Porous silicon carbide material and preparation method thereof

By chemical vapor deposition in porous carbon, nanosilicon is generated and reacted with carbon in situ, combined with calcination treatment, the problem of porous silicon carbide material is solved, the stability and high-temperature performance of the material are achieved, and it is suitable for a variety of application fields. .

CN119019175AActive Publication Date: 2024-11-26NINGBO YINGCHUANG SCI & TECH ACHIEVEMENTS TRANSFORMATION SERVICE PARTNERSHIP (LLP)
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411481200.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-26
Estimated Expiration
2044-10-23

AI Technical Summary

Technical Problem

The existing methods are difficult to stabilize the pore structure of the material when preparing porous silicon carbide materials, and high-temperature heating reactions will destroy the skeleton structure of the porous carbon.

Method used

Using porous carbon as a support, a gas-phase silicon source is deposited in a protective atmosphere by chemical vapor deposition to generate amorphous nanosilicon particles, and react with carbon in situ during calcining to form a silicon carbide skeleton to avoid the production of CO2, and then remove unreacted The elemental carbon and silicon retain the porous carbon skeleton structure.

Benefits of technology

It has achieved effective control of the porous silicon carbide material porous carbon skeleton structure, retained the material's stability, corrosion resistance, oxidation resistance and high temperature performance, and is suitable for catalyst support, gas filtration adsorbents and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019175A_ABST
    Figure CN119019175A_ABST
Patent Text Reader

Abstract

The invention relates to a porous silicon carbide material and a preparation method thereof.The preparation method of the porous silicon carbide material comprises the steps that porous carbon serves as a carrier, protective gas and a gas-phase silicon source are introduced for chemical vapor deposition, and a first intermediate is obtained; continuously introducing protective gas, and calcining the first intermediate to obtain a second intermediate; and removing elemental carbon and / or elemental silicon in the second intermediate to obtain the porous silicon carbide material. In the preparation method disclosed by the invention, the gas-phase silicon source can be decomposed into amorphous nano silicon in situ in the porous carbon, and then the nano silicon can react with the carbon in situ to generate a silicon carbide skeleton during calcination treatment, so that the obtained porous silicon carbide material basically retains the skeleton structure of the porous carbon, and therefore, the porous silicon carbide material can be used for preparing the porous silicon carbide material. According to the preparation method, the pore structure of the porous silicon carbide material can be effectively controlled, and porous silicon carbide materials with different pore structures can be controllably prepared by selecting porous carbon with different pore structures as templates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new materials, and in particular to a porous silicon carbide material and a preparation method thereof. Background Art

[0002] Currently, the preparation methods of porous silicon carbide include organosilicon cracking, carbon thermal reaction, electrochemical etching, magnesium thermal reduction, nano-coating, etc. However, these methods cannot stably control the morphology of the material.

[0003] The template method uses porous carbon as a template, and can use the skeleton of porous carbon to retain the carbon skeleton structure while preparing porous silicon carbide. However, when using the template method to prepare porous silicon carbide, porous carbon is mainly used as a template. SiO is gasified by high-temperature heating and then infiltrated into the porous carbon, reacting with carbon to obtain porous silicon carbide. During the reaction of SiO and carbon, C will be consumed and CO2 will be generated, which will destroy the skeleton structure of the porous carbon, causing the porous carbon skeleton structure to collapse easily, and the pore structure of the obtained silicon carbide material cannot be controlled. Summary of the invention

[0004] Based on this, it is necessary to provide a mesoporous porous silicon carbide material and a preparation method thereof to address the above problems. The preparation method can effectively control the pore structure of the porous silicon carbide material.

[0005] The present invention provides a method for preparing a porous silicon carbide material, comprising the following steps: Using porous carbon as a carrier, introducing protective gas and a gas-phase silicon source to perform chemical vapor deposition to obtain a first intermediate; Continue to introduce the protective gas and calcine the first intermediate to obtain a second intermediate; The elemental carbon and / or elemental silicon in the second intermediate is removed to obtain a porous silicon carbide material.

[0006] In one embodiment, the porous carbon is selected from at least one of asphalt-based porous carbon, biomass-based porous carbon or resin-based porous carbon.

[0007] In one embodiment, the porous carbon satisfies at least one of the following conditions: (1) Specific surface area is 50m² / g-2300m² / g; (2) Pore volume is 0.1cm³ / g-5.0cm³ / g; (3) The pore size is 1nm-1μm.

