Organic compound and application thereof
By introducing B-N resonant organic compounds with imidazole groups into organic electroluminescent devices, the problem of low utilization efficiency of triplet excitons is solved, and efficient yellow and green light emission is achieved, which meets high performance and low cost Require.
Patent Information
- Application Number
- CN202310599438.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
Existing organic electroluminescent devices have low efficiency when using triplet excitons, making it difficult to effectively improve luminescence efficiency. Especially in the field of blue and yellow luminescence, the external quantum efficiency of traditional fluorescent materials is limited, and the cost of phosphorescent materials is high.
A B-N resonant organic compound containing imidazole groups was designed to adjust the emission wavelength through C-B and N-B bonds, improve carrier transmission performance and luminous efficiency, and is applied to organic electroluminescent devices.
It achieves a higher luminous efficiency and better service life, especially in the emission of yellow and green light, which meets the needs of high-performance materials and is relatively low in cost.
Smart Images

Figure CN119019429A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an organic compound, belonging to the technical field of organic electroluminescence. The present invention specifically discloses a BN resonance type organic compound, and the present invention also relates to the application of such organic compound and an organic electroluminescent device using such organic compound. Background Art
[0002] In recent years, optoelectronic devices based on organic materials have become increasingly popular. The inherent flexibility of organic materials makes them very suitable for manufacturing on flexible substrates. Beautiful and cool optoelectronic products can be designed and produced according to demand, gaining unparalleled advantages over inorganic materials. Examples of such organic optoelectronic devices include organic light-emitting diodes (OLEDs), organic field-effect transistors, organic photovoltaic cells, organic sensors, etc. Among them, OLED has developed particularly rapidly and has achieved commercial success in the field of information display. OLED can provide highly saturated red, green, and blue colors. Full-color display devices made of OLEDs do not require additional backlight sources and have the advantages of brilliant colors, lightness, thinness, and softness.
[0003] The core of OLED devices is a thin film structure containing a variety of organic functional materials. Common functionalized organic materials include: hole injection materials, hole transport materials, hole blocking materials, electron injection materials, electron transport materials, electron blocking materials, luminescent host materials and luminescent guest (dyes), etc. When power is turned on, electrons and holes are injected and transported to the luminescent area respectively and recombine there, thereby generating excitons and emitting light.
[0004] People have developed a variety of organic materials, combined with various unique device structures, which can improve carrier mobility, regulate carrier balance, break through electroluminescence efficiency, and delay device attenuation. For quantum mechanical reasons, common fluorescent luminescent bodies mainly use singlet excitons generated when electrons and holes combine to emit light, and are still widely used in various OLED products. Some metal complexes, such as iridium complexes, can simultaneously use triplet excitons and singlet excitons to emit light, and are called phosphorescent luminescent bodies. Their energy conversion efficiency can be increased by up to four times that of traditional fluorescent luminescent bodies. Thermally excited delayed fluorescence (TADF) technology promotes the transformation of triplet excitons to singlet excitons. Without the use of metal complexes, triplet excitons can still be effectively utilized to achieve higher luminescence efficiency. Thermally excited sensitized fluorescence (TASF) technology uses materials with TADF properties to sensitize luminescent bodies by energy transfer, which can also achieve higher luminescence efficiency. Especially in the field of blue luminescence, which has always been difficult to effectively improve luminescence efficiency, it has a very broad application prospect.
[0005] Under the condition of electrical excitation, organic electroluminescent devices will produce 25% singlet and 75% triplet excitons. Traditional fluorescent materials can only use 25% of singlet excitons due to spin prohibition, so the external quantum efficiency is limited to less than 5%. Almost all triplet excitons can only be lost in the form of heat. In order to improve the efficiency of organic electroluminescent devices, triplet excitons must be fully utilized.
[0006] To this end, researchers have proposed many methods, the most notable of which is the use of phosphorescent materials. Phosphorescent materials introduce heavy atoms and have a spin-orbit coupling effect, which can fully utilize 75% of triplet excitons and achieve 100% internal quantum efficiency. However, phosphorescent materials use rare heavy metals, which makes the materials expensive and not conducive to cost control. If fluorescent devices can make good use of triplet excitons, this problem can be solved well. Researchers have proposed a method to improve the efficiency of fluorescent devices by quenching triplet excitons to produce singlet excitons in fluorescent devices, but the maximum external quantum efficiency that this method can theoretically achieve is only 62.5%, which is much lower than that of phosphorescent materials. Therefore, it is very necessary to find new technologies to make full use of the triplet energy levels of fluorescent materials to improve the luminescence efficiency.
[0007] In recent years, new π-conjugated organic unit materials containing organic boron and nitrogen co-embedded have become a research hotspot of OLED material systems due to their good photophysical and electrochemical properties. The present invention introduces imidazole groups in this material system. Imidazole has both acidity and alkalinity and is a bipolar compound. Its application in OLED materials is conducive to improving the transport performance of carriers, balancing carrier recombination, and improving luminous efficiency. At the same time, the emission wavelength can be adjusted according to the formation of CB and NB bonds with boron atoms at different sites in imidazole to achieve green to yellow light emission, covering a wider range of light colors, and more flexible molecular structure adjustment. It can be applied to devices to achieve purer chromaticity and higher efficiency than traditional dyes. Summary of the invention
[0008] Through in-depth research, the researchers of the present invention proposed a new molecular design scheme, and obtained a compound with more balanced luminous efficiency and life span characteristics.
[0009] Specifically, the present invention provides an organic compound having a structure shown in formula (1) or formula (2):
[0010]
[0011] In the general formula (1) and the formula (2), X1, X2, X3, and X4 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted C1-C20 silyl, substituted or unsubstituted C6-C60 aryl, substituted or unsubstituted C3-C60 heteroaryl, substituted or unsubstituted C6-C60 arylamine, and substituted or unsubstituted C3-C60 heteroarylamine; two adjacent ones of X1, X2, X3, and X4 may be connected to form a ring or not;
[0012] Y1, Y2, Y3, Y4, Y5, Y6, and Y7 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted C1-C20 silyl, substituted or unsubstituted C6-C60 aryl, substituted or unsubstituted C3-C60 heteroaryl, substituted or unsubstituted C6-C60 arylamine, and substituted or unsubstituted C3-C60 heteroarylamine; two adjacent ones of Y1, Y2, Y3, Y4, Y5, Y6, and Y7 may be connected to form a ring or not;
[0013] Z1, Z2, and Z3 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted C1-C20 silyl, substituted or unsubstituted C6-C60 aryl, substituted or unsubstituted C3-C60 heteroaryl, substituted or unsubstituted C6-C60 arylamine, and substituted or unsubstituted C3-C60 heteroarylamine; two adjacent Z1, Z2, and Z3 may be connected to form a ring or not;
[0014] The substituents substituted in X1, X2, X3, X4, Y1, Y2, Y3, Y4, Y5, Y6, Y7, Z1, Z2, and Z3 are each independently selected from any one of halogen, cyano, nitro, hydroxyl, amino, C1-C20 chain alkyl, C3-C20 cycloalkyl, C2-C20 alkenyl, C1-C20 alkoxy, C1-C20 silyl, C6-C60 arylamine, C3-C60 heteroarylamine, C6-C30 aryloxy, C3-C30 heteroaryloxy, C6-C60 aryl, and C3-C60 heteroaryl. A combination of at least two.
[0015] In the present invention, the "substituted or unsubstituted" group may be substituted with one substituent or with multiple substituents. When there are multiple substituents, they may be selected from different substituents. When the same expressions are involved in the present invention, they all have the same meaning, and the selection range of substituents is as shown above and will not be repeated one by one.
[0016] In the present specification, the expression of Ca to Cb represents that the number of carbon atoms in the group is a to b. Unless otherwise specified, the number of carbon atoms generally does not include the number of carbon atoms in the substituent.
[0017] In the present specification, the expression of a ring structure crossed by “—” indicates that the connection site is any position on the ring structure that can form a bond.
[0018] In the present specification, “each independently” means that when there are multiple subjects, they may be the same as or different from each other.
[0019] In the present invention, the expression of chemical elements, unless otherwise specified, generally includes the concept of isotopes thereof. For example, the expression "hydrogen (H)" includes its isotopes. 1 H (hydrogen or H), 2 The concept of H (deuterium or D); carbon (C) includes 12 C. 13 C, etc., no further details.
[0020] The heteroatom in the present invention generally refers to an atom or an atom group selected from N, O, S, P, Si and Se, preferably selected from N, O, S and Se.
[0021] In the present specification, examples of halogen include fluorine, chlorine, bromine, and iodine.
[0022] In the present invention, unless otherwise specified, aryl and heteroaryl include both monocyclic and condensed ring forms.
[0023] In the present invention, the C6-C60 can be C6, C9, C10, C12, C14, C16, C18, C20, C22, C24, C26, C28, C30, C32, C34, C36, C38, C40, C42, C44, C46, C48, C50, C52, C54, C56 or C58, etc.
