Solid oxide battery support body and functional layer preparation method

By spraying a transition layer roughening agent onto the support surface and spraying a functional layer of molten NiO-8YSZ, the problems of reduced pore size and porosity of the support and low bonding strength were solved, thus realizing a solid oxide battery with high strength, high porosity and high catalytic performance.

CN119019183AActive Publication Date: 2024-11-26SHANDONG RES & DESIGN ACADEMY OF IND CERAMICS

Patent Information

Application Number
CN202410927524.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-26
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

In existing technologies, solid oxide batteries suffer from reduced pore size and porosity during secondary heating, resulting in weak bonding between the functional layer and the support and decreased catalytic activity.

Method used

By spraying a transition layer containing a surface roughening agent onto the surface of the primary blank of the support, which then evaporates during sintering, an uneven transition layer is formed. Combined with a molten NiO-8YSZ spray functional layer, secondary sintering is avoided, and the bonding strength and porosity between the support and the functional layer are improved.

Benefits of technology

This approach achieves high support strength and high porosity, strong catalytic performance of the functional layer, and high bonding strength between the support and the functional layer, thus avoiding the reduction of pore size and open porosity and ensuring that the catalytic activity of the functional layer is not reduced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a solid oxide battery supporting body and a functional layer. The preparation method comprises the following steps: preparing supporting body pug, wherein the supporting body pug comprises N O, (Y2O3) 0.03-(ZrO2) 0.97 and a pore-forming agent; preparing a support body transition layer spraying material, wherein the support body transition layer spraying material comprises a transition layer surface roughening agent; preparing functional layer material slurry, wherein the functional layer material slurry is molten N O-8YSZ; preparing a primary blank of the support body through the support body pug; spraying a support body transition layer spraying material on the surface of the support body primary green body to obtain a support body secondary green body; carrying out glue removal on the secondary blank of the support body; sintering the support body biscuit, wherein the support body comprises a support body transition layer with an uneven surface and a support body base body layer connected with the support body transition layer; the solid oxide battery has the advantages of high support strength, high porosity, high aperture ratio, high catalytic performance of the functional layer, and high bonding strength between the support and the functional layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solid oxide batteries, and in particular to the field of a solid oxide battery support and a method for preparing a functional layer. Background Art

[0002] Solid oxide cell (SOC) is an all-solid-state ceramic device with the dual functions of solid oxide fuel cell (SOFC) and solid oxide electrolysis cell (SOEC). Solid oxide fuel cell (SOFC) can convert the chemical energy of fuel (such as H2, natural gas and other hydrocarbons) into electrical energy, while solid oxide electrolysis cell (SOEC) can convert renewable electricity such as solar energy and wind energy into hydrogen fuel by electrolyzing water, or co-electrolyze water and carbon dioxide to prepare synthesis gas, and then synthesize basic chemical raw materials such as methanol, thereby realizing the resource conversion of carbon dioxide.

[0003] The functional layer in the solid oxide battery has high electronic / ionic conductivity, thermal stability and chemical catalytic performance, and needs to have a high porosity to facilitate the passage of raw gas;

[0004] The support in the solid oxide battery needs to have high thermal stability and mechanical strength, as well as high porosity;

[0005] Traditional solid oxide batteries need to first prepare a support body to obtain a finished support body, and then make a functional layer on the surface of the support body. This method has the problem that the support body needs to be heated twice, resulting in a decrease in the pore size of the support body or a decrease in the open porosity, or the bonding strength between the functional layer and the support body is not high; and the functional layer has a problem of reduced catalytic activity during the sintering process.

[0006] Therefore, how to achieve high strength of the support body in the prepared solid oxide battery while having high porosity and high open area, high catalytic performance of the functional layer, and high bonding strength between the support body and the functional layer has become a difficult problem that needs to be solved urgently in this field. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a solid oxide battery support and a functional layer, so as to achieve high strength of the support in the solid oxide battery while having high porosity and high opening rate, high catalytic performance of the functional layer, and high bonding strength between the support and the functional layer.

