Preparation method and application of Mn-MOF material suitable for large-scale production

By using the mixed heating and stirring method of manganese salt and terephthalic acid under normal pressure, the problem of long-term and poor repeatability of the preparation process of Mn-MOF materials is solved, and efficient adsorption performance under acidic conditions is achieved, which is suitable for large-scale production And significantly improve the removal rates of Fe(III), Mn(II), Cu(II), and Zn(II).

CN119019707AActive Publication Date: 2024-11-26SINOSTEEL MAANSHAN INST OF MINING RES CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411303750.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-26
Estimated Expiration
2044-09-19

AI Technical Summary

Technical Problem

The existing preparation methods of Mn-MOF materials have problems such as long preparation process, high reaction temperature, high reaction pressure, uncontrollable, poor repeatability, and limited adsorption effect of traditional adsorbents under acidic conditions.

Method used

Using the rapid synthesis method under normal pressure, the stirring temperature and time of manganese salt and terephthalic acid are mixed with heating and stirring in a specific solvent, the stirring temperature and time are controlled, and the solvent ratio and stirring rate are adjusted to prepare a stable and suitable for large-scale production. -MOF material.

Benefits of technology

The rapid synthesis of Mn-MOF under normal pressure is achieved. The product quality is stable, suitable for large-scale production, and it shows excellent adsorption performance under strong acid conditions. It is suitable for Fe(III), Mn(II), Cu(II), Zn The adsorption rate of (II) reaches as high as 100%, 97.8%, and 99.7%, significantly improving the treatment efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005048476650000071
    Figure BDA0005048476650000071
  • Figure HDA0005048476660000011
    Figure HDA0005048476660000011
  • Figure HDA0005048476660000012
    Figure HDA0005048476660000012
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a Mn-MOF material suitable for large-scale production. Manganese salt is dissolved in a solvent A, and terephthalic acid is dissolved in a solvent B; respectively feeding the two materials into a reaction container for mixing, heating and stirring, reacting, washing and drying to obtain a Mn-MOF material; the molar ratio of the manganese salt to the terephthalic acid is (1-1.5): 1, the heating and stirring temperature is controlled to be 70-90 DEG C, and the reaction time is controlled to be 50-80 min. The Mn-MOF material prepared by the method is used for adsorbing Fe (III) and / or Mn (II) and / or Cu (II) and / or Zn (II) in a water body, has excellent adsorption performance, and can be used for removing Fe (III), Mn (II), Cu (II) and Zn (II). Compared with a traditional hydrothermal method, the preparation method has the advantages that Mn-MOF is simply and rapidly synthesized under the normal pressure condition, the reaction process is safe and reliable, and the preparation method is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of MOF material manufacturing, and specifically relates to a preparation method of a Mn-MOF material and an application of the Mn-MOF material. Background Art

[0002] Mining production is prone to environmental pollution, among which acid mine wastewater pollution is a prominent problem. Usually, acid mine wastewater contains a variety of metals, including Fe(III), Mn(II), Cu(II), Zn(II), etc. Excessive metal ions have a profound impact on human health and environmental ecology. Therefore, developing a method and treatment material for treating Fe(III), Mn(II), Cu(II), and Zn(II) under acidic conditions is of great significance to humans and the natural environment.

[0003] At present, the main methods used to treat Fe(III), Mn(II), Cu(II), and Zn(II) include adsorption, membrane separation, and chemical precipitation. Among them, the adsorption method has the advantages of simple operation and wide application. The key to the adsorption method lies in the design and selection of adsorption materials. Traditional adsorbents are greatly affected by the pH of water, and the adsorption effect is limited under strong acidic conditions. In recent years, metal-organic framework materials (MOFs), as a porous compound composed of metal ions and organic ligands, not only have a large specific surface area and high porosity, but also have good water stability and acid-base stability, making them an excellent adsorption material for treating Fe(III), Mn(II), Cu(II), and Zn(II) under acidic conditions.

[0004] Metal-Organnic Frameworks (MOFs) are porous crystalline materials formed by the self-assembly of metal ions or metal clusters and organic ligands. This material combines the excellent properties of inorganic and organic materials. It not only has a high specific surface area, but also has good water stability and acid-base stability. It has attracted the research interest of many scholars. With its unique advantages, it is widely used in catalysis, gas separation, sensors, drug delivery and other fields. The main synthesis methods of MOF include solvothermal method, hydrothermal method, microwave method, ultrasound-assisted method, etc.

[0005] The existing Mn-MOF synthesis method is mainly a hydrothermal reactor synthesis method, which takes a long time to synthesize and needs to be completed in a high-temperature and high-pressure reactor. In addition, the pressure in the container is uncontrollable during the reaction, which often leads to poor repeatability of the results. Therefore, a method for quickly and stably synthesizing Mn-MOF under normal pressure is invented.