[0024] The C3~C60 can all be C3, C4, C5, C6, C9, C10, C12, C14, C16, C18, C20, C22, C24, C26, C28, C30, C32, C34, C36, C38, C40, C42, C44, C46, C48, C50, C52, C54, C56 or C58, etc.
[0025] The C1-C20 can all be C2, C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18 or C19, etc.
[0026] The C3~C20 can all be C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18 or C19, etc.
[0027] The C6 to C30 can all be C6, C9, C10, C12, C14, C16, C18, C20, C22, C24, C26 or C28, etc.
[0028] The C3~C30 can all be C3, C4, C5, C6, C9, C10, C12, C14, C16, C18, C20, C22, C24, C26 or C28, etc.
[0029] The C2 to C10 can all be C2, C3, C4, C5, C6, C7, C8, C9 or C10.
[0030] In the present invention, the substituted or unsubstituted C6-C60 aryl group includes a monocyclic aryl group and a condensed aryl group, preferably a C6-C30 aryl group, and more preferably a C6-C20 aryl group. The so-called monocyclic aryl group refers to a molecule containing at least one phenyl group. When the molecule contains at least two phenyl groups, the phenyl groups are independent of each other and connected by a single bond, such as: phenyl, biphenyl, terphenyl, etc. Specifically, the biphenyl group includes 2-biphenyl, 3-biphenyl and 4-biphenyl; the terphenyl group includes p-terphenyl-4-yl, p-terphenyl-3-yl, p-terphenyl-2-yl, m-terphenyl-4-yl, m-terphenyl-3-yl and m-terphenyl-2-yl. A condensed aryl group refers to a molecule containing at least two aromatic rings, and the aromatic rings are not independent of each other but share two adjacent carbon atoms to condense each other. For example, naphthyl, anthracenyl, phenanthrenyl, indenyl, fluorenyl, fluoranthenyl, triphenylene, pyrenyl, peryl, The naphthyl group includes 1-naphthyl or 2-naphthyl; the anthracenyl group is selected from 1-anthracenyl, 2-anthracenyl and 9-anthracenyl; the fluorenyl group is selected from 1-fluorenyl, 2-fluorenyl, 3-fluorenyl, 4-fluorenyl and 9-fluorenyl; the pyrenyl group is selected from 1-pyrenyl, 2-pyrenyl and 4-pyrenyl; the naphthacenyl group is selected from 1-naphthacenyl, 2-naphthacenyl and 9-naphthacenyl. The fluorene derivative group is selected from 9,9-dimethylfluorenyl, 9,9-diethylfluorenyl, 9,9-dipropylfluorenyl, 9,9-dibutylfluorenyl, 9,9-dipentylfluorenyl, 9,9-dihexylfluorenyl, 9,9-diphenylfluorenyl, 9,9-dinaphthylfluorenyl, 9,9'-spirobifluorene and benzofluorenyl.
[0031] The C3-C60 heteroaryl mentioned in the present invention includes monocyclic heteroaryl and condensed ring heteroaryl, preferably C3-C30 heteroaryl, more preferably C4-C20 heteroaryl, and more preferably C5-C12 heteroaryl. A monocyclic heteroaryl refers to a molecule containing at least one heteroaryl. When the molecule contains one heteroaryl and other groups (such as aryl, heteroaryl, alkyl, etc.), the heteroaryl and other groups are independent of each other and connected by a single bond. Examples of monocyclic heteroaryl include furanyl, thienyl, pyrrolyl, pyridyl, etc. A condensed ring heteroaryl refers to a molecule containing at least one aromatic heterocycle and one aromatic ring (aromatic heterocycle or aromatic ring), and the two are not independent of each other but share two adjacent atoms and are fused to each other. Examples of fused ring heteroaryl groups include benzofuranyl, benzothiophenyl, indolyl, dibenzofuranyl, dibenzothiophenyl, carbazolyl, acridinyl, isobenzofuranyl, isobenzothiophenyl, benzocarbazolyl, azacarbazolyl, phenothiazinyl, phenazinyl, 9-phenylcarbazolyl, 9-naphthylcarbazolyl, dibenzocarbazolyl, indolocarbazolyl and the like.
[0032] The chain alkyl mentioned in the present invention, unless otherwise specified, includes straight chain alkyl and branched chain alkyl. Specifically, the substituted or unsubstituted C1-C30 chain alkyl is preferably a substituted or unsubstituted C1-C16 chain alkyl, and more preferably a substituted or unsubstituted C1-C10 chain alkyl. The substituted or unsubstituted C1-C10 chain alkyl includes, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, 2-methylbutyl, n-pentyl, sec-pentyl, neopentyl, n-hexyl, neohexyl, n-heptyl, n-octyl, 2-ethylhexyl, etc.
[0033] In the present invention, the cycloalkyl group includes monocycloalkyl and polycycloalkyl; wherein the monocycloalkyl group refers to an alkyl group containing a single cyclic structure; the polycycloalkyl group refers to a structure composed of two or more cycloalkyl groups sharing one or more carbon atoms on the ring; the C3-C20 cycloalkyl group can be exemplified by cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, adamantyl, etc.
[0034] In the present specification, the substituted or unsubstituted C1~C20 alkoxy group is preferably a substituted or unsubstituted C1~C10 alkoxy group. Examples of C1~C10 alkoxy groups include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, sec-butoxy, isobutoxy, tert-butoxy, pentyloxy, isopentyloxy, hexyloxy, heptyloxy, octyloxy, nonyloxy, decyloxy, undecyloxy, dodecyloxy and the like. Among them, methoxy, ethoxy, n-propoxy, isopropoxy, tert-butoxy, sec-butoxy, isobutoxy and isopentyloxy are preferred, and methoxy is more preferred.
[0035] In the present specification, as the substituted or unsubstituted C1~C20 silyl group, as the substituted or unsubstituted C1~C10 silyl group, examples of the C1~C10 silyl group can be a silyl group substituted by the groups listed in the above-mentioned C1~C10 alkyl group, specifically including: methylsilyl, dimethylsilyl, trimethylsilyl, ethylsilyl, diethylsilyl, triethylsilyl, tert-butyldimethylsilyl, tert-butyldiphenylsilyl and the like groups.
[0036] In the present specification, the C2~C20 alkenyl group is a hydrocarbon group containing at least one C=C double bond, and illustratively includes but is not limited to: vinyl, propenyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, butadienyl, pentadienyl and the like.
[0037] It should be noted that, for the sake of convenience, the possible effects of each group / feature are described separately in this application, but this does not mean that these groups / features act in isolation. In fact, the reason for obtaining good performance is essentially the optimized combination of the entire molecule, which is the result of the synergistic effect between the various groups, rather than the effect of a single group.
[0038] Furthermore, in the above general formula, preferably, X1, X2, X3, and X4 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C10 chain alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C3-C10 cycloalkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, substituted or unsubstituted C6-C30 arylamine, and substituted or unsubstituted C3-C30 heteroarylamine; two adjacent ones of X1, X2, X3, and X4 may be connected to form a ring or not;
[0039] The substituents in X1, X2, X3, and X4 are each independently selected from any one or a combination of at least two of halogen, C1-C10 chain alkyl, C3-C10 cycloalkyl, C2-C10 alkenyl, C1-C10 alkoxy, C6-C30 aryl, and C3-C30 heteroaryl;
[0040] More preferably, X1, X2, X3, and X4 are each independently selected from one or a combination of at least two of hydrogen, C1-C10 chain alkyl, C2-C10 alkenyl, C3-C10 cycloalkyl, C1-C10 alkoxy, C6-C30 aryl, and C3-C30 heteroaryl;
[0041] More preferably, X2 and X3 are each independently selected from hydrogen, methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, cyclopentyl, cyclohexyl, tert-butyl, 2-methylbutyl, pentyl, vinyl, propenyl, butenyl, butadienyl, phenyl, biphenyl, naphthyl, anthracenyl, phenanthrenyl, indenyl, fluorenyl, fluoranthenyl, triphenylene, pyrenyl, peryl, The invention can be selected from the group consisting of benzofuranyl, benzothiophenyl, isobenzofuranyl, isobenzothiophenyl, dibenzofuranyl, dibenzothiophenyl, indolyl, N-phenylindolyl, diphenylamine, carbazolyl, acridinium, imidazolyl and benzimidazolyl, or a combination of at least two of the following:
[0042] Furthermore, in the above general formula, preferably, Y1, Y2, Y3, Y4, Y5, Y6, and Y7 are each independently selected from hydrogen, substituted or unsubstituted C1-C10 chain alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C3-C10 cycloalkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, substituted or unsubstituted C6-C30 arylamine, substituted or unsubstituted one of substituted C3-C30 heteroarylamine groups; two adjacent ones of Y1, Y2, Y3, Y4, Y5, Y6, and Y7 are connected to form a ring or are not connected to form a ring; the substituents substituted in Y1, Y2, Y3, Y4, Y5, Y6, and Y7 are independently selected from any one of halogen, C1-C10 chain alkyl, C3-C10 cycloalkyl, C2-C10 alkenyl, C1-C10 alkoxy, C6-C30 aryl, and C3-C30 heteroaryl, or a combination of at least two thereof;
[0043] More preferably, Y2 and Y5 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C10 chain alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C3-C10 cycloalkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, substituted or unsubstituted C6-C30 arylamine, substituted or unsubstituted C3-C30 heteroarylamine; the substituents in Y2 and Y5 are each independently selected from any one of halogen, C1-C10 chain alkyl, C3-C10 cycloalkyl, C1-C10 alkoxy, C6-C30 aryl, C3-C30 heteroaryl, or a combination of at least two thereof;
[0044] Continuing to be preferred, Y2 and Y5 are each independently selected from one or a combination of at least two of hydrogen, C1-C10 chain alkyl, C2-C10 alkenyl, C3-C10 cycloalkyl, C1-C10 alkoxy, C6-C30 aryl, C3-C30 heteroaryl, C6-C30 arylamine, and C3-C30 heteroarylamine;
[0045] More preferably, Y2 and Y5 are each independently selected from hydrogen, methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, tert-butyl, 2-methylbutyl, pentyl, vinyl, propenyl, butenyl, butadienyl, cyclopentyl, cyclohexyl, phenyl, biphenyl, naphthyl, anthracenyl, phenanthrenyl, indenyl, fluorenyl, fluoranthenyl, triphenylene, pyrenyl, peryl, The invention can be selected from the group consisting of phenyl, tetraphenyl, furanyl, thienyl, pyridyl, carbazolyl, benzofuranyl, benzothienyl, isobenzofuranyl, isobenzothienyl, dibenzofuranyl, dibenzothienyl, indolyl, N-phenylindolyl, diphenylamino, acridinyl, imidazolyl, and benzimidazolyl, or a combination of at least two thereof.
