Method for rapidly separating viscous high polymer material from glassware

Through heating and low-temperature placement combined with external force strike, the problem of difficult separation of polymer materials and glassware is solved, and rapid and efficient separation is achieved, ensuring efficient utilization of materials.

CN119019726APending Publication Date: 2024-11-26WEIMU MEDICAL
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411220701.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Polymer materials tend to adhere to the inner wall of glassware after polymerization, resulting in difficulty in separation, and there are often broken glass residues during separation, affecting the reuse of the material.

Method used

By heating the glassware to a higher temperature than the glass transition temperature of the polymer material, then cooling down and placing it in a low temperature environment, the separation of the viscous polymer material and glassware is achieved by using external force strikes, creating a tiny gap close to the vacuum state to achieve rapid Separation.

Benefits of technology

It improves the separation efficiency between polymer materials and glassware, reduces material losses and working hours, ensures that there is no broken glass residue on the surface of polymer materials, simplifies the separation process, and improves the reusable efficiency of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005022942550000061
    Figure BDA0005022942550000061
  • Figure HDA0005022942560000011
    Figure HDA0005022942560000011
  • Figure HDA0005022942560000012
    Figure HDA0005022942560000012
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, in particular to a method for rapidly separating a viscous high polymer material from glassware, which comprises the following steps: S1, heating the glassware filled with the viscous high polymer material, and then cooling; s2, placing the glassware at a low temperature, and separating the viscous high polymer material from the glassware under the action of external force; by adopting the rapid separation method provided by the invention, the high polymer material does not need to be subjected to subsequent separation treatment, so that the efficiency of obtaining the high polymer material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a method for quickly separating a viscous polymer material from a glass container. Background Art

[0002] During the current experimental research and development stage, it is necessary to add reaction monomers into glassware for polymerization reaction to obtain polymer materials. Generally, polymer materials are sticky and will adhere to the inner wall of the glassware. After the reaction, it is not easy to quickly separate the sticky polymer materials from the glassware. Generally, after separation, glass materials will adhere to the surface of the polymer materials, and broken glass slag will remain on the surface of the sticky polymer materials. This problem will make it impossible for the polymer materials to be directly mechanically crushed and used as production materials. The polymer materials adhered to the glass materials need to be post-processed, and organic solvents are used to dissolve and separate the glass and polymer materials. This post-processing process reduces the separation efficiency and increases the loss of materials.

[0003] The Chinese patent with patent application number CN202210860686.6 discloses polymer materials and their preparation methods, self-repairing systems and reprocessable systems. The technical solution provided realizes the repeatable self-repairing and recyclable functions of the polymer materials, and the polymer materials have shape memory and degradable functions. The patent does not involve the issue of separation of polymer materials and glassware.

[0004] Therefore, providing a method for quickly separating viscous polymer materials from glassware is the main technical problem that needs to be solved at present. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method for quickly separating a viscous polymer material from a glass container, comprising the following steps:

[0006] S1. Heat the glass container containing the viscous polymer material first, and then cool it down;

[0007] S2. Place the glass container at low temperature and separate the viscous polymer material from the glass container by external force.

[0008] In order to create a gap at the contact point between the viscous polymer material and the glassware, the inventor discovered during the experiment that by overcoming the effect of gravity, a tiny gap close to a vacuum state can be created between the viscous polymer material in contact with the wall of the glassware and the wall of the glassware.

[0009] In one embodiment, the viscous polymer material can be obtained by the following steps:

[0010] The reactants are placed in a glass container for a first stage polymerization reaction. After the first stage polymerization reaction is completed, the temperature is lowered to below 30° C. to perform a second stage polymerization reaction to obtain a viscous polymer material.

[0011] In one embodiment, a magnetic stirrer is placed in the glass container, and the first stage polymerization reaction is completed when the magnetic stirrer continuously rotates at an angle less than 360°.

[0012] In one embodiment, after the first stage polymerization reaction is completed, the temperature is lowered to 22-28°C.

[0013] In a preferred embodiment, the temperature is lowered to 25° C. after the first stage polymerization reaction is completed.

[0014] In a preferred embodiment, no oily or viscous substance is present during the second stage polymerization reaction, and the reaction is judged to be complete.

[0015] In one embodiment, the glassware includes a beaker or a round bottom flask.

[0016] In one embodiment, the polymerization reaction in the beaker is performed to obtain a viscous polymer material. The difference before and after the treatment is shown in the schematic diagram. Figure 1 .

[0017] In one embodiment, the viscous polymer material obtained by the polymerization reaction in the round bottom flask is compared before and after the treatment. Figure 2 .