[0008] In one embodiment, the step of introducing a protective gas and a gas-phase silicon source for chemical vapor deposition satisfies at least one of the following conditions: (1) The gas phase silicon source is selected from at least one of monosilane, ethylsilane or silicon tetrachloride; (2) Temperature is 450℃-800℃; (3) The flow ratio of the gas-phase silicon source to the protective gas is 0.1:1-1:0.1; (4) The protective gas is selected from at least one of nitrogen and argon.

[0009] In one embodiment, the step of introducing a protective gas and a gas-phase silicon source for chemical vapor deposition satisfies at least one of the following conditions: (1) Temperature is 500℃-600℃; (2) The flow ratio of the gas-phase silicon source to the protective gas is 1:1-5:1.

[0010] In one embodiment, in the step of calcining the first intermediate, the temperature is 800° C.-2000° C. and the time is 0.5 h-10 h.

[0011] In one embodiment, in the step of calcining the first intermediate, the temperature is 800° C.-1100° C. and the time is 5 h-7 h.

[0012] In one embodiment, the step of removing elemental carbon in the second intermediate includes: placing the second intermediate in an aerobic environment for calcination, wherein the heating rate is 0.5°C / min-10°C / min, the calcination temperature is 800°C-2000°C, and the calcination time is 0.5h-10h.

[0013] In one embodiment, the step of removing elemental silicon in the second intermediate comprises: placing the second intermediate in a strong base or hydrofluoric acid solution for reaction.

[0014] The present invention also provides a porous silicon carbide material prepared by the method for preparing the porous silicon carbide material.

[0015] In the preparation method of the present invention, when porous carbon is used as a carrier and protective gas and gas phase silicon source are introduced for chemical vapor deposition, the gas phase silicon source can be in situ decomposed into amorphous nano silicon inside the porous carbon, and then in the process of calcination, the nano silicon will react with carbon in situ to generate a silicon carbide skeleton, and C will not be consumed to produce CO2 during the reaction process, so this method will basically not destroy the skeleton structure of the porous carbon, and then, the unreacted elemental silicon and / or elemental carbon can be removed to obtain a porous silicon carbide material, which basically retains the skeleton structure of the porous carbon. Therefore, the preparation method of the present invention can effectively control the pore structure of the porous silicon carbide material, and porous carbon with different pore structures can be selected as a template to control the preparation of porous silicon carbide materials with different pore structures. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0017] Figure 1 This is the SEM spectrum of the biomass-based porous carbon in Example 1; Figure 2 This is the SEM spectrum of the porous silicon carbide material prepared in Example 1; Figure 3 This is the XRD spectrum of the porous silicon carbide material prepared in Example 1; Figure 4 This is the TEM spectrum of the porous silicon carbide material prepared in Example 1; Figure 5 is the SEM spectrum of the resin-based porous carbon in Example 2; Figure 6 This is the SEM spectrum of the porous silicon carbide material prepared in Example 2; Figure 7 This is the XRD spectrum of the porous silicon carbide material prepared in Example 2; Figure 8 This is the TEM spectrum of the porous silicon carbide material prepared in Example 2. DETAILED DESCRIPTION

[0018] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.

[0020] In the present invention, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0021] The method for preparing the porous silicon carbide material provided by the present invention comprises the following steps: S1, using porous carbon as a carrier, introducing protective gas and gas-phase silicon source to perform chemical vapor deposition to obtain a first intermediate; S2, continuing to introduce the protective gas and calcining the first intermediate to obtain a second intermediate; S3, removing the elemental carbon and / or elemental silicon in the second intermediate to obtain a porous silicon carbide material.

[0022] In step S1, when chemical vapor deposition is performed using a vapor-phase silicon source with porous carbon as a carrier under a protective atmosphere, the vapor-phase silicon source can be in situ decomposed into amorphous nano-silicon particles inside the porous carbon. The nano-silicon particles can be evenly distributed in the porous carbon due to their extremely small particle size and high specific surface area.

[0023] Furthermore, during the calcination treatment process in step S2, the nano-silicon particles will react in situ with the carbon in the porous carbon skeleton to generate a silicon carbide skeleton. No C will be consumed to produce CO2 during the reaction, so the reaction process of this method will basically not destroy the skeleton structure of the porous carbon. The unreacted elemental silicon and / or elemental carbon can be removed through step S3 to obtain a porous silicon carbide material, and the obtained porous silicon carbide material basically retains the skeleton structure of the porous carbon.