[0046] Furthermore, in the above general formula, preferably, Z1, Z2, and Z3 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C10 chain alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C3-C10 cycloalkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, substituted or unsubstituted C6-C30 arylamine, and substituted or unsubstituted C3-C30 heteroarylamine; two adjacent Z1, Z2, and Z3 may be connected to form a ring or not;
[0047] The substituents in Z1, Z2 and Z3 are each independently selected from any one or a combination of at least two of halogen, C1-C10 chain alkyl, C3-C10 cycloalkyl, C2-C10 alkenyl, C1-C10 alkoxy, C6-C30 aryl and C3-C30 heteroaryl;
[0048] More preferably, one of Z1 and Z3 is selected from hydrogen, and the other of Z1 and Z3 and Z2 are independently selected from C1-C10 chain alkyl groups and are connected to each other to form a ring;
[0049] More preferably, Z1 and Z3 are selected from hydrogen, and Z2 is selected from one or a combination of at least two of C1-C10 chain alkyl, C3-C10 cycloalkyl, C1-C10 alkoxy, C6-C30 aryl, and C3-C30 heteroaryl;
[0050] More preferably, Z2 is selected from methyl, ethyl, propyl, isopropyl, cyclopentyl, cyclohexyl, tert-butyl, 2-methylbutyl, phenyl, biphenyl, naphthyl, anthracenyl, phenanthrenyl, indenyl, fluoranthenyl, triphenylene, pyrenyl, peryl, The invention can be selected from the group consisting of phenyl, tetraphenyl, fluorenyl, pyridyl, furyl, thienyl, pyrrolyl, pyridyl, indolyl, N-phenylindolyl, diphenylamino, acridinyl, carbazolyl, benzofuranyl, benzothienyl, dibenzofuran, and dibenzothiophene, or a combination of at least two thereof.
[0051] Furthermore, the organic compound of the present invention is preferably a compound having the following structure, but is not limited to the following compounds:
[0052]
[0053]
[0054]
[0055]
[0056]
[0057]
[0058]
[0059]
[0060]
[0061]
[0062] The above-mentioned compound of the present invention has excellent luminescent properties, can give triplet excitons to achieve higher luminescent efficiency, and is suitable for use as a luminescent dye based on its excellent carrier transfer efficiency, especially as a yellow and green luminescent dye. Of course, since the compound of the present invention can also be used as a sensitizer together with the host material and the dye to achieve a good luminescent layer. The devices used include but are not limited to organic electroluminescent devices, optical sensors, solar cells, lighting elements, organic thin film transistors, organic field effect transistors, organic thin film solar cells, information tags, electronic artificial skin sheets, sheet-type scanners or electronic paper, preferably organic electroluminescent devices.
[0063] The present invention also provides an organic electroluminescent device, which comprises a first electrode, a second electrode and at least one or more light-emitting functional layers inserted between the first electrode and the second electrode, wherein the light-emitting functional layer contains at least one compound described in the present invention.
[0064] The organic electroluminescent device of the present invention has the same structure as the existing devices, for example, including an anode layer, multiple light-emitting functional layers and a cathode layer; the multiple light-emitting functional layers at least include a light-emitting layer, wherein the light-emitting layer contains the above-mentioned organic compound of the present invention.
[0065] The present invention further discloses a display screen or a display panel, wherein the organic electroluminescent device as described above is adopted in the display screen or the display panel; preferably, the display screen or the display panel is an OLED display.
[0066] The present invention also discloses an electronic device, wherein the electronic device has a display screen or a display panel, and the display screen or the display panel adopts the organic electroluminescent device as described above.
[0067] The OLED device prepared using the compound of the present invention has high luminous efficiency and better service life, especially can adjust the light color of yellow and green dyes to achieve the light color required for mass production, and can meet the requirements of current panel and display manufacturers for high-performance materials. DETAILED DESCRIPTION
[0068] In order to enable those skilled in the art to better understand the present invention, the present invention is further described in detail below in conjunction with specific implementation methods.
[0069] The compounds of the synthesis methods not mentioned in the present invention are all raw materials obtained through commercial channels. The solvents and reagents used in the present invention, such as dichloromethane, petroleum ether, ethanol, toluene, anhydrous sodium sulfate, carbazole, benzimidazole and other chemical reagents, can be purchased from the domestic chemical product market, such as Sinopharm Group Reagent Company, TCI Company, Shanghai Bid Pharmaceutical Company, Bailingwei Reagent Company, etc. In addition, those skilled in the art can also synthesize by known methods.
[0070] The analysis and detection of the intermediates and compounds in the present invention were performed using an ABSCIEX mass spectrometer (4000QTRAP).
[0071] The synthesis method of the compound of the present invention is briefly described below.
[0072] The general synthetic formula of the compound of the present invention is as follows:
[0073]
[0074]
[0075] Synthesis Example 1: Synthesis of S1
[0076]
[0077] Synthesis of intermediate M1-1:
[0078] At room temperature, raw material 1 (40 g, 141.84 mmol), raw material 2 (24.72 g, 141.84 mmol), tri(dibenzylideneacetone)dipalladium (2.6 g, 2.84 mmol), tri-tert-butylphosphine tetrafluoroborate (1.65 g, 5.67 mmol), sodium tert-butoxide (24.45 g, 212.76 mmol), toluene (300 mL) as solvent were added to a 1L single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 100°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography in a silica gel column filled with silica gel, with dichloromethane as the eluent, concentrated, and washed with ethanol to obtain 45 g of white solid M1-1, with a yield of 84.5%. The molecular ion mass determined by mass spectrometry was: 374.22 (theoretical value: 374.13).
[0079] Synthesis of intermediate M1-2:
[0080] At room temperature, raw material M1-1 (10 g, 26.64 mmol), raw material 3 (4.45 g, 24.64 mmol), tri(dibenzylideneacetone)dipalladium (0.49 g, 0.53 mmol), tri-tert-butylphosphine tetrafluoroborate (0.31 g, 1.07 mmol), sodium tert-butoxide (3.84 g, 39.96 mmol), toluene (200 mL) as solvent were added to a 1L single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography on a silica gel column filled with silica gel, with dichloromethane as the eluent, concentrated, and washed with ethanol to obtain 7 g of white solid M1-2, with a yield of 51.9%. The molecular ion mass determined by mass spectrometry was: 505.31 (theoretical value: 505.23).
[0081] Synthesis of final product S1:
[0082] At room temperature, M1-2 (7 g, 13.83 mmol) and xylene (50 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 ° C, tert-butyl lithium n-hexane solution (17.3 mL, 27.66 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 ° C for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (2.67 mL, 27.66 mmol, 2.69 g / mL) was added to the system at -40 ° C, and stirred at low temperature for 10 min. The system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (8.8 mL, 41.49 mmol, 0.74 g / mL) was added at -40 ° C, and the temperature was raised to 120 ° C for overnight reaction. The system was cooled to room temperature, dichloromethane (100 mL) was added and mixed with silica gel for concentration, column chromatography (PE: DCM = 20: 1, v / v), and the crude product was recrystallized twice from toluene / ethanol to obtain 2 g of the sample before sublimation, with a yield of 30.16%. The molecular ion mass determined by mass spectrometry was 479.32 (theoretical value: 479.25).