[0008] In one aspect of the present invention, a method for preparing a solid oxide battery support and a functional layer is provided, comprising the following steps:

[0009] Prepare a support mud material, the support mud material includes NiO, (Y2O3) 0.03 -(ZrO2) 0.97 , pore-forming agent;

[0010] preparing a support body transition layer spray material, wherein the support body transition layer spray material includes a transition layer surface roughening agent;

[0011] Prepare a functional layer material slurry, wherein the functional layer material slurry is molten NiO-8YSZ;

[0012] Prepare a primary green body of a support body by using a support body clay material;

[0013] Spraying a support transition layer spray material on the surface of the support primary body to obtain a support secondary body;

[0014] Debinding the secondary support body to obtain a support body blank;

[0015] The support body blank is sintered to obtain a support body, wherein the support body comprises a support body transition layer with an uneven surface and a support body base layer connected to the support body transition layer; the roughness of the support body transition layer is Ra;

[0016] Spraying the functional layer material slurry onto the surface of the support body, and obtaining the functional layer combined with the support body after cooling, wherein the solid oxide battery comprises a support body and a functional layer; the functional layer is connected to the support body transition layer of the support body;

[0017] When the solid oxide battery is a forward power generation solid fuel cell SOFC, the functional layer of the solid oxide battery is the anode of the SOFC; taking the traditional NiO-3YSZ / 8YSZ / GDC / LSCF SOFC battery prepared by the solid oxide battery support and functional layer preparation method as an example, the power density can reach 0.5W / cm 2 Above, preferably, the power density can reach 1W / cm 2 above;

[0018] When the solid oxide battery is a reverse electrolysis solid oxide electrolytic cell SOEC, the functional layer of the solid oxide battery is the cathode of SOEC; a conventional NiO-3YSZ / 8YSZ / GDC / LSCF SOEC electrolytic cell is prepared according to the solid oxide battery support and functional layer preparation method, and the electrolysis current density can reach 0.48A / cm 2 Above, preferably, the electrolysis current density can reach 0.97A / cm 2 above.

[0019] The beneficial effect of the present invention over the prior art is that the material sprayed through the support transition layer includes a transition layer surface roughening agent, and the support transition layer sprayed material is sprayed on the surface of the support primary blank, so that the transition layer surface roughening agent is embedded in the uniform surface of the support primary blank; after the secondary blank of the support is debinded and subsequently sintered, the transition layer surface roughening agent is volatilized, so the support obtained after sintering includes a support transition layer with an uneven surface and a support base layer connected to the support transition layer; the support base layer is used to achieve high strength of the support, and the uneven surface of the support transition layer is conducive to subsequent connection with the functional layer, and the connection strength is high; and the transition layer is further conducive to improving the porosity and opening rate of the support; and this method achieves high surface roughness of the support and is simple to operate;

[0020] By spraying molten NiO-8YSZ onto the surface of the support body, a functional layer combined with the support body is obtained after cooling. The molten NiO-8YSZ is combined with the uneven transition layer, so that the functional layer has a high bonding strength, and at the same time avoids secondary sintering of the support body. The functional layer needs to be sintered for a long time, thereby avoiding the problem of reduced porosity and open porosity of the support body during the secondary sintering process, and avoiding the problem of reduced catalytic activity of the functional layer due to sintering; at the same time, the support body has high strength.

[0021] Further, the support body clay material includes a first support body clay material;

[0022] The first support body mud material includes NiO, (Y2O3) in a mass ratio of (55-65): (35-45): (5-15): (15-25) 0.03 -(ZrO2) 0.97 , pore-forming agent, first forming agent;

[0023] The first molding agent includes a binder, a plasticizer, and deionized water in a mass ratio of (20-30):(30-50):(30-50);

[0024] The binder includes one or more of polyacrylate, polyacrylamide, and carboxymethyl cellulose;

[0025] The plasticizer includes one of glycerol and polyethylene glycol.

[0026] The beneficial effect of adopting the previous step is that, through the clay pore-forming agent, the shaping agent and the addition amount in the first support, the strength of the support base layer is high, and at the same time, the porosity of the support base layer meets the requirements of the solid oxide battery, and at the same time, through the mass ratio of the binder, the plasticizer and the deionized water (20-30): (30-50): (30-50), the strength of the support primary blank or the support main body primary blank is high, which meets the requirement that the support main body primary blank will not be deformed or damaged when the support transition layer spraying material is subsequently sprayed, and there is no other change on the surface of the support primary blank except that the support transition layer spraying material is embedded in the surface of the support primary blank.