[0024] Therefore, the preparation method of the present invention can effectively control the pore structure of the porous silicon carbide material, and can select porous carbon with different pore structures as a template to control the preparation of porous silicon carbide materials with different pore structures.

[0025] The present invention does not limit the selection of porous carbon. Preferably, the porous carbon in step S1 is selected from at least one of asphalt-based porous carbon, biomass-based porous carbon or resin-based porous carbon.

[0026] Among them, the specific surface area of ​​the porous carbon is preferably 50m² / g to 2300m² / g, the pore volume is preferably 1.0cm³ / g to 5.0cm³ / g, and the pore size is preferably 1nm to 1μm. Therefore, by selecting porous carbon with different pore structures as templates, porous silicon carbide materials with different pore structures can be prepared in a controlled manner, especially silicon carbide materials with mesoporous structures can be prepared in a controlled manner.

[0027] In step S1, in the step of introducing a protective gas and a gas-phase silicon source for chemical vapor deposition, the gas-phase silicon source is selected from at least one of monosilane, ethylsilane or silicon tetrachloride, the protective gas is selected from at least one of nitrogen or an inert gas, and the inert gas can be selected from argon, etc. Among them, the flow ratio of the gas-phase silicon source to the protective gas is preferably 0.1:1 to 1:0.1, more preferably 1:1 to 5:1, specifically, the flow ratio of the gas-phase silicon source to the protective gas includes but is not limited to 1:1, 2:1, 3:1, 4:1, 5:1, etc., which is more conducive to the deposition effect of nano silicon particles.

[0028] Furthermore, the temperature in the chemical vapor deposition step is preferably 450°C to 800°C, further preferably 450°C to 750°C, more preferably 500°C to 600°C, including but not limited to 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, etc., which can also be more conducive to the deposition effect of nano-silicon particles.

[0029] In step S2, in the step of calcining the first intermediate, the temperature is preferably 800°C-2000°C, more preferably 800°C-1100°C, including but not limited to 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, etc., and the time is preferably 0.5h-10h, more preferably 5h-7h, including but not limited to 5h, 5.5h, 6h, 6.5h, 7h, etc., which is conducive to the full reaction of nano-silicon particles and carbon.

[0030] In step S3, a carbon removal treatment or a silicon removal treatment can be selectively performed according to the residual elemental carbon in the second intermediate. The step of removing the elemental carbon in the second intermediate includes: placing the second intermediate in an aerobic environment such as an air atmosphere or an oxygen atmosphere for calcination, wherein the heating rate is 0.5°C / min-10°C / min, specifically, the heating rate includes but is not limited to 0.5°C / min, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, and the calcination temperature is 800°C-2000°C, specifically, the calcination temperature is Including but not limited to 800℃, 900℃, 1000℃, 1100℃, 1200℃, 1300℃, 1400℃, 1500℃, 1600℃, 1700℃, 1800℃, 1900℃, 2000℃, etc., the calcination time is 0.5h-10h, specifically, the calcination time includes but is not limited to 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, etc.; the step of removing elemental silicon in the second intermediate includes: placing the second intermediate in a strong alkali solution such as sodium hydroxide or a hydrofluoric acid solution for reaction.

[0031] The present invention also provides a porous silicon carbide material prepared by the method for preparing the porous silicon carbide material.

[0032] The porous silicon carbide material of the present invention has stable chemical properties, excellent corrosion resistance, oxidation resistance and high temperature resistance, and also has the advantages of excellent high temperature strength. It has broad application prospects in many fields such as catalyst carriers, high temperature gas filtration adsorbents, molten metal filters, and thermal insulation or wave absorbing materials.

[0033] Hereinafter, the porous silicon carbide material and the preparation method thereof will be further described through the following specific examples.

[0034] Example 1 Take 1 kg of biomass-based porous carbon, the specific surface area of ​​the biomass-based porous carbon is 1200 m² / g, the pore volume is 0.5 cm³ / g, and the average pore diameter is 2.07 nm.