[0083] Synthesis Example 2: Synthesis of S3
[0084]
[0085] Synthesis of intermediate M3-1:
[0086] At room temperature, raw material M1-1 (7 g, 18.65 mmol), raw material 4 (5.21 g, 18.65 mmol), tris(dibenzylideneacetone)dipalladium (0.34 g, 0.37 mmol), tri-tert-butylphosphine tetrafluoroborate (0.22 g, 0.75 mmol), sodium tert-butoxide (2.69 g, 27.97 mmol), toluene (60 mL) as solvent were added to a 1L single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography on a silica gel column filled with silica gel, with dichloromethane as the eluent, concentrated, and washed with ethanol to obtain 6 g of white solid M3-1, with a yield of 52.03%. The molecular ion mass determined by mass spectrometry was: 617.40 (theoretical value: 617.35).
[0087] Synthesis of final product S3:
[0088] At room temperature, add M3-1 (6 g, 9.70 mmol) and xylene (50 mL) to a 500 mL three-necked flask, replace nitrogen 3 times, add tert-butyl lithium n-hexane solution (12.1 mL, 19.41 mmol, 1.6 M) to the system at -70 ° C, stir at room temperature for 5 min, heat to 60 ° C and react for 2 h, the system changes from anhydrous clear to dark red. Add boron tribromide (1.9 mL, 19.41 mmol, 2.69 g / mL) to the system at -40 ° C, stir at low temperature for 10 min, the system changes from dark red transparent to red turbid. Then add N, N-diisopropylethylamine (6.2 mL, 29.11 mmol, 0.74 g / mL) at -40 ° C, heat to 120 ° C and react overnight. The system was cooled to room temperature, dichloromethane (100 mL) was added, and the mixture was concentrated by silica gel, and then column chromatography (PE:DCM=20:1, v / v) was performed. The crude product was recrystallized twice from toluene / ethanol to obtain 2.2 g of the pre-sublimation sample, with a yield of 38.3%. The molecular ion mass determined by mass spectrometry was 591.41 (theoretical value: 591.38).
[0089] Synthesis Example 3: Synthesis of S7
[0090]
[0091] Synthesis of intermediate M7-1:
[0092] At room temperature, raw material 5 (50 g, 145.32 mmol), raw material 2 (25.32 g, 145.32 mmol), tri(dibenzylideneacetone)dipalladium (2.66 g, 2.91 mmol), tri-tert-butylphosphine tetrafluoroborate (1.69 g, 5.81 mmol), sodium tert-butoxide (20.95 g, 217.98 mmol), toluene (500 mL) as solvent were added to a 1L single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 100°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography on a silica gel column filled with silica gel, with dichloromethane as the eluent, concentrated, and washed with ethanol to obtain 52 g of white solid M7-1, with a yield of 81.8%. The molecular ion mass determined by mass spectrometry was: 436.22 (theoretical value: 436.15).
[0093] Synthesis of intermediate M7-2:
[0094] At room temperature, raw material M7-1 (10 g, 22.86 mmol), raw material 4 (6.39 g, 22.86 mmol), tri(dibenzylideneacetone)dipalladium (0.42 g, 0.46 mmol), tri-tert-butylphosphine tetrafluoroborate (0.27 g, 0.92 mmol), sodium tert-butoxide (3.3 g, 34.29 mmol), toluene (200 mL) as solvent were added to a 500 mL single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography on a silica gel column filled with silica gel, with dichloromethane as the eluent, concentrated, and washed with ethanol to obtain 8.5 g of white solid M7-2, with a yield of 54.7%. The molecular ion mass determined by mass spectrometry was: 679.42 (theoretical value: 679.37).
[0095] Synthesis of final product S7:
[0096] At room temperature, M7-2 (8 g, 11.76 mmol) and xylene (40 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 ° C, tert-butyl lithium n-hexane solution (14.7 mL, 23.52 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 ° C for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (2.27 mL, 23.52 mmol, 2.69 g / mL) was added to the system at -40 ° C, stirred at low temperature for 10 min, and the system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (7.5 mL, 35.27 mmol, 0.74 g / mL) was added at -40 ° C, and the temperature was raised to 120 ° C for overnight reaction. The system was cooled to room temperature, dichloromethane (100 mL) was added, and the mixture was concentrated by silica gel, and column chromatography (PE:DCM=20:1, v / v) was performed. The crude product was recrystallized twice from toluene / ethanol to obtain 3.1 g of the pre-sublimation sample, with a yield of 40.3%. The molecular ion mass determined by mass spectrometry was 653.43 (theoretical value: 653.39).
[0097] Synthesis Example 4: Synthesis of S9
[0098]
[0099] Synthesis of intermediate M9-1:
[0100] At room temperature, raw material M7-1 (10 g, 22.86 mmol), raw material 6 (4.97 g, 22.86 mmol), tris(dibenzylideneacetone)dipalladium (0.42 g, 0.46 mmol), tri-tert-butylphosphine tetrafluoroborate (0.27 g, 0.91 mmol), sodium tert-butoxide (3.3 g, 34.3 mmol), toluene (60 mL) as solvent were added to a 250 mL single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography on a silica gel column filled with silica gel, with dichloromethane as the eluent, concentrated, and washed with ethanol to obtain 8.2 g of white solid M9-1, with a yield of 58%. The molecular ion mass determined by mass spectrometry was: 617.31 (theoretical value: 617.26).
[0101] Synthesis of final product S9:
[0102] At room temperature, M9-1 (7.5 g, 12.13 mmol) and xylene (50 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 ° C, tert-butyl lithium n-hexane solution (15.2 mL, 24.26 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 ° C for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (2.34 mL, 24.26 mmol, 2.69 g / mL) was added to the system at -40 ° C, stirred at low temperature for 10 min, and the system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (7.74 mL, 36.39 mmol, 0.74 g / mL) was added at -40 ° C, and the temperature was raised to 120 ° C for overnight reaction. The system was cooled to room temperature, dichloromethane (100 mL) was added, and the mixture was concentrated by silica gel, and then column chromatography (PE:DCM=20:1, v / v) was performed. The crude product was recrystallized twice from toluene / ethanol to obtain 2.5 g of the pre-sublimation sample, with a yield of 34.8%. The molecular ion mass determined by mass spectrometry was 591.33 (theoretical value: 591.28).
[0103] Synthesis Example 5: Synthesis of S10
[0104]
[0105] Synthesis of intermediate M10-1:
[0106] At room temperature, raw material 5 (50 g, 145.32 mmol), raw material 7 (28.23 g, 145.32 mmol), tris(dibenzylideneacetone)dipalladium (2.66 g, 2.91 mmol), tri-tert-butylphosphine tetrafluoroborate (1.69 g, 5.81 mmol), sodium tert-butoxide (20.95 g, 217.96 mmol), toluene (300 mL) as solvent were added to a 1L single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 100°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography on a silica gel column filled with silica gel, with dichloromethane as the eluent, concentrated, and washed with ethanol to obtain 45 g of white solid M10-1, with a yield of 70.8%. The molecular ion mass determined by mass spectrometry was: 456.16 (theoretical value: 456.12).
[0107] Synthesis of intermediate M10-2:
[0108] At room temperature, raw material M10-1 (15 g, 32.79 mmol), raw material 6 (7.13 g, 32.79 mmol), tri(dibenzylideneacetone)dipalladium (0.6 g, 0.66 mmol), tri-tert-butylphosphine tetrafluoroborate (0.38 g, 1.31 mmol), sodium tert-butoxide (4.73 g, 49.19 mmol), toluene (200 mL) as solvent were added to a 500 mL single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography in a silica gel column filled with silica gel, with dichloromethane as the eluent, concentrated, and washed with ethanol to obtain 12 g of white solid M10-2, with a yield of 57.3%. The molecular ion mass determined by mass spectrometry was: 637.26 (theoretical value: 637.23).
[0109] Synthesis of final product S10:
[0110] At room temperature, M10-2 (10 g, 15.67 mmol) and xylene (50 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 ° C, tert-butyl lithium n-hexane solution (21.7 mL, 34.7 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 ° C for reaction for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (3.34 mL, 34.7 mmol, 2.69 g / mL) was added to the system at -40 ° C, stirred at low temperature for 10 min, and the system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (11 mL, 52.07 mmol, 0.74 g / mL) was added at -40 ° C, and the temperature was raised to 120 ° C for reaction overnight. The system was cooled to room temperature, dichloromethane (100 mL) was added, and the mixture was concentrated by silica gel, and then column chromatography (PE:DCM=20:1, v / v) was performed. The crude product was recrystallized twice from toluene / ethanol to obtain 3.1 g of the pre-sublimation sample with a yield of 29.2%. The molecular ion mass determined by mass spectrometry was 611.32 (theoretical value: 611.25).
[0111] Synthesis Example 6: Synthesis of S12
[0112]
[0113] Synthesis of intermediate M12-1:
[0114] At room temperature, raw material M10-1 (15 g, 32.79 mmol), raw material 7 (7.13 g, 32.79 mmol), tris(dibenzylideneacetone)dipalladium (0.6 g, 0.66 mmol), tri-tert-butylphosphine tetrafluoroborate (0.38 g, 1.31 mmol), sodium tert-butoxide (4.73 g, 49.19 mmol), toluene (200 mL) as solvent were added to a 500 mL single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography on a silica gel column filled with silica gel, with dichloromethane as the eluent, concentrated, and washed with ethanol to obtain 10 g of white solid M12-1, with a yield of 47.8%. The molecular ion mass determined by mass spectrometry was: 637.28 (theoretical value: 637.23).
