C / min and keep it warm for 2 hours to discharge the colloid, then sinter at 825°C~900°C in a high-temperature furnace in an air atmosphere, keep it warm for 4 hours, and cool naturally with the furnace.

[0011] In summary, the present invention adopts the traditional solid phase sintering method to obtain the LiVO2-Li2TiO3 binary system microwave dielectric ceramics, and can obtain the LiVO2-Li2TiO3 binary system microwave dielectric ceramics with a resonant frequency temperature coefficient of near zero, which can meet the basic needs of microwave communication. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 XRD diffraction patterns corresponding to Examples 1, 2, 3, and 4

[0013] Figure 2 XRD diffraction patterns corresponding to Examples 5, 6, 7, and 8 DETAILED DESCRIPTION

[0014] The present invention is further described in detail below with reference to the accompanying drawings and embodiments.

[0015] The chemical formula of the material of the present invention is: xLiVO2-(1-x)Li2TiO3. The material can be prepared by solid phase reaction. The specific steps of the embodiment are as follows:

[0016] Step 1: According to the chemical formula of xLiVO2-(1-x)Li2TiO3, accurately weigh the oxide raw materials Li2CO3, V2O5, and TiO2 according to the stoichiometric ratio.

[0017] Step 2: Put the prepared powder into a nylon ball mill, use zirconium balls and deionized water as the ball milling media, the mass ratio of powder, zirconium balls and anhydrous ethanol is 1:5:2, use a planetary mill for 6 hours, dry the ball-milled slurry in an oven at 100°C, and sieve it with a 100-mesh screen.

[0018] Step 3: Pre-sinter the LiVO2 and Li2TiO3 powders at a heating rate of 3°C / min to 500°C and 800°C, respectively.

[0019] Step 4: The powder pre-fired in step 3 is subjected to secondary ball milling, and the ratio of powder, zirconium balls and anhydrous ethanol is maintained at 1:5:2. The mixture is mixed for 6 hours, taken out and dried, and the powder is granulated with 13wt% PVA solution as a binder. The granulated powder is then pressed into shape.

[0020] Step 5: First, increase the temperature to 600°C at a rate of 3°C / min and keep it warm for 2 hours to discharge the colloid, then sinter at 825°C~900°C in a high-temperature furnace in an air atmosphere, keep it warm for 4 hours, and cool naturally with the furnace.

[0021] The specific composition and microwave dielectric properties of each embodiment are as follows:

[0022] Table 1 Sample number of the embodiment

[0023]

[0024] Table 2 Microwave dielectric properties of the samples of the embodiment

[0025]

[0026]

[0027] The data in Tables 1 and 2 above include the serial numbers corresponding to the example samples within the scope of the general chemical formula and the microwave dielectric properties of the example samples after sintering. It can be seen from the table that as x decreases from 0.2 to 0.05, the Q×f value of the LiVO2-Li2TiO3 binary system microwave dielectric ceramics shows a significant upward trend, indicating that the amount of LiVO2 added has a decisive influence on the Q×f value. Among them, excessive LiVO2 addition will significantly deteriorate the Q×f value of the system. At the same time, inappropriate sintering temperature will also lead to a decrease in the Q×f value of the system. Among them, the Q×f value of Example 3 can reach 13788GHz, and the dielectric constant is 22.56, showing the highest Q×f value within the scope of the general chemical formula; the τ of Example 5 f =-4ppm / ℃, that is, a near-zero resonant frequency temperature coefficient is obtained. At this time, the Q×f value is 11939GHz, the dielectric constant is 23, and the best comprehensive dielectric performance is obtained.

[0028] Figure 1 and Figure 2 The XRD patterns corresponding to Examples 3 and 5 respectively, the diffraction peaks of the samples match with the Li2V2O4 cards (PDF#38-0192) and Li2TiO3 (PDF#33-0831), indicating that the materials of Examples 3 and 5 correspond to layered structures and are solid solutions of Li2TiO3.

Claims

1. A LiVO2-Li2TiO3 binary system microwave dielectric ceramic with adjustable resonant frequency temperature coefficient and a preparation method thereof, characterized in that: The general chemical formula is xLiVO2-(1-x)Li2TiO3, where x ranges from 0.025 to 0.5, the dielectric constant is 17 to 25, the Q×f value can reach up to 13788GHz, and the resonant frequency temperature coefficient can reach -4ppm / ℃.

2. The microwave dielectric material according to claim 1, characterized in that: xLiVO2-(1-x)Li2TiO3, where x ranges from 0.025 to 0.5, and the raw materials used are Li2CO3, V2O5, and TiO2.

3. The method for preparing the dielectric material according to claim 2 comprises the following steps: Step 1: According to the chemical formula of LiVO2 and Li2TiO3, the oxide raw materials are accurately weighed and mixed according to the stoichiometric ratio; Step 2: Place the prepared powder in a nylon ball mill, the ball milling media is zirconium balls and anhydrous ethanol, the mass ratio of powder, zirconium balls and anhydrous ethanol is 1:5:1 to 1:5:2, use a planetary mill for 4h to 8h, dry the milled slurry in an oven at 100°C, and sieve it with a 100-mesh screen; Step 3: Pre-sintering the powders of LiVO2 and Li2TiO3 at a heating rate of 3°C / min to 500°C and 800°C respectively; Step 4: The powder fired in step 3 is subjected to secondary ball milling, and the ratio of powder, zirconium ball and anhydrous ethanol is maintained at 1:5:1 to 1:5:2, mixed for 4h to 8h, taken out and dried, and the powder is granulated with 13wt% PVA solution as a binder, and pressed into shape; Step 5: First, increase the temperature to 600°C at a rate of 3°C / min and keep it warm for 2 hours to discharge the colloid, then sinter at 825°C~900°C in a high-temperature furnace in an air atmosphere, keep it warm for 4 hours, and cool naturally with the furnace.

Citation Information

Patent Citations

  • Lithium ion battery anode material and preparation method thereof

    CN108461730A

  • Novel low-dielectric-constant microwave dielectric ceramic and preparation method thereof

    CN117945756A

  • Electrodes comprising mixed active particles

    CN1795514A