[0035] The biomass-based porous carbon was placed in a rotary kiln and nitrogen was introduced to replace the gas. The temperature was then raised to 500°C, and monosilane gas and nitrogen were introduced at a flow rate of 0.5 L / min and a flow rate of 3 L / min, respectively, for 360 min, to obtain a first intermediate with a silane deposition amount of 20%.

[0036] The nitrogen was continued to flow for 30 min, the temperature was raised to 800°C and calcined for 5 h, and then the temperature was naturally lowered to obtain the second intermediate.

[0037] The second intermediate was placed in a muffle furnace, the temperature was adjusted to 800° C., and calcined in air for 5 hours to obtain a porous silicon carbide material.

[0038] Figure 1 The SEM spectrum of biomass-based porous carbon. Figure 2 The SEM spectrum of the prepared porous silicon carbide material is compared with Figure 1 and Figure 2 It can be seen that the porous silicon carbide material basically retains the overall framework and structure of the porous carbon material, but adds some mesopores to the pore structure, which inevitably leads to partial collapse of the microporous structure of the material, resulting in an increase in the pore volume of the material and a decrease in the specific surface area, but this ratio is fixed. Figure 3 is the XRD spectrum of the prepared porous silicon carbide material. Figure 3 It can be seen that there are obvious characteristic peaks of silicon carbide in the material. Figure 4 TEM spectrum of the prepared porous silicon carbide material. Figure 4 It can be clearly seen that there are a large number of micropores distributed in the material.

[0039] Example 2 Take 1 kg of resin-based porous carbon, the specific surface area of ​​the resin-based porous carbon is 2000 m² / g, the pore volume is 0.8 cm³ / g, and the pore diameter is 2.41 nm.

[0040] The resin-based porous carbon was placed in a rotary kiln and nitrogen was introduced to replace the gas. The temperature was then raised to 450°C, and monosilane gas and nitrogen were introduced at a flow rate of 3 L / min and a flow rate of 15 L / min, respectively, for a time of 300 min, to obtain a first intermediate with a silane deposition amount of 55%.

[0041] After continuing to flow nitrogen for 30 minutes, the temperature was raised to 1000°C and calcined for 5 hours, and then naturally cooled to obtain the second intermediate.

[0042] The second intermediate is placed in a hydrofluoric acid ethanol solution, wherein the hydrofluoric acid is a 50% aqueous solution. The ethanol is a high-purity ethanol with a concentration of >99.5%, and the volume ratio of the hydrofluoric acid solution to the ethanol solution is 1:5. The mixture is immersed and stirred with a polytetrafluoroethylene stirrer for 12 hours to obtain a porous silicon carbide material.

[0043] Figure 5 The SEM spectrum of resin-based porous carbon. Figure 6 The SEM spectrum of the prepared porous silicon carbide material is compared with Figure 5 and Figure 6It can be seen that after the treatment, the overall material still maintains the overall structure of porous carbon. Similar to Example 1, a large number of mesoporous pores are added to the material, and the changes in pore volume and specific surface area are similar, which shows that this ratio change has nothing to do with the type of porous carbon material. In addition, Figure 7 is the XRD spectrum of the prepared porous silicon carbide material. Figure 7 It can be seen that the material is a porous carbon structure. Figure 8 TEM spectrum of the prepared porous silicon carbide material. Figure 8 It can be seen that there are a large number of microporous structures in the material, confirming that the material is porous silicon carbide material.

[0044] Example 3 Take 1kg of petroleum coke-based porous carbon, the specific surface area of ​​the petroleum coke-based porous carbon is 2200m² / g, the pore volume is 1.2cm³ / g, and the pore diameter is 1.89nm.

[0045] The petroleum coke-based porous carbon was placed in a rotary kiln and nitrogen was introduced to replace the gas. The temperature was then raised to 520°C, and monosilane gas and nitrogen were introduced at a flow rate of 3 L / min and a flow rate of 3 L / min, respectively, for a time of 300 min, to obtain a first intermediate with a silane deposition amount of 55%.

[0046] After nitrogen was continuously passed through for 30 min, the temperature was raised to 1100°C and calcined for 5 h, and then naturally cooled to obtain a second intermediate.

[0047] The second intermediate is placed in a hydrofluoric acid ethanol solution, wherein the hydrofluoric acid is a 49% aqueous solution, the ethanol is a high-purity ethanol with a concentration of >99.5%, and the volume ratio of the hydrofluoric acid solution to the ethanol solution is 1:5. The mixture is immersed and stirred with a polytetrafluoroethylene stirrer for 12 hours to obtain a porous silicon carbide material.