[0115] Synthesis of final product S12:
[0116] At room temperature, M12-1 (10 g, 15.67 mmol) and xylene (50 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 ° C, tert-butyl lithium n-hexane solution (19.6 mL, 31.4 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 ° C for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (3.0 mL, 31.34 mmol, 2.69 g / mL) was added to the system at -40 ° C, stirred at low temperature for 10 min, and the system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (10 mL, 47.01 mmol, 0.74 g / mL) was added at -40 ° C, and the temperature was raised to 120 ° C for overnight reaction. The system was cooled to room temperature, dichloromethane (100 mL) was added and mixed with silica gel for concentration, column chromatography (PE: DCM = 20: 1, v / v), and the crude product was recrystallized twice from toluene / ethanol to obtain 3.4 g of the sample before sublimation, with a yield of 35.5%. The molecular ion mass determined by mass spectrometry was 611.31 (theoretical value: 611.25).
[0117] Synthesis Example 7: Synthesis of S31
[0118]
[0119] Synthesis of intermediate M31-1:
[0120] At room temperature, raw material M1-1 (10 g, 26.64 mmol), raw material 8 (8.86 g, 26.64 mmol), tris(dibenzylideneacetone)dipalladium (0.49 g, 0.53 mmol), tri-tert-butylphosphine tetrafluoroborate (0.31 g, 1.07 mmol), sodium tert-butoxide (3.84 g, 39.96 mmol), toluene (60 mL) as solvent were added to a 500 mL single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography on a silica gel column filled with silica gel, with dichloromethane as the eluent, concentrated, and washed with ethanol to obtain 11 g of white solid M31-1, with a yield of 61.5%. The molecular ion mass determined by mass spectrometry was: 670.33 (theoretical value: 670.29).
[0121] Synthesis of final product S31:
[0122] At room temperature, M31-1 (7.5 g, 31.17 mmol) and xylene (50 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 °C, tert-butyl lithium n-hexane solution (14 mL, 22.35 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 °C for reaction for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (2.2 mL, 21.35 mmol, 2.69 g / mL) was added to the system at -40 °C, stirred at low temperature for 10 min, and the system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (7.1 mL, 33.52 mmol, 0.74 g / mL) was added at -40 °C, and the temperature was raised to 120 °C for reaction overnight. The system was cooled to room temperature, dichloromethane (100 mL) was added and mixed with silica gel for concentration, column chromatography (PE: DCM = 20: 1, v / v), and the crude product was recrystallized twice from toluene / ethanol to obtain 3.5 g of the pre-sublimation sample with a yield of 44.6%. The molecular ion mass determined by mass spectrometry was 644.36 (theoretical value: 644.31).
[0123] Synthesis Example 8: Synthesis of S91
[0124]
[0125] Synthesis of intermediate M91-1:
[0126] At room temperature, raw material 1 (20 g, 70.92 mmol), raw material 9 (15.47 g, 70.92 mmol), tetrakis(triphenylphosphine)palladium (2.46 g, 2.13 mmol), potassium carbonate (14.7 g, 106.38 mmol), 1,4-dioxane (100 mL) and water (10 mL) were added to a 500 mL single-mouth bottle as solvents, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, the solvent was dried, dichloromethane (200 mL) and water (100 mL) were added, and extraction was performed three times. The organic phase was collected, mixed with silica gel, concentrated, and column chromatographed (PE: DCM = 20: 1). 19.5 g of white solid M91-1 was obtained by washing with ethanol, with a yield of 73.25%. The molecular ion mass determined by mass spectrometry was 374.19 (theoretical value: 374.13).
[0127] Synthesis of intermediate M91-2:
[0128] At room temperature, raw material M91-1 (10 g, 26.64 mmol), raw material 4 (7.44 g, 26.64 mmol), tris(dibenzylideneacetone)dipalladium (0.49 g, 0.53 mmol), tri-tert-butylphosphine tetrafluoroborate (0.31 g, 1.07 mmol), sodium tert-butoxide (3.84 g, 39.96 mmol), toluene (60 mL) as solvent were added to a 500 mL single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110° C. overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography in a silica gel column equipped with silica gel, with dichloromethane as the eluent, concentrated, and recrystallized from toluene / ethanol to obtain 11.5 g of white solid M91-2, with a yield of 69.18%. The molecular ion mass determined by mass spectrometry was: 617.41 (theoretical value: 617.35).
[0129] Synthesis of final product S91:
[0130] At room temperature, M91-2 (11 g, 17.79 mmol) and xylene (60 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 ° C, tert-butyl lithium n-hexane solution (22.2 mL, 35.58 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 ° C for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (3.43 mL, 35.58 mmol, 2.69 g / mL) was added to the system at -40 ° C, stirred at low temperature for 10 min, and the system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (11.4 mL, 53.37 mmol, 0.74 g / mL) was added at -40 ° C, and the temperature was raised to 120 ° C for overnight reaction. The system was cooled to room temperature, dichloromethane (100 mL) was added, and the mixture was concentrated by silica gel, and then column chromatography (PE:DCM=20:1, v / v) was performed. The crude product was recrystallized twice from toluene / ethanol to obtain 3.4 g of the sample before sublimation, with a yield of 39.9%. The molecular ion mass determined by mass spectrometry was 591.43 (theoretical value: 591.38).
[0131] Synthesis Example 9: Synthesis of S95
[0132]
[0133] Synthesis of intermediate M95-1:
[0134] At room temperature, raw material 1 (15 g, 53.19 mmol), raw material 10 (12.66 g, 53.19 mmol), tetrakis(triphenylphosphine)palladium (1.84 g, 1.6 mmol), potassium carbonate (11.03 g, 79.79 mmol), 1,4-dioxane (100 mL) and water (10 mL) were added to a 500 mL single-mouth bottle as solvents, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, the solvent was dried, dichloromethane (200 mL) and water (100 mL) were added, and extraction was carried out three times. The organic phase was collected, mixed with silica gel, concentrated, column chromatography (PE: DCM = 20: 1), and ethanol was boiled and washed to obtain 14.3 g of white solid M95-1, with a yield of 68%. The molecular ion mass determined by mass spectrometry was: 394.15 (theoretical value: 394.10).
[0135] Synthesis of intermediate M95-2:
[0136] At room temperature, raw material M95-1 (10 g, 25.3 mmol), raw material 4 (7.07 g, 25.3 mmol), tris(dibenzylideneacetone)dipalladium (0.46 g, 0.51 mmol), tri-tert-butylphosphine tetrafluoroborate (0.29 g, 1.01 mmol), sodium tert-butoxide (3.65 g, 37.94 mmol), toluene (60 mL) as solvent were added to a 500 mL single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110° C. overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography in a silica gel column equipped with silica gel, with dichloromethane as the eluent, concentrated, and recrystallized from toluene / ethanol to obtain 11.5 g of white solid M95-2, with a yield of 71.2%. The molecular ion mass determined by mass spectrometry was: 637.38 (theoretical value: 637.32).
[0137] Synthesis of final product S95:
[0138] At room temperature, M95-2 (14 g, 21.93 mmol) and xylene (60 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 ° C, tert-butyl lithium n-hexane solution (27.4 mL, 43.87 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 ° C for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (4.2 mL, 43.87 mmol, 2.69 g / mL) was added to the system at -40 ° C, stirred at low temperature for 10 min, and the system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (14 mL, 65.8 mmol, 0.74 g / mL) was added at -40 ° C, and the temperature was raised to 120 ° C for overnight reaction. The system was cooled to room temperature, dichloromethane (100 mL) was added, and the mixture was concentrated by silica gel, and then column chromatography (PE:DCM=20:1, v / v) was performed. The crude product was recrystallized twice from toluene / ethanol to obtain 3.5 g of the sample before sublimation, with a yield of 33.8%. The molecular ion mass determined by mass spectrometry was 611.41 (theoretical value: 611.35).
[0139] Synthesis Example 10: Synthesis of S97
[0140]
[0141] Synthesis of intermediate M97-1:
[0142] At room temperature, raw material 5 (20 g, 58.13 mmol), raw material 9 (12.68 g, 58.13 mmol), tetrakis(triphenylphosphine)palladium (2.02 g, 1.74 mmol), potassium carbonate (12.05 g, 87.19 mmol), 1,4-dioxane (200 mL) and water (20 mL) were added to a 500 mL single-mouth bottle as solvents, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, the solvent was dried, dichloromethane (200 mL) and water (100 mL) were added, and extraction was carried out three times. The organic phase was collected, mixed with silica gel, concentrated, column chromatography (PE: DCM = 20: 1), and ethanol was boiled and washed to obtain 15 g of white solid M97-1, with a yield of 58.73%. The molecular ion mass determined by mass spectrometry was: 438.22 (theoretical value: 438.16).