[0006] For example, Chinese patent CN201911179183.7 discloses a synthesis method of MOF74 (Mn) assembled from sheets into rods, comprising dissolving 2,5-dihydroxyterephthalic acid and 50% manganese nitrate solution in a mixture of N,N-dimethylformamide, anhydrous ethanol, and deionized water to obtain a mixed solution, transferring the mixed solution to a reactor, and heating for a period of time; after the reaction, washing and drying by centrifugation to obtain a sheet-assembled rod-shaped manganese-based MOF. The synthesis method obtains sheet-assembled rod-shaped manganese-based MOF by hydrothermal synthesis, and the size and morphology of the MOFs can be controlled by adjusting the reactant ratio, reaction solvent, reaction temperature, and reaction time. The prepared sheet-assembled rod-shaped MOF74 (Mn) material can be used as a new catalytic material. The synthesis method is carried out at high temperature and high pressure, and also has problems such as long reaction time, uncontrollable pressure in the container during the reaction, and poor reproducibility of results. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing Mn-MOF materials under normal pressure, with short reaction time, stable and controllable product quality, and suitable for large-scale production, in order to address the technical difficulties existing in the existing hydrothermal reactor synthesis method for preparing Mn-MOF materials, such as long preparation process, high reaction temperature, high and uncontrollable reaction pressure, poor repeatability, difficulty in large-scale production, and traditional adsorbents being greatly affected by the pH of the water body.

[0008] Another object of the present invention is to provide applications of the above-mentioned Mn-MOF material.

[0009] To achieve the above-mentioned purpose of the present invention, a preparation method of a Mn-MOF material suitable for large-scale production of the present invention comprises the following steps: a manganese salt is dissolved in a solvent A, and terephthalic acid is dissolved in a solvent B; the two are respectively introduced into a reaction container for mixing, heating and stirring, and after the reaction, the Mn-MOF material is obtained by washing and drying; the molar ratio between the manganese salt and terephthalic acid is (1-1.5): 1, the heating and stirring temperature is controlled at 70-90°C, and the reaction time is controlled at 50-80min.

[0010] Preferably, the solvent A is N,N-dimethylformamide.

[0011] Preferably, the solvent B is acetonitrile.

[0012] Preferably, the manganese salt is manganese acetate tetrahydrate.

[0013] Preferably, the molar ratio between the manganese salt and terephthalic acid is (1.3-1.5):1.

[0014] Preferably, the stirring rate is 250-400 rpm.

[0015] Furthermore, the heating and stirring temperature is 80° C., the reaction time is 60 min, and the stirring rate is 320 rpm.

[0016] The present invention discloses an application of a Mn-MOF material suitable for large-scale production, comprising: putting the Mn-MOF material into a water body containing Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) at a pH of 1.0 to 2.0 as an adsorbent to adsorb Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) in the water body.

[0017] Preferably, by detecting the metal ion concentration in the water containing Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II), the calculated mass of Mn-MOF is added to the water containing Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) at a solid-liquid ratio of 1:1 g / L at pH = 1.0 to 2.0, the mixture is mixed and reacted for 3 hours, and the Mn-MOF loaded with Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) is filtered out.

[0018] Furthermore, the present invention provides an application of a Mn-MOF material suitable for large-scale production, which is used to treat a solution containing Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II), wherein the Fe(III) concentration is 0.1 to 10.4 mg / L, the Mn(II) concentration is 0.1 to 10.6 mg / L, the Cu(II) concentration is 0.1 to 10.3 mg / L, and the Zn(II) concentration is 0.1 to 10.2 mg / L.

[0019] In practical applications, the present invention provides an application of a Mn-MOF material suitable for large-scale production, which specifically includes the following steps:

[0020] (1) A certain mass of Mn-MOF was added to an aqueous solution containing a certain concentration of Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) at a solid-liquid ratio of 1:1 g / L at a pH of 1.0-2.0, and the mixture was mixed and reacted for 3 h. The Mn-MOF loaded with Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) was filtered out.

[0021] (2) The Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) solution in step (1) has an Fe(III) concentration of 0.1 to 10.4 mg / L, a Mn(II) concentration of 0.1 to 10.6 mg / L, a Cu(II) concentration of 0.1 to 10.3 mg / L, and a Zn(II) concentration of 0.1 to 10.2 mg / L.

[0022] (3) After filtering out the Mn-MOF loaded with Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II), the concentration of Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) in the aqueous phase is further determined, and the amount of Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) adsorbed by Mn-MOF is determined by subtraction method, and the adsorption rate (E%) is calculated.