[0048] Example 4 Take 1kg of biomass porous carbon, the specific surface area of ​​the resin-based porous carbon is 2300m² / g, the pore volume is 1.3cm³ / g, and the pore diameter is 3.26nm.

[0049] The resin-based porous carbon was placed in a rotary kiln and nitrogen was introduced to replace the gas. The temperature was then raised to 450°C, and monosilane gas and nitrogen were introduced at a flow rate of 3 L / min and a flow rate of 3 L / min, respectively, for a time of 358 min, to obtain a first intermediate with a silane deposition amount of 57%.

[0050] After nitrogen was continuously passed through for 30 min, the temperature was raised to 900°C and calcined for 5 h, and then naturally cooled to obtain a second intermediate.

[0051] The second intermediate is placed in a hydrofluoric acid ethanol solution, wherein the hydrofluoric acid is a 51% aqueous solution, the ethanol is a high-purity ethanol with a concentration of >99.5%, and the volume ratio of the hydrofluoric acid solution to the ethanol solution is 1:5. The mixture is immersed and stirred with a polytetrafluoroethylene stirrer for 14 hours to obtain a porous silicon carbide material.

[0052] Example 5 Take 1kg of resin-based porous carbon, the specific surface area of ​​the resin-based porous carbon is 2200m² / g, the pore volume is 1.2cm³ / g, and the pore diameter is 4.03nm.

[0053] The resin-based porous carbon was placed in a rotary kiln and nitrogen was introduced to replace the gas. The temperature was then raised to 450°C, and monosilane gas and nitrogen were introduced at a flow rate of 3 L / min and a flow rate of 3 L / min, respectively, for a time of 358 min, to obtain a first intermediate with a silane deposition amount of 57%.

[0054] After nitrogen was continuously passed through for 30 min, the temperature was raised to 900°C and calcined for 5 h, and then naturally cooled to obtain a second intermediate.

[0055] The second intermediate is placed in an ethanol solution of hydrofluoric acid. The hydrofluoric acid is an aqueous solution with a concentration of 48%. The ethanol is a high-purity ethanol with a concentration of >99.5%. The volume ratio of the hydrofluoric acid solution to the ethanol solution is 1:5. The mixture is immersed and stirred with a polytetrafluoroethylene stirrer for 14 hours to obtain a porous silicon carbide material.

[0056] Example 6 Take 1kg of resin-based porous carbon. The specific surface area of ​​the resin-based porous carbon is 1500m² / g, the pore volume is 0.61cm³ / g, and the pore diameter is 2.11nm.

[0057] The resin-based porous carbon was placed in a rotary kiln and nitrogen was introduced to replace the gas. The temperature was then raised to 500°C, and monosilane gas and nitrogen were introduced at a flow rate of 1 L / min and a flow rate of 3 L / min, respectively, for 360 min, to obtain a first intermediate with a silane deposition amount of 31%.

[0058] After nitrogen was continuously passed through for 30 min, the temperature was raised to 800°C and calcined for 5 h, and then naturally cooled to obtain a second intermediate.

[0059] The second intermediate was placed in a muffle furnace, the temperature was adjusted to 800° C., and calcined in air for 5 hours to obtain a porous silicon carbide material.

[0060] Example 7 Take 1kg of resin-based porous carbon, the specific surface area of ​​the resin-based porous carbon is 1600m² / g, the pore volume is 0.75cm³ / g, and the pore diameter is 1.79nm.

[0061] The resin-based porous carbon was placed in a rotary kiln and nitrogen was introduced to replace the gas. The temperature was then raised to 450°C, and monosilane gas and nitrogen were introduced at a flow rate of 1 L / min and a flow rate of 3 L / min, respectively, for 360 min, to obtain a first intermediate with a silane deposition rate of 31%.

[0062] After nitrogen was continuously passed through for 30 min, the temperature was raised to 800°C and calcined for 5 h, and then naturally cooled to obtain a second intermediate.

[0063] The second intermediate was placed in a muffle furnace, the temperature was adjusted to 800° C., and calcined in air for 5 hours to obtain a porous silicon carbide material.

[0064] Example 8 Take 1kg of biomass porous carbon, the specific surface area of ​​the resin-based porous carbon is 1650m² / g, the pore volume is 0.78cm³ / g, and the pore diameter is 1.88nm.