[0143] Synthesis of intermediate M97-2:
[0144] At room temperature, raw material M97-1 (15 g, 34.29 mmol), raw material 4 (9.58 g, 34.29 mmol), tris(dibenzylideneacetone)dipalladium (0.63 g, 0.69 mmol), tri-tert-butylphosphine tetrafluoroborate (0.40 g, 1.37 mmol), sodium tert-butoxide (4.94 g, 51.44 mmol), toluene (80 mL) as solvent were added to a 500 mL single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110° C. overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography in a silica gel column equipped with silica gel, with dichloromethane as the eluent, concentrated, and recrystallized from toluene / ethanol to obtain 16.5 g of white solid M97-2, with a yield of 70.7%. The molecular ion mass determined by mass spectrometry was: 679.41 (theoretical value: 679.37).
[0145] Synthesis of final product S97:
[0146] At room temperature, add M97-2 (16.5 g, 24.25 mmol) and xylene (80 mL) to a 500 mL three-necked flask, replace nitrogen 3 times, add tert-butyl lithium n-hexane solution (30.3 mL, 48.5 mmol, 1.6 M) to the system at -70 ° C, stir at room temperature for 5 min, heat to 60 ° C and react for 2 h, the system changes from anhydrous clear to dark red. Add boron tribromide (4.7 mL, 48.5 mmol, 2.69 g / mL) to the system at -40 ° C, stir at low temperature for 10 min, the system changes from dark red transparent to red turbid. Then add N, N-diisopropylethylamine (15.5 mL, 72.75 mmol, 0.74 g / mL) at -40 ° C, heat to 120 ° C and react overnight. The system was cooled to room temperature, dichloromethane (100 mL) was added, and the mixture was concentrated by silica gel, and then column chromatography (PE:DCM=20:1, v / v) was performed. The crude product was recrystallized twice from toluene / ethanol to obtain 4.1 g of the sample before sublimation, with a yield of 35.3%. The molecular ion mass determined by mass spectrometry was 653.44 (theoretical value: 653.39).
[0147] Synthesis Example 11: Synthesis of S99
[0148]
[0149] Synthesis of intermediate M99-1:
[0150] At room temperature, raw material 5 (15 g, 43.6 mmol), raw material 10 (10.38 g, 43.6 mmol), tetrakis(triphenylphosphine)palladium (1.51 g, 1.31 mmol), potassium carbonate (9.04 g, 65.39 mmol), 1,4-dioxane (200 mL) and water (20 mL) were added to a 500 mL single-mouth bottle as solvents, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, the solvent was dried, dichloromethane (200 mL) and water (100 mL) were added, and extraction was performed three times. The organic phase was collected, mixed with silica gel, concentrated, and column chromatographed (PE: DCM = 20: 1). 12.6 g of white solid M99-1 was obtained by ethanol washing, with a yield of 62.9%. The molecular ion mass determined by mass spectrometry was 458.19 (theoretical value: 458.13).
[0151] Synthesis of intermediate M99-2:
[0152] At room temperature, raw material M99-1 (12.6 g, 97.55 mmol), raw material 4 (7.7 g, 27.55 mmol), tris(dibenzylideneacetone)dipalladium (0.5 g, 0.55 mmol), tri-tert-butylphosphine tetrafluoroborate (0.32 g, 1.1 mmol), sodium tert-butoxide (3.97 g, 41.3 mmol), toluene (80 mL) as solvent, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography in a silica gel column equipped with silica gel, with dichloromethane as the eluent, concentrated, and recrystallized from toluene / ethanol to obtain 10.7 g of white solid M99-2, with a yield of 55.5%. The molecular ion mass determined by mass spectrometry was 699.41 (theoretical value: 699.34).
[0153] Synthesis of final product S99:
[0154] At room temperature, M99-2 (10.7 g, 15.28 mmol) and xylene (80 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 ° C, tert-butyl lithium n-hexane solution (19.1 mL, 30.56 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 ° C for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (2.9 mL, 30.56 mmol, 2.69 g / mL) was added to the system at -40 ° C, stirred at low temperature for 10 min, and the system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (9.7 mL, 45.83 mmol, 0.74 g / mL) was added at -40 ° C, and the temperature was raised to 120 ° C for overnight reaction. The system was cooled to room temperature, dichloromethane (100 mL) was added and mixed with silica gel for concentration, column chromatography (PE: DCM = 20: 1, v / v), and the crude product was recrystallized twice from toluene / ethanol to obtain 2.2 g of the sample before sublimation, with a yield of 30%. The molecular ion mass determined by mass spectrometry was 673.41 (theoretical value: 673.36).
[0155] Synthesis Example 12: Synthesis of S127
[0156]
[0157] Synthesis of intermediate M127-1:
[0158] At room temperature, raw material 11 (15 g, 39.05 mmol), raw material 10 (9.3 g, 39.05 mmol), tetrakis(triphenylphosphine)palladium (1.35 g, 1.17 mmol), potassium carbonate (8.1 g, 58.57 mmol), 1,4-dioxane (200 mL) and water (20 mL) were added to a 500 mL single-mouth bottle as solvent, nitrogen was replaced three times, and the reaction was carried out at 110°C overnight. After the reaction solution was cooled, the solvent was dried, dichloromethane (200 mL) and water (100 mL) were added, and extraction was carried out three times. The organic phase was collected, mixed with silica gel for concentration, column chromatography (PE: DCM = 20: 1), and ethanol was boiled and washed to obtain 13.2 g of white solid M127-1, with a yield of 67.7%. The molecular ion mass determined by mass spectrometry was: 498.22 (theoretical value: 498.16).
[0159] Synthesis of intermediate M127-2:
[0160] At room temperature, raw material M127-1 (13.2 g, 26.53 mmol), raw material 4 (7.41 g, 26.53 mmol), tris(dibenzylideneacetone)dipalladium (0.49 g, 0.53 mmol), tri-tert-butylphosphine tetrafluoroborate (0.31 g, 1.06 mmol), sodium tert-butoxide (3.83 g, 39.8 mmol), toluene (80 mL) as solvent were added to a 500 mL single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110° C. overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography in a silica gel column equipped with silica gel, with dichloromethane as the eluent, concentrated, and recrystallized from toluene / ethanol to obtain 11.3 g of white solid M127-2, with a yield of 57.5%. The molecular ion mass determined by mass spectrometry was 739.41 (theoretical value: 739.37).
[0161] Synthesis of final product S127:
[0162] At room temperature, M127-2 (11.3 g, 15.26 mmol) and xylene (80 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 ° C, tert-butyl lithium n-hexane solution (19 mL, 30.52 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 ° C for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (2.9 mL, 30.52 mmol, 2.69 g / mL) was added to the system at -40 ° C, stirred at low temperature for 10 min, and the system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (9.5 mL, 45.78 mmol, 0.74 g / mL) was added at -40 ° C, and the temperature was raised to 120 ° C for overnight reaction. The system was cooled to room temperature, dichloromethane (100 mL) was added, and the mixture was concentrated by silica gel, and then column chromatography (PE:DCM=20:1, v / v) was performed. The crude product was recrystallized twice from toluene / ethanol to obtain 2.6 g of the pre-sublimation sample, with a yield of 35.5%. The molecular ion mass determined by mass spectrometry was 713.42 (theoretical value: 713.39).
[0163] Synthesis Example 13: Synthesis of S145
[0164]
[0165] Synthesis of intermediate M145-1:
[0166] At room temperature, raw material M91-1 (10 g, 26.64 mmol), raw material 8 (8.86 g, 26.64 mmol), tris(dibenzylideneacetone)dipalladium (0.49 g, 0.53 mmol), tri-tert-butylphosphine tetrafluoroborate (0.31 g, 1.07 mmol), sodium tert-butoxide (3.84 g, 39.96 mmol), toluene (50 mL) as solvent were added to a 500 mL single-mouth bottle, nitrogen was replaced three times, and the reaction was carried out at 110° C. overnight. After the reaction solution was cooled, it was subjected to rapid column chromatography in a silica gel column equipped with silica gel, with dichloromethane as the eluent, concentrated, and recrystallized from toluene / ethanol to obtain 10.5 g of white solid M145-1, with a yield of 58.7%. The molecular ion mass determined by mass spectrometry was: 670.33 (theoretical value: 670.29).
[0167] Synthesis of final product S145:
[0168] At room temperature, M145-1 (10.5 g, 15.64 mmol) and xylene (50 mL) were added to a 500 mL three-necked flask, and nitrogen was replaced 3 times. At -70 ° C, tert-butyl lithium n-hexane solution (19.6 mL, 31.28 mmol, 1.6 M) was added to the system, stirred at room temperature for 5 min, heated to 60 ° C for 2 h, and the system changed from anhydrous clear to dark red. Boron tribromide (3 mL, 31.28 mmol, 2.69 g / mL) was added to the system at -40 ° C, stirred at low temperature for 10 min, and the system changed from dark red transparent to red turbid. Then N, N-diisopropylethylamine (10 mL, 46.92 mmol, 0.74 g / mL) was added at -40 ° C, and the temperature was raised to 120 ° C for overnight reaction. The system was cooled to room temperature, dichloromethane (100 mL) was added, and the mixture was concentrated by silica gel, and then column chromatography (PE:DCM=20:1, v / v) was performed. The crude product was recrystallized twice from toluene / ethanol to obtain 3.1 g of the pre-sublimation sample with a yield of 41.3%. The molecular ion mass determined by mass spectrometry was 644.37 (theoretical value: 644.31).