[0027] Furthermore, the support body clay material further includes a second support body clay material;

[0028] The support body mud also includes a second support body mud; the second support body mud includes NiO, (Y2O3) in a mass ratio of (55-65): (35-45): (20-25): (30-60) 0.03 -(ZrO2) 0.97 , pore-forming agent, second forming agent;

[0029] The second molding agent includes a binder, a plasticizer, and deionized water in a mass ratio of (15-25): (15-30): (60-100).

[0030] The beneficial effect of the above step is that the content of the pore-forming agent and the shaping agent in the second support body mud is higher than that in the first support body, so that the porosity of the support body portion after the primary green body of the support body connecting layer is sintered is higher than the porosity of the support body portion after the primary green body of the support body main body is sintered;

[0031] At the same time, the second molding agent includes a binder, a plasticizer, and deionized water in a mass ratio of (15-25): (15-30) (60-100), so that the hardness of the second support mud after molding is lower than the hardness of the first support mud after molding, thereby achieving the hardness of the support body connecting layer primary green body lower than the hardness of the support body main body primary green body, which is conducive to embedding the support body transition layer sprayed material into the support body connecting layer primary green body, and ultimately helps to achieve a high bonding strength between the support body and the functional layer after sintering.

[0032] Further, the surface roughening agent includes one or more of naphthalene, PMMA microspheres, PVB, starch, walnut powder, and graphite;

[0033] The D50 of the surface roughening agent particles is β; the ratio of Ra to β is 1:(1.5-2).

[0034] Preferably, the roughness Ra of the transition layer of the support body is 18-25 microns, and the D50 of the surface roughening agent particles is 27-50 microns.

[0035] The beneficial effect of the above step is that the surface roughening agent can be embedded in the surface of the primary support body during spraying, and can be volatilized during the subsequent debinding and sintering process, so that the surface of the support body obtained after sintering is uneven and the strength of the support body and other aspects except the surface roughness are not deformed;

[0036] The ratio of Ra to β through the support is about 1:(1.5-2), which is beneficial to controlling the roughness of the support surface.

[0037] Furthermore, the support body transition layer spray material also includes a transition layer binder, and the mass ratio of the transition layer binder to the surface roughening agent is (10-30): (50-80);

[0038] The transition layer binder is paraffin;

[0039] The preparation process of the support body transition layer spray material is as follows: the transition layer binder is heated to 47-50° C. to be in a liquid state, and then a surface roughening agent is added and mixed to obtain the support body transition layer spray material.

[0040] The beneficial effect of adopting the previous step is that the material sprayed through the support body transition layer also includes a transition layer binder, which is conducive to increasing the probability of the surface roughening agent being embedded in the surface of the support body primary blank, and avoiding a reduction in the strength of the support body after subsequent sintering or changes in other shapes of the support body except for the roughness of the outer surface.

[0041] Furthermore, the preparation process of the support secondary green body comprises the following steps:

[0042] When the primary support body is non-cylindrical, the primary support body is kept stationary during the spraying process;

[0043] When the primary support body is cylindrical, the primary support body rotates along the axis during the injection process;

[0044] The support transition layer spray material is sprayed onto the support primary body surface at an angle α to the non-cylindrical support primary body surface or the cylindrical support primary body surface tangent line, and adheres to or enters the support primary body surface.

[0045] The beneficial effect of adopting the previous step is that by spraying the support transition layer material at an angle α to the surface of the non-cylindrical support primary billet or the tangent of the cylindrical support primary billet onto the surface of the support primary billet, it is beneficial to achieve that the surface roughening agent enters the surface of the support primary billet at an angle, that is, it is beneficial to avoid that after sintering, the support body has no changes except for the change in surface roughness. At the same time, after subsequent debinding and volatilization, the axis of the cavity formed on the surface of the support body is not perpendicular to the non-cylindrical support body surface, and the axis of the cavity formed is not perpendicular to the tangent of the cylindrical support body surface; that is, inclined cavities are formed on the surface of the support body, thereby significantly improving the bonding strength between the functional layer and the support body.

[0046] Further, the first support body clay material is extruded to obtain the support body primary green body; or, the first support body clay material and the second support body clay material are simultaneously extruded to obtain the support body primary green body;

[0047] The support body primary green body comprises a support body main body primary green body and a support body connecting layer primary green body located on the surface of the support body main body primary green body;

[0048] The first support body clay material is extruded to form a support body main body primary green body; the second support body clay material is extruded to form a support body connecting layer primary green body;

[0049] The sprayed material of the support body transition layer adheres to or enters the surface of the primary green body of the support body connecting layer.