[0065] The resin-based porous carbon was placed in a rotary kiln and nitrogen was introduced to replace the gas. The temperature was then raised to 450°C, and monosilane gas and nitrogen were introduced at a flow rate of 1 L / min and a flow rate of 3 L / min, respectively, for 360 min, to obtain a first intermediate with a silane deposition rate of 31%.

[0066] After nitrogen was continuously passed through for 30 min, the temperature was raised to 800°C and calcined for 5 h, and then naturally cooled to obtain a second intermediate.

[0067] The second intermediate was placed in a muffle furnace, the temperature was adjusted to 800° C., and calcined in air for 5 hours to obtain a porous silicon carbide material.

[0068] The specific surface area, pore volume and pore diameter of the porous carbon raw materials and the prepared porous silicon carbide in Examples 1 to 8 were tested and calculated, and the results are shown in Table 1 below.

[0069] Table 1

[0070] As can be seen from Table 1, the preparation method of the present invention can effectively control the pore structure of the porous silicon carbide material, and porous carbon with different pore structures can be selected as a template to control the preparation of porous silicon carbide materials with different pore structures.

[0071] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0072] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a porous silicon carbide material, characterized in that: The steps include: Using porous carbon as a carrier, introducing protective gas and a gas-phase silicon source to perform chemical vapor deposition to obtain a first intermediate; Continue to introduce the protective gas and calcine the first intermediate to obtain a second intermediate; The elemental carbon and / or elemental silicon in the second intermediate is removed to obtain a porous silicon carbide material.

2. The method for preparing the porous silicon carbide material according to claim 1, characterized in that: The porous carbon is selected from at least one of pitch-based porous carbon, biomass-based porous carbon or resin-based porous carbon.

3. The method for preparing the porous silicon carbide material according to claim 1, characterized in that: The porous carbon satisfies at least one of the following conditions: (1) Specific surface area is 50m² / g-2300m² / g; (2) Pore volume is 0.1cm³ / g-5.0cm³ / g; (3) The pore size is 1nm-1μm.

4. The method for preparing the porous silicon carbide material according to claim 1, characterized in that: The step of introducing a protective gas and a gas-phase silicon source for chemical vapor deposition satisfies at least one of the following conditions: (1) The gas phase silicon source is selected from at least one of monosilane, ethylsilane or silicon tetrachloride; (2) Temperature is 450℃-800℃; (3) The flow ratio of the gas-phase silicon source to the protective gas is 0.1:1-1:0.1; (4) The protective gas is selected from at least one of nitrogen and argon.

5. The method for preparing the porous silicon carbide material according to claim 1, characterized in that: The step of introducing a protective gas and a gas-phase silicon source for chemical vapor deposition satisfies at least one of the following conditions: (1) Temperature is 500℃-600℃; (2) The flow ratio of the gas-phase silicon source to the protective gas is 1:1-5:

1.

6. The method for preparing the porous silicon carbide material according to claim 1, characterized in that: In the step of calcining the first intermediate, the temperature is 800° C.-2000° C. and the time is 0.5 h-10 h.

7. The method for preparing the porous silicon carbide material according to claim 1, characterized in that: In the step of calcining the first intermediate, the temperature is 800° C.-1100° C. and the time is 5 h-7 h.

8. The method for preparing a porous silicon carbide material according to claim 1, characterized in that: The step of removing elemental carbon in the second intermediate includes: placing the second intermediate in an aerobic environment for calcination, wherein the heating rate is 0.5°C / min-10°C / min, the calcination temperature is 800°C-2000°C, and the calcination time is 0.5h-10h.

9. The method for preparing a porous silicon carbide material according to claim 1, characterized in that: The step of removing elemental silicon in the second intermediate comprises: placing the second intermediate in a strong base or hydrofluoric acid solution for reaction.

10. A porous silicon carbide material prepared by the method for preparing a porous silicon carbide material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method for mesoporous silicon carbide material

    CN102674354A

  • Method for preparing porous silicon carbide ceramic based on template

    CN105237034A

  • Preparation method for silicon carbide / epoxy resin composite material

    CN109627691A

  • Ordered porous material constructed by silicon carbide and carbon material and preparation method thereof

    CN113060735A

  • Method of preparing a porous silicon carbide

    NL9300816A