[0169] The present invention exemplifies the specific synthesis methods of the above compounds. For other compounds for which no specific synthesis methods are given, they can be prepared by similar methods, and they can be obtained by simply replacing the raw materials. They will not be described in detail here, or those skilled in the art can also prepare them by other methods in the prior art. DETAILED DESCRIPTION
[0171] OLED includes a first electrode, a second electrode, and an organic material layer between the electrodes. The organic material layer can be divided into multiple regions. For example, the organic material layer can include a hole transport region, a light emitting layer, and an electron transport region.
[0172] In a specific embodiment, a substrate may be used below the first electrode or above the second electrode. The substrate is a glass or polymer material with excellent mechanical strength, thermal stability, water resistance, and transparency. In addition, a thin film transistor (TFT) may also be provided on the substrate used as a display.
[0173] The first electrode can be formed by sputtering or depositing the material used as the first electrode on the substrate. When the first electrode is used as an anode, an oxide transparent conductive material such as indium tin oxide (ITO), indium zinc oxide (IZO), tin dioxide (SnO2), zinc oxide (ZnO) and any combination thereof can be used. When the first electrode is used as a cathode, a metal or alloy such as magnesium (Mg), silver (Ag), aluminum (Al), aluminum-lithium (Al-Li), calcium (Ca), magnesium-indium (Mg-In), magnesium-silver (Mg-Ag) and any combination thereof can be used.
[0174] The organic material layer can be formed on the electrode by vacuum thermal evaporation, spin coating, printing, etc. The compound used as the organic material layer can be organic small molecules, organic macromolecules and polymers, and combinations thereof.
[0175] The hole transport region is located between the anode and the light-emitting layer. The hole transport region can be a hole transport layer (HTL) of a single-layer structure, including a single-layer hole transport layer containing only one compound and a single-layer hole transport layer containing multiple compounds. The hole transport region can also be a multi-layer structure including at least one layer of a hole injection layer (HIL), a hole transport layer (HTL), and an electron blocking layer (EBL).
[0176] The material of the hole transport region can be selected from, but not limited to, phthalocyanine derivatives such as CuPc, conductive polymers or polymers containing conductive dopants such as polyphenylene ethylene, polyaniline / dodecylbenzenesulfonic acid (Pani / DBSA), poly(3,4-ethylenedioxythiophene) / poly(4-styrenesulfonate) (PEDOT / PSS), polyaniline / camphorsulfonic acid (Pani / CSA), polyaniline / poly(4-styrenesulfonate) (Pani / PSS), aromatic amine derivatives such as the compounds shown in HT-1 to HT-34 below; or any combination thereof.
[0177]
[0178]
[0179] The hole injection layer is located between the anode and the hole transport layer. The hole injection layer can be a single compound material or a combination of multiple compounds. For example, the hole injection layer can use one or more compounds of HT-1 to HT-34 mentioned above, or one or more compounds of HI1-HI3 described below; or one or more compounds of HT-1 to HT-34 can be doped with one or more compounds of HI1-HI3 described below.
[0180]
[0181] The light-emitting layer includes the light-emitting dye (i.e., dopant) of the present invention that can emit different wavelength spectra, and can also include a host material (Host). In one aspect of the present invention, the light-emitting layer adopts the technology of fluorescent electroluminescence. The fluorescent host material of the light-emitting layer can be selected from, but not limited to, one or more combinations of BFH-1 to BFH-13 listed below.
[0182]
[0183] The OLED organic material layer may further include an electron transport region between the light emitting layer and the cathode. The electron transport region may be a single-layer electron transport layer (ETL), including a single-layer electron transport layer containing only one compound and a single-layer electron transport layer containing multiple compounds. The electron transport region may also be a multilayer structure including at least one layer of an electron injection layer (EIL), an electron transport layer (ETL), and a hole blocking layer (HBL).
[0184] In one aspect of the present invention, the electron transport layer material can be selected from, but not limited to, one or more combinations of ET-1 to ET-57 listed below.
[0185]
[0186]
[0187]
[0188] The device may further include an electron injection layer located between the electron transport layer and the cathode. Materials for the electron injection layer include, but are not limited to, one or more combinations of the following.
[0189] LiQ, LiF, NaCl, CsF, Li2O, Cs2CO3, BaO, Na, Li, Ca.
[0190] Theoretical calculation: The calculations described in the present invention were all completed using the Gaussian16 program, and the ground state structure of the molecule was optimized using B3LYP. The calculation for the first singlet excited state (S1) was based on the TDDFT level, and the maximum fluorescence emission wavelength was based on the S1 state structure. The calculation simulation results are shown in Table 1.
[0191] Table 1:
[0192] Compound No. Fluorescence maximum emission wavelength (nm) S1 582 (yellow light) S91 545 (green light)
[0193] According to theoretical calculations, the emission wavelength of the imidazole CB bond is within the yellow light range, which is the light color required by the present invention. Stable yellow light of different wavelengths can be adjusted by adjusting the substituents. The imidazole NB bond has a stronger resonance effect, which causes the emission wavelength to shift from blue to green light. The desired green light can be adjusted by adjusting the group coordinated with boron on the other side.
[0194] Application effect embodiment of the present invention:
[0195] Device Example 1:
[0196] The device structure is shown below:
[0197] ITO(150nm) / HI-2(10nm) / HT-2(40nm) / BFH-3:S1(30nm, 5%wt) / ET-59(25nm) / LiF(0.5nm) / Al(150nm).
[0198] The organic electroluminescent device was prepared as follows: a glass plate coated with a transparent conductive layer of ITO (thickness 150 nm) was ultrasonically treated in a commercial cleaning agent, rinsed in deionized water, ultrasonically degreased in a mixed solvent of acetone:ethanol, baked in a clean environment until the water was completely removed, cleaned with ultraviolet light and ozone, and bombarded with a low-energy cation beam;
[0199] Place the glass substrate with the anode in a vacuum chamber and evacuate to 1×10 -5 ~1×10 -4 Pa, HI-2 and HT-2 were vacuum evaporated on the above anode layer as hole injection layer and hole transport layer, respectively, with an evaporation rate of 0.1 nm / s and an evaporation film thickness of 10 nm and 40 nm, respectively;
[0200] "BFH-3: S1 (30nm, 5%wt)" is vacuum evaporated on the hole transport layer as the light-emitting layer of the organic electroluminescent device. The evaporation rate is 0.1nm / s and the total film thickness of the evaporation is 30nm; "5%wt" refers to the doping ratio of the blue light dye, that is, the weight ratio of the main material to S1 is 95:5.
[0201] ET-59 was vacuum-deposited on the light-emitting layer as the electron transport layer of the organic electroluminescent device, with a deposition rate of 0.1 nm / s and a total deposition film thickness of 20 nm;
[0202] 0.5 nm of LiF as an electron injection layer and 150 nm of Al as a cathode were vacuum-deposited on the electron transport layer.
[0203] Device Examples 2-13 and Comparative Examples 1-4:
[0204] The manufacturing process of device examples 2-13 and comparative examples 1-4 is the same as that of device example 1, except that the dye is replaced with prior art compounds R-1, R-2, R-3 and R-4.
[0205]
[0206] The organic electroluminescent device prepared by the above process was subjected to the following performance tests:
[0207] At the same brightness, the driving voltage and current efficiency of the organic electroluminescent devices prepared in Examples 1-13 and Comparative Examples 1-4 were measured using a digital source meter and a brightness meter. Specifically, the voltage was increased at a rate of 0.1 V per second, and the brightness of the organic electroluminescent device was measured when it reached 1000 cd / m 2 The voltage at this time is the driving voltage, and the current density at this time is measured at the same time; the external quantum efficiency is measured using an integrating sphere; the life test of LT95 is as follows: use a brightness meter at 1000cd / m 2 At the same brightness, the current is kept constant and the brightness of the organic electroluminescent device is measured to drop to 950cd / m 2 The time is in hours, and the LT95 life test value of device comparative example 1 is recorded as 1.0, and the ratio of the LT95 life test value of other devices to the LT95 life test value of device comparative example 1 is calculated. The test results are shown in Table 2 below.
[0208] Table 2:
[0209]
[0210]
[0211] The compounds of the present invention are used in organic electroluminescent devices. Compared with R-1, R-2 and R-3, in Examples 1-7, the other side of the molecules of the compounds of the present invention connected to the boron atom is a carbazole group. Since this structure is more rigid than the aromatic amine structure, it can suppress the vibration of the molecular bonds in the excited state and reduce energy loss. Therefore, while keeping the voltage relatively unchanged, the device using the compounds of the present invention obtains a better device life and EQE.