[0050] Further, the angle α=15-90°, preferably the angle α=15-45°;

[0051] The injection pressure of the support transition layer injection material is 0.04MPa-0.1MPa;

[0052] The distance between the ejection outlet of the support body transition layer ejection material and the surface of the support body primary blank is 20-100 mm.

[0053] The beneficial effect of adopting the previous step is that it is conducive to achieving an uneven surface of the support body obtained after sintering, and the strength of the support body and other aspects except the surface roughness do not deform; and at the same time, the bonding strength between the support body and the functional layer is high.

[0054] Furthermore, the process of debinding the secondary support body is to heat the secondary support body, and the heating process is to heat the secondary support body to 90-105°C at a heating rate of 9-10°C / min; and to heat the secondary support body from 90-105°C to 180-200°C at a heating rate of 5-6°C / min;

[0055] The temperature is increased from 180-200°C to 330-360°C at a rate of 3-4°C / min.

[0056] The beneficial effect of the above step is that by heating to 90-105°C at a heating rate of 9-10°C / min, it is beneficial to achieve rapid volatilization of small molecular volatiles in the secondary green body of the support body, forming openings with small pore sizes, and there will be no problems such as cracking or deformation of the secondary green body of the support body;

[0057] By heating from 90-105°C to 180-200°C at a heating rate of 5-6°C / min; and from 180-200°C to 330-360°C at a heating rate of 3-4°C / min, it is beneficial to achieve slow decomposition of volatiles with larger molecular weight, and slow volatilization based on small-aperture through holes generated by volatilization of small molecules, and the pore size gradually increases, avoiding cracking or deformation of the secondary green body of the support during the sintering process.

[0058] Furthermore, during the sintering process of the support body green body, the sintering temperature is 1100-1350° C. and the heat preservation time is 2-3 hours.

[0059] The beneficial effect of adopting the previous step is that it is conducive to achieving the strength of the support body, while helping to avoid the reduction of the porosity and open porosity of the support body; and it is also conducive to improving the activity of the functional layer. DETAILED DESCRIPTION

[0060] In order to better understand the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments.

[0061] Embodiment 1:

[0062] This embodiment provides a method for preparing a solid oxide battery support and a functional layer, comprising the following steps:

[0063] Prepare a support mud material, the support mud material includes NiO, (Y2O3) 0.03 -(ZrO2) 0.97 , pore-forming agent;

[0064] The support body mud is a first support body mud; the first support body mud includes NiO, (Y2O3) in a mass ratio of 60:40:10:20 0.03 -(ZrO2) 0.97 , pore-forming agent, first forming agent;

[0065] The first molding agent includes a binder, a plasticizer, and deionized water in a mass ratio of 25:40:40;

[0066] The binder includes polyacrylate; and the plasticizer includes glycerol.

[0067] preparing a support body transition layer spray material, wherein the support body transition layer spray material includes a transition layer surface roughening agent;

[0068] The surface roughening agent includes PMMA microspheres and PVB; the roughness Ra of the transition layer of the support is 21 microns, and the D50 of the surface roughening agent particles is 39 microns.

[0069] Prepare a functional layer material slurry, wherein the functional layer material slurry is molten NiO-8YSZ;

[0070] Prepare a primary green body of a support body by using a support body clay material;

[0071] The first support body clay material is extruded to obtain the support body primary body; a support body transition layer spray material is sprayed on the surface of the support body primary body to obtain a support body secondary body;

[0072] The preparation process of the support secondary green body comprises the following steps:

[0073] The primary support body is cylindrical, and the primary support body rotates along the axis during the injection process;

[0074] The spraying direction of the support transition layer spray material forms an angle α with the tangent line of the cylindrical support primary body surface and sprays it onto the support primary body surface, and adheres to or enters the support primary body surface; wherein α=30°;

[0075] The injection pressure of the support body transition layer injection material is 0.07 MPa; the distance between the injection outlet of the support body transition layer injection material and the surface of the support body primary blank is 60 mm.

[0076] Debinding the secondary support body to obtain a support body blank;

[0077] The process of debinding the secondary support body is to heat the secondary support body, and the heating process is to heat the secondary support body to 98°C at a heating rate of 9.5°C / min; and to heat the secondary support body from 98°C to 190°C at a heating rate of 5.5°C / min;

[0078] The temperature was increased from 190°C to 345°C at a rate of 3.5°C / min.