[0023] Compared with the prior art, the present invention provides a preparation method and application of Mn-MOF materials suitable for large-scale production, provides a special synthesis reaction environment for metal ions and organic ligands, and provides new adsorption materials for the treatment of Fe(III), Mn(II), Cu(II), and Zn(II) under acidic conditions. It has the following beneficial effects:

[0024] (1) Compared with the traditional hydrothermal method, the preparation method of the present invention can control the crystal growth rate by regulating the stirring rate, and the reaction can be carried out under normal pressure conditions. The reaction process is safe and reliable.

[0025] (2) The preparation method of the present invention can control the product grain size and nucleation rate by adjusting the solvent ratio and stirring rate, and can also adjust the product morphology according to market demand.

[0026] (3) The preparation method of the present invention can rapidly synthesize and prepare Mn-MOF at a relatively low temperature of about 80°C, and is suitable for large-scale production.

[0027] (4) The Mn-MOF material prepared by the method of the present invention has C, Mn, and O elements, has rich oxygen-containing functional groups, provides active sites, has excellent adsorption performance for Fe(III), Mn(II), Cu(II), and Zn(II) in water, and can be used to remove Fe(III), Mn(II), Cu(II), and Zn(II).

[0028] (5) Compared with traditional adsorbents, the Mn-MOF prepared in the present invention can quickly and effectively remove Fe(III), Mn(II), Cu(II), and Zn(II) within 3 h under strong acid conditions of pH = 1-2. The adsorption rate of Fe(III) is almost 100%, and that of Mn(II), Cu(II), and Zn(II) is as high as 97.8%, 99.4%, and 99.7%, respectively. The effect is extremely significant. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a process diagram of a preparation method of a Mn-MOF material suitable for large-scale production of the present invention

[0030] Figure 2 This is a bar graph showing the adsorption rate (E%) of Fe(III), Mn(II), Cu(II) and Zn(II) in acidic water using the Mn-MOF material prepared by the method of the present invention. DETAILED DESCRIPTION

[0031] To describe the present invention, the following is a further detailed description of a preparation method and application of a Mn-MOF material suitable for large-scale production of the present invention in conjunction with an embodiment. If no specific conditions are specified in the embodiments, the conventional conditions or the conditions recommended by the manufacturer are followed. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially. The scope of protection of the present invention is not limited by the following embodiments.

[0032] Example 1

[0033] Combined with Figure 1 The present invention provides a method for preparing a Mn-MOF material suitable for large-scale production, comprising the following steps:

[0034] (1) Weigh 0.0692 g of manganese acetate tetrahydrate and dissolve it in 18 mL of N,N-dimethylformamide.

[0035] (2) Weigh 0.0332 g of terephthalic acid and dissolve it in 14 mL of acetonitrile.

[0036] (3) The solutions in (1) and (2) were mixed so that the molar ratio of manganese acetate tetrahydrate to terephthalic acid was close to 1.5:1, and the mixture was transferred into a glass beaker.

[0037] (4) Set the operating parameters of the magnetic stirring heating apparatus: temperature 80°C, reaction time 60 min, and stirring rate 320 rpm.

[0038] (5) Place the magnetic stirring rotor into the sample, connect the temperature probe, and start the operation.

[0039] (6) After the synthesis is completed, the sample is removed and centrifuged. The separated solid is washed three times with ethanol and centrifuged three times. The synthesized Mn-MOF is dried in a vacuum drying oven at 100° C. to obtain the Mn-MOF material.

[0040] In order to verify the adsorption rate (E%) of Fe(III), Mn(II), Cu(II) and Zn(II) in acidic water by the Mn-MOF material prepared by the method of the present invention, in this embodiment, 0.01 g of Mn-MOF was weighed and added to an aqueous solution with a pH of 1.5 containing 10.4 mg / L Fe(III), 10.6 mg / L Mn(II), 10.3 mg / L Cu(II) and 10.2 mg / L Zn(II), and ultrasonically assisted mixing was performed. The reaction was allowed to stand for 3 hours, the loaded Mn-MOF was filtered out, and the adsorption rate (E%) was calculated.

[0041] Depend on Figure 2 As shown in the bar graph of the adsorption rate (E%) of the Mn-MOF material prepared by the method of the present invention for Fe(III), Mn(II), Cu(II) and Zn(II) in acidic water, the Mn-MOF material prepared by the method of the present invention has excellent adsorption performance for Fe(III), Mn(II), Cu(II) and Zn(II) in water, and the adsorption rate for Fe(III) is almost 100%, and the adsorption rate for Mn(II), Cu(II) and Zn(II) is as high as 97.8%, 99.4% and 99.7% respectively, which is very significant. The material can be used to remove Fe(III), Mn(II), Cu(II) and Zn(II), and has achieved unexpected technical effects.

[0042] Comparative Example 1

[0043] This comparative example adopts a synthesis method of Mn-MOF, comprising the following steps:

[0044] (1) Weigh 0.0492 g of manganese acetate tetrahydrate and dissolve it in 5 mL of N,N-dimethylformamide.