[0212] In Examples 8-13, due to the presence of BN polar bonds in the molecules of the compounds of the present invention, the resonance of the entire molecule can be enhanced, which is beneficial to the reverse intersystem crossing of the excited state, thereby making more effective use of triplet excitons. Therefore, the compounds of the present invention are used in devices to obtain better device luminescence efficiency and lifespan.
[0213] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the organic compounds of the present invention and the organic electroluminescent devices containing the same, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. An organic compound, characterized in that Having a structure as shown in formula (1) or formula (2): In formula (1) and formula (2), X1, X2, X3, and X4 are each independently selected from hydrogen, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted C1-C20 silyl, substituted or unsubstituted C6-C60 aryl, substituted or unsubstituted C3-C60 heteroaryl, substituted or unsubstituted C6-C60 arylamine, and substituted or unsubstituted C3-C60 heteroarylamine; two adjacent ones of X1, X2, X3, and X4 may be connected to form a ring or not; Y1, Y2, Y3, Y4, Y5, Y6, and Y7 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted C1-C20 silyl, substituted or unsubstituted C6-C60 aryl, substituted or unsubstituted C3-C60 heteroaryl, substituted or unsubstituted C6-C60 arylamine, and substituted or unsubstituted C3-C60 heteroarylamine; two adjacent ones of Y1, Y2, Y3, Y4, Y5, Y6, and Y7 may be connected to form a ring or not; Z1, Z2, and Z3 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted C1-C20 silyl, substituted or unsubstituted C6-C60 aryl, substituted or unsubstituted C3-C60 heteroaryl, substituted or unsubstituted C6-C60 arylamine, and substituted or unsubstituted C3-C60 heteroarylamine; two adjacent Z1, Z2, and Z3 may be connected to form a ring or not; The substituents substituted in X1, X2, X3, X4, Y1, Y2, Y3, Y4, Y5, Y6, Y7, Z1, Z2, and Z3 are each independently selected from any one of halogen, cyano, nitro, hydroxyl, amino, C1-C20 chain alkyl, C3-C20 cycloalkyl, C2-C20 alkenyl, C1-C20 alkoxy, C1-C20 silyl, C6-C60 arylamine, C3-C60 heteroarylamine, C6-C30 aryloxy, C3-C30 heteroaryloxy, C6-C60 aryl, and C3-C60 heteroaryl. A combination of at least two.
2. The organic compound according to claim 1, characterized in that The X1, X2, X3, and X4 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C10 chain alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C3-C10 cycloalkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, substituted or unsubstituted C6-C30 arylamine, and substituted or unsubstituted C3-C30 heteroarylamine; two adjacent ones of X1, X2, X3, and X4 may be connected to form a ring or not; The substituents in X1, X2, X3, and X4 are each independently selected from any one or a combination of at least two of halogen, C1-C10 chain alkyl, C3-C10 cycloalkyl, C2-C10 alkenyl, C1-C10 alkoxy, C6-C30 aryl, and C3-C30 heteroaryl; Preferably, X1, X2, X3, and X4 are each independently selected from one or a combination of at least two of hydrogen, C1-C10 chain alkyl, C2-C10 alkenyl, C3-C10 cycloalkyl, C1-C10 alkoxy, C6-C30 aryl, and C3-C30 heteroaryl; More preferably, X2 and X3 are each independently selected from hydrogen, methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, cyclopentyl, cyclohexyl, tert-butyl, 2-methylbutyl, pentyl, vinyl, propenyl, butenyl, butadienyl, phenyl, biphenyl, naphthyl, anthracenyl, phenanthrenyl, indenyl, fluorenyl, fluoranthenyl, triphenylene, pyrenyl, peryl, The invention can be selected from the group consisting of benzofuranyl, benzothiophenyl, isobenzofuranyl, isobenzothiophenyl, dibenzofuranyl, dibenzothiophenyl, indolyl, N-phenylindolyl, diphenylamine, carbazolyl, acridinium, imidazolyl and benzimidazolyl, or a combination of at least two of the following:
3. The organic compound according to claim 1, characterized in that The Y1, Y2, Y3, Y4, Y5, Y6, and Y7 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C10 chain alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C3-C10 cycloalkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, substituted or unsubstituted C6-C30 arylamine, and substituted or unsubstituted C3-C30 heteroarylamine; two adjacent ones of Y1, Y2, Y3, Y4, Y5, Y6, and Y7 are connected to form a ring or not; The substituents in Y1, Y2, Y3, Y4, Y5, Y6 and Y7 are each independently selected from any one or a combination of at least two of halogen, C1-C10 chain alkyl, C3-C10 cycloalkyl, C2-C10 alkenyl, C1-C10 alkoxy, C6-C30 aryl and C3-C30 heteroaryl; Preferably, Y2 and Y5 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C10 chain alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C3-C10 cycloalkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, substituted or unsubstituted C6-C30 arylamine, and substituted or unsubstituted C3-C30 heteroarylamine; The substituents in Y2 and Y5 are each independently selected from any one or a combination of at least two of halogen, C1-C10 chain alkyl, C3-C10 cycloalkyl, C1-C10 alkoxy, C6-C30 aryl, and C3-C30 heteroaryl; More preferably, Y2 and Y5 are each independently selected from one or a combination of at least two of hydrogen, C1-C10 chain alkyl, C2-C10 alkenyl, C3-C10 cycloalkyl, C1-C10 alkoxy, C6-C30 aryl, C3-C30 heteroaryl, C6-C30 arylamine, and C3-C30 heteroarylamine; More preferably, Y2 and Y5 are each independently selected from hydrogen, methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, tert-butyl, 2-methylbutyl, pentyl, vinyl, propenyl, butenyl, butadienyl, cyclopentyl, cyclohexyl, phenyl, biphenyl, naphthyl, anthracenyl, phenanthrenyl, indenyl, fluorenyl, fluoranthenyl, triphenylene, pyrenyl, peryl, The invention can be selected from the group consisting of phenyl, tetraphenyl, furanyl, thienyl, pyridyl, carbazolyl, benzofuranyl, benzothienyl, isobenzofuranyl, isobenzothienyl, dibenzofuranyl, dibenzothienyl, indolyl, N-phenylindolyl, diphenylamino, acridinyl, imidazolyl, and benzimidazolyl, or a combination of at least two thereof.
4. The organic compound according to claim 1, characterized in that The Z1, Z2, and Z3 are each independently selected from one of hydrogen, substituted or unsubstituted C1-C10 chain alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C3-C10 cycloalkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, substituted or unsubstituted C6-C30 arylamine, and substituted or unsubstituted C3-C30 heteroarylamine; two adjacent Z1, Z2, and Z3 may be connected to form a ring or not; The substituents in Z1, Z2 and Z3 are each independently selected from any one or a combination of at least two of halogen, C1-C10 chain alkyl, C3-C10 cycloalkyl, C2-C10 alkenyl, C1-C10 alkoxy, C6-C30 aryl and C3-C30 heteroaryl; Preferably, one of Z1 and Z3 is selected from hydrogen, and the other of Z1 and Z3 and Z2 are independently selected from C1-C10 chain alkyl groups and are connected to each other to form a ring; Preferably, Z1 and Z3 are selected from hydrogen, and Z2 is selected from one or a combination of at least two of C1-C10 chain alkyl, C3-C10 cycloalkyl, C1-C10 alkoxy, C6-C30 aryl, and C3-C30 heteroaryl; More preferably, Z2 is selected from methyl, ethyl, propyl, isopropyl, cyclopentyl, cyclohexyl, tert-butyl, 2-methylbutyl, phenyl, biphenyl, naphthyl, anthracenyl, phenanthrenyl, indenyl, fluoranthenyl, triphenylene, pyrenyl, peryl, The invention can be selected from the group consisting of phenyl, tetraphenyl, fluorenyl, pyridyl, furyl, thienyl, pyrrolyl, pyridyl, indolyl, N-phenylindolyl, diphenylamino, acridinyl, carbazolyl, benzofuranyl, benzothienyl, dibenzofuran, and dibenzothiophene, or a combination of at least two thereof.
5. The organic compound according to claim 1 is a compound having the following structure:
6. Use of the organic compound according to any one of claims 1 to 5, characterized in that: The organic compound is applied to organic electronic devices; Preferably, the organic electronic device comprises an organic electroluminescent device; Preferably, the organic compound is used as a light-emitting layer material in an organic electroluminescent device.
7. An organic electroluminescent device, characterized in that: The organic electroluminescent device comprises a first electrode, a second electrode and at least one organic layer disposed between the first electrode and the second electrode; the organic layer comprises at least one organic compound as described in any one of claims 1 to 5; Preferably, the organic layer comprises a light-emitting layer, and the light-emitting layer comprises at least one organic compound as described in any one of claims 1 to 5; Preferably, the light-emitting layer comprises a host material and a doping material, and the doping material comprises at least one organic compound as described in any one of claims 1 to 5.
8. A display device, characterized in that: The display device comprises the organic electroluminescent device according to claim 7.