[0079] The support body blank is sintered to obtain a support body, which includes a support body transition layer with an uneven surface and a support body base layer connected to the support body transition layer; the roughness of the support body transition layer is Ra; during the sintering process of the support body blank, the sintering temperature is 1225°C and the insulation time is 2.5h.

[0080] Spraying the functional layer material slurry onto the surface of the support body, and obtaining the functional layer combined with the support body after cooling, wherein the solid oxide battery comprises a support body and a functional layer; the functional layer is connected to the support body transition layer of the support body;

[0081] The solid oxide battery is a reverse electrolytic solid oxide electrolytic cell SOEC, and the functional layer of the solid oxide battery is the cathode of SOEC; a conventional NiO-3YSZ / 8YSZ / GDC / LSCF SOEC electrolytic cell is prepared according to the solid oxide battery support and functional layer preparation method, and the electrolysis current density can reach 0.99A / cm 2 .

[0082] Embodiment 2:

[0083] The same contents as those in Example 1 are not described in detail here. The differences between this embodiment and Example 1 are as follows:

[0084] This embodiment provides a method for preparing a solid oxide battery support and a functional layer, which also includes the following steps:

[0085] The support body mud material further includes a second support body mud material;

[0086] The support body mud also includes a second support body mud; the second support body mud includes NiO, (Y2O3) in a mass ratio of 58:38:24:58 0.03 -(ZrO2) 0.97 , pore-forming agent, second forming agent;

[0087] The second molding agent includes a binder, a plasticizer, and deionized water in a mass ratio of 18:18:90.

[0088] The first support body clay material and the second support body clay material are simultaneously extruded to obtain the support body primary green body;

[0089] The support body primary green body comprises a support body main body primary green body and a support body connecting layer primary green body located on the surface of the support body main body primary green body;

[0090] The first support body clay material is extruded to form a support body main body primary green body; the second support body clay material is extruded to form a support body connecting layer primary green body;

[0091] The sprayed material of the support body transition layer adheres to or enters the surface of the primary green body of the support body connecting layer.

[0092] The primary support body is in a plate shape, and the primary support body remains stationary during the spraying process;

[0093] The support transition layer spray material is sprayed onto the surface of the support primary blank at an angle of α to the surface of the plate-shaped support primary blank, and adheres to or enters the surface of the support primary blank; wherein α=18°.

[0094] The injection pressure of the support body transition layer injection material is 0.08MPa;

[0095] The distance between the ejection outlet of the support body transition layer ejection material and the surface of the support body primary blank is 30 mm.

[0096] The support body mud is the first support body mud; the first support body mud includes NiO, (Y2O3) in a mass ratio of 63:43:8:18 0.03 -(ZrO2) 0.97 , pore-forming agent, first forming agent;

[0097] The first molding agent includes a binder, a plasticizer, and deionized water in a mass ratio of 28:48:48;

[0098] The binder includes polyacrylamide; and the plasticizer includes polyethylene glycol.

[0099] The surface roughening agent includes PVB and starch; the roughness Ra of the transition layer of the support is 24 microns, and the D50 of the surface roughening agent particles is 48 microns.

[0100] The process of debinding the secondary support body is to heat the secondary support body, and the heating process is to heat the secondary support body to 103°C at a heating rate of 9.8°C / min; and to heat the secondary support body from 103°C to 195°C at a heating rate of 5.8°C / min;

[0101] The temperature was increased from 195°C to 350°C at a rate of 3.8°C / min.

[0102] During the sintering process of the support body green body, the sintering temperature is 1330° C. and the heat preservation time is 2.2 h.

[0103] The solid oxide battery is a forward power generation solid fuel cell SOFC, and the functional layer of the solid oxide battery is the anode of the SOFC; taking the traditional NiO-3YSZ / 8YSZ / GDC / LSCF SOFC battery prepared by the solid oxide battery support and functional layer preparation method as an example, the power density can reach 1.1W / cm 2 .

[0104] Embodiment 3:

[0105] The same contents as those in Example 1 are not described in detail here. The differences between this embodiment and Example 1 are as follows:

[0106] This embodiment provides a method for preparing a solid oxide battery support and a functional layer, which also includes the following steps:

[0107] The support body mud material further includes a second support body mud material;

[0108] The support body mud also includes a second support body mud; the second support body mud includes NiO, (Y2O3) in a mass ratio of 62:43:22:35 0.03 -(ZrO2) 0.97 , pore-forming agent, second forming agent;

[0109] The second molding agent includes a binder, a plasticizer, and deionized water in a mass ratio of 22:28:70.