[0045] (2) Weigh 0.0332 g of terephthalic acid and dissolve it in 10 mL of water.

[0046] (3) The solutions in (1) and (2) are mixed so that the molar ratio of manganese acetate tetrahydrate to terephthalic acid is close to 1:1, and the mixture is transferred into a polytetrafluoroethylene-lined reactor and placed in a forced air drying oven.

[0047] (4) Set the operating parameters of the blast drying oven to 100°C and reaction time to 7h.

[0048] (5) After the synthesis is completed, the sample is removed and centrifuged. The separated solid is washed three times with ethanol and centrifuged three times. The synthesized Mn-MOF is dried in a vacuum drying oven at 70° C. to obtain a Mn-MOF material.

[0049] Example 2

[0050] 0.01 g of Mn-MOF was weighed and added to an aqueous solution with a pH of 1.8 containing 10 mg / L Fe(III), 10 mg / L Mn(II), 10 mg / L Cu(II), and 10 mg / L Zn(II). Ultrasonic-assisted mixing was performed and the reaction was allowed to stand for 3 h. The loaded Mn-MOF was filtered out and the adsorption rate (E%) was calculated (see Table 1 for experimental data).

[0051] Table 1 shows the test results of using the Mn-MOF material prepared by the method example of the present invention as an adsorbent to remove Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) in water.

[0052] Table 1 Mn-MOF as adsorbent for removal of Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) from water

[0053]

[0054] Note: C0 is the initial concentration of the ion in the solution; C e is the concentration of the ion in the solution after the reaction.

Claims

1. A method for preparing a Mn-MOF material suitable for large-scale production, characterized in that The method comprises the following steps: dissolving a manganese salt in a solvent A and dissolving terephthalic acid in a solvent B; respectively feeding the two into a reaction container for mixing, heating and stirring, and after reaction, washing and drying to obtain a Mn-MOF material; the molar ratio between the manganese salt and the terephthalic acid is (1-1.5):1, the heating and stirring temperature is controlled at 70-90°C, and the reaction time is controlled at 50-80min.

2. A method for preparing a Mn-MOF material suitable for large-scale production as claimed in claim 1, characterized in that: The solvent A is N,N-dimethylformamide.

3. The method for preparing a Mn-MOF material suitable for large-scale production according to claim 1, characterized in that: The solvent B is acetonitrile.

4. The method for preparing a Mn-MOF material suitable for large-scale production according to claim 1, characterized in that: The manganese salt is manganese acetate tetrahydrate.

5. The method for preparing a Mn-MOF material suitable for large-scale production according to claim 1, characterized in that: The solvent A is N,N-dimethylformamide, the solvent B is acetonitrile; the manganese salt is manganese acetate tetrahydrate; and the molar ratio between the manganese salt and terephthalic acid is (1.3-1.5):

1.

6. A method for preparing a Mn-MOF material suitable for large-scale production as claimed in claim 5, characterized in that: The stirring rate was 250-400 rpm.

7. A method for preparing a Mn-MOF material suitable for large-scale production as claimed in claim 6, characterized in that: The heating and stirring temperature was 80°C, the reaction time was 60 min, and the stirring rate was 320 rpm.

8. The use of a Mn-MOF material suitable for large-scale production as claimed in claim 1, 2, 3, 4, 5, 6 or 7, characterized in that: The Mn-MOF material is put into a water body containing Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) at a pH of 1.0 to 2.0 as an adsorbent to adsorb Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) in the water body.

9. The use of a Mn-MOF material suitable for large-scale production as claimed in claim 8, characterized in that: By detecting the metal ion concentration in the water containing Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II), the calculated mass of Mn-MOF is added to the water containing Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) at a solid-liquid ratio of 1:1 g / L at pH = 1.0-2.0, the mixture is mixed and reacted for 3 hours, and the Mn-MOF loaded with Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) is filtered out.

10. The use of a Mn-MOF material suitable for large-scale production as claimed in claim 9, characterized in that: The Fe(III) concentration of the solution containing Fe(III) and / or Mn(II) and / or Cu(II) and / or Zn(II) used for treatment is 0.1-10.4 mg / L, 0.1-10.6 mg / L for Mn(II), 0.1-10.3 mg / L for Cu(II), and 0.1-10.2 mg / L for Zn(II).

Citation Information

Patent Citations

  • Synthesis method of sheet-assembled rod-like MOF-74(Mn)

    CN110898855A

  • Method for treating antibiotic wastewater by using manganese ion doped metal organic framework material

    CN111533237A

  • Preparation method and application of MOF / corn straw composite material and device

    CN114797798A

  • Manganese-based catalytic material as well as preparation method and application thereof

    CN114950409A

  • Method for synthesizing, regulating and controlling MOF (Metal Organic Framework) material in large scale with high space-time yield and high quality

    CN118126343A