[0110] The first support body clay material and the second support body clay material are simultaneously extruded to obtain the support body primary green body;

[0111] The support body primary green body comprises a support body main body primary green body and a support body connecting layer primary green body located on the surface of the support body main body primary green body;

[0112] The first support body clay material is extruded to form a support body main body primary green body; the second support body clay material is extruded to form a support body connecting layer primary green body;

[0113] The sprayed material of the support body transition layer adheres to or enters the surface of the primary green body of the support body connecting layer.

[0114] The support body transition layer spray material also includes a transition layer binder, the mass ratio of the transition layer binder to the surface roughening agent is 20:65; the transition layer binder is paraffin;

[0115] The preparation process of the support body transition layer spray material is as follows: the transition layer binder is heated to 49° C. to be in a liquid state, and then a surface roughening agent is added and mixed to obtain the support body transition layer spray material.

[0116] The primary support body is in a plate shape, and the primary support body remains stationary during the spraying process;

[0117] The spraying direction of the support transition layer spray material is at an angle of α to the surface of the plate-shaped support primary blank, and the spray material adheres to or enters the surface of the support primary blank; the 43°;

[0118] The injection pressure of the support body transition layer injection material is 0.05;

[0119] The distance between the ejection outlet of the support body transition layer ejection material and the surface of the support body primary blank is 80 mm.

[0120] The support body mud is the first support body mud; the first support body mud includes NiO, (Y2O3) in a mass ratio of 58:38:8:18 0.03 -(ZrO2) 0.97 , pore-forming agent, first forming agent;

[0121] The first molding agent includes a binder, a plasticizer, and deionized water in a mass ratio of 22:32:32;

[0122] The binder includes polyacrylate and polyacrylamide; the plasticizer includes.

[0123] The surface roughening agent includes PMMA microspheres; the D50 of the surface roughening agent particles is β; the ratio of Ra to β is 1:(1.5-2); the roughness of the support transition layer is Ra of 19 microns, and the D50 of the surface roughening agent particles is 36 microns.

[0124] The process of debinding the secondary support body is to heat the secondary support body, and the heating process is to heat the secondary support body to 93°C at a heating rate of 9.2°C / min; and to heat the secondary support body from 93°C to 185°C at a heating rate of 5.2°C / min;

[0125] The temperature was increased from 185°C to 335°C at a rate of 3.2°C / min.

[0126] During the sintering process of the support body green body, the sintering temperature is 1180° C. and the heat preservation time is 2.8 h.

[0127] The solid oxide battery is a forward power generation solid fuel cell SOFC, and the functional layer of the solid oxide battery is the anode of the SOFC; taking the traditional NiO-3YSZ / 8YSZ / GDC / LSCF SOFC battery prepared by the solid oxide battery support and functional layer preparation method as an example, the power density can reach 1.2W / cm 2 .

[0128] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features have similar functions to those disclosed in the present application (but not limited to).

Claims

1. A method for preparing a solid oxide battery support and a functional layer, It is characterized in that The following steps are involved: Prepare a support mud material, the support mud material includes NiO, (Y 2 O 3 ) 0.03 -(ZrO 2 ) 0.97 , pore-forming agent; preparing a support body transition layer spray material, wherein the support body transition layer spray material includes a transition layer surface roughening agent; Prepare a functional layer material slurry, wherein the functional layer material slurry is molten NiO-8YSZ; Prepare a primary green body of a support body by using a support body clay material; Spraying a support transition layer spray material on the surface of the support primary body to obtain a support secondary body; Debinding the secondary support body to obtain a support body blank; The support body blank is sintered to obtain a support body, wherein the support body comprises a support body transition layer with an uneven surface and a support body base layer connected to the support body transition layer; the roughness of the support body transition layer is Ra; The functional layer material slurry is sprayed onto the surface of the support body, and after cooling, a functional layer combined with the support body is obtained. The solid oxide battery includes a support body and a functional layer; the functional layer is connected to the support body transition layer of the support body.

2. The method for preparing a solid oxide battery support and a functional layer according to claim 1, It is characterized in that The support body mud material includes a first support body mud material; The first support body mud material includes NiO, (Y 2 O 3 ) 0.03 -(ZrO 2 ) 0.97 , pore-forming agent, first forming agent; The first molding agent includes a binder, a plasticizer, and deionized water in a mass ratio of (20-30):(30-50):(30-50); The binder includes one or more of polyacrylate, polyacrylamide, and carboxymethyl cellulose; The plasticizer includes one of glycerol and polyethylene glycol.

3. The method for preparing a solid oxide battery support and a functional layer according to claim 2, It is characterized in that The support body mud material further includes a second support body mud material; The second support body mud material includes NiO, (Y 2 O 3 ) 0.03 -(ZrO 2 ) 0.97 , pore-forming agent, second forming agent; The second molding agent includes a binder, a plasticizer, and deionized water in a mass ratio of (15-25): (15-30): (60-100).

4. The method for preparing a solid oxide battery support and a functional layer according to claim 1, It is characterized in that The surface roughening agent includes one or more of naphthalene, PMMA microspheres, PVB, starch, walnut powder, and graphite; The D50 of the surface roughening agent particles is β; the ratio of Ra to β is about 1:(1.5-2). Preferably, the roughness Ra of the transition layer of the support body is 18-25 microns, and the D50 of the surface roughening agent particles is 27-50 microns.

5. The method for preparing a solid oxide battery support and a functional layer according to claim 4, It is characterized in that The support body transition layer spray material also includes a transition layer binder, and the mass ratio of the transition layer binder to the surface roughening agent is (10-30): (50-80); The transition layer binder is paraffin; The preparation process of the support body transition layer spray material is as follows: the transition layer binder is heated to 47-50° C. to be in a liquid state, and then a surface roughening agent is added and mixed to obtain the support body transition layer spray material.

6. The method for preparing a solid oxide battery support and a functional layer according to claim 3, It is characterized in that The preparation process of the support secondary green body comprises the following steps: When the primary support body is non-cylindrical, the primary support body is kept stationary during the spraying process; When the primary support body is cylindrical, the primary support body rotates along the axis during the injection process; The support transition layer spray material is sprayed onto the support primary body surface at an angle α to the non-cylindrical support primary body surface or the cylindrical support primary body surface tangent line, and adheres to or enters the support primary body surface.

7. The method for preparing a solid oxide battery support and a functional layer according to claim 3, It is characterized in that The first support body clay material is formed by extrusion to obtain the support body primary green body; or The first support body clay material and the second support body clay material are simultaneously extruded to obtain the support body primary green body; The support body primary green body comprises a support body main body primary green body and a support body connecting layer primary green body located on the surface of the support body main body primary green body; The first support body clay material is extruded to form a support body main body primary green body; the second support body clay material is extruded to form a support body connecting layer primary green body; The sprayed material of the support body transition layer adheres to or enters the surface of the primary green body of the support body connecting layer.

8. The method for preparing a solid oxide battery support and a functional layer according to claim 3, It is characterized in that The α=15-90°, preferably the α=15-45°; The injection pressure of the support transition layer injection material is 0.04MPa-0.1MPa; The distance between the ejection outlet of the support body transition layer ejection material and the surface of the support body primary blank is 20-100 mm.

9. The method for preparing a solid oxide battery support and a functional layer according to claim 3, It is characterized in that The process of debinding the secondary support body is to heat the secondary support body, and the heating process is to heat the secondary support body to 90-105°C at a heating rate of 9-10°C / min; from 90-105°C to 180-200°C at a heating rate of 5-6°C / min; from 180-200°C to 330-360°C at a heating rate of 3-4°C / min.

10. The method for preparing a solid oxide battery support and a functional layer according to claim 3, It is characterized in that During the sintering process of the support body green body, the sintering temperature is 1100-1350° C. and the heat preservation time is 2-3 hours.

Citation Information

Patent Citations

  • Metal support half-cell of solid oxide fuel cell and preparation method thereof

    CN103928693A

  • Method for manufacturing fuel electrode support for solid oxide fuel cell and fuel electrode support for solid oxide fuel cell

    CN105493328A

  • Method for manufacturing a film on a support having a non-flat surface

    CN111295743A

Cited By

  • Metal support type solid oxide electrolytic cell substrate and preparation process thereof

    CN121381004A

  • Metal support type solid oxide electrolysis cell substrate and process for making same

    CN121381004B