[0018] In one embodiment, in S1, the glass container containing the viscous polymer material is first heated to a temperature higher than the glass transition temperature of the polymer material.

[0019] In one embodiment, in S1, the glass container containing the viscous polymer material is first heated to a temperature that is 30° C. or higher than the glass transition temperature of the polymer material.

[0020] In one embodiment, the polymer material has a tensile modulus of less than 8400 MPa and an elongation at break of less than 2.5% when tested according to the GB1040-79 test method.

[0021] In one embodiment, the polymer material has a notched Izod impact strength greater than 60 J / m as measured by GB / T 1843-2008 for the Izod impact strength of plastics.

[0022] In one embodiment, the glassware is heated in S1 at a temperature of 110 to 120° C. for 1 to 10 minutes.

[0023] In a preferred embodiment, the heating temperature includes but is not limited to 110°C, 111°C, 112°C, 113°C, 114°C, 115°C, 116°C, 117°C, 118°C, 119°C, and 120°C.

[0024] In a preferred embodiment, the heating time of the glassware includes but is not limited to 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, and 10 min.

[0025] In one embodiment, the temperature in S1 is lowered to a temperature lower than the glass transition temperature of the polymer material.

[0026] In one embodiment, the temperature in S1 is lowered to a temperature that is 10° C. or more below the glass transition temperature of the polymer material.

[0027] In one embodiment, in S1, the glassware is cooled to 20-30°C.

[0028] In one embodiment, the temperature of the glassware is lowered to include but is not limited to 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, and 30°C in S1.

[0029] In a preferred embodiment, the glassware is cooled to 25° C. in S1.

[0030] In one embodiment, the method for preparing the viscous polymer material comprises the following steps:

[0031] Methyl methacrylate was put into a round-bottom flask for a first stage polymerization reaction. After the first stage polymerization reaction was completed, the temperature was lowered to 25° C. for a second stage polymerization reaction to obtain a viscous polymer material PMMA.

[0032] A magnetic stirrer is placed in the round-bottom flask, and the first stage of polymerization reaction is completed when the magnetic stirrer continuously rotates at an angle less than 360°.

[0033] In a preferred embodiment, in S2, the glassware is placed in an environment with a temperature of -15°C or below.

[0034] In one embodiment, in S2, the glassware is kept vertically inverted and placed at -15 to -80°C for 40 to 55 hours.

[0035] In one embodiment, the temperature at which the glassware is placed in S2 includes but is not limited to -15°C, -25°C, -35°C, -45°C, -55°C, -65°C, -75°C, and -80°C.

[0036] In one embodiment, the time for placing the glassware in S2 includes but is not limited to 40h, 41h, 42h, 43h, 44h, 45h, 46h, 47h, 48h, 49h, 50h, 51h, 52h, 53h, 54h, and 55h.

[0037] In a preferred embodiment, in S2, the glass container is kept vertically inverted and placed at -15 to -80°C for 42 to 50 hours.

[0038] In a preferred embodiment, in S2, the glassware is kept upright and placed at -20°C for 48 hours.

[0039] In order to achieve rapid separation of viscous polymer materials from glassware and avoid residual broken glass slag on the surface of the polymer materials, the inventors found in the experimental process that the viscous polymer materials and glassware can be quickly separated by adopting the above-mentioned separation method; in particular, the viscous polymer material obtained by the polymerization reaction is first heated, and the heating temperature is higher than 30°C of the Tg of the polymer material. After the heating is completed, the glassware is cooled to more than 10°C lower than the Tg of the polymer material and kept vertically inverted; then the glassware is placed in an environment with a temperature of -15°C or below, the glassware is taken out, and the glassware is knocked to separate the viscous polymer material from the glassware, which can effectively separate the viscous polymer material from the glassware. The polymer material and the glassware are separated quickly; the possible reason is that the heating temperature is more than 30℃ higher than the Tg of the polymer material, which will cause the molecular chain segments of the polymer material to relax and obtain a relaxed state. Then the polymer material is cooled and placed in an environment with a temperature of -15℃ or below, and the molecular chain segments of the polymer material will shrink. In particular, in S3, the glassware is placed at -15 to -80℃ for 40 to 55h. The stress caused by its volume shrinkage is greater than the van der Waals force between the material and the glass wall, and a certain gap is generated at the contact surface between the polymer material and the glassware, which realizes the rapid separation of the viscous polymer material and the glassware, and there is no broken glass or glass slag remaining on the surface of the polymer material.

[0040] In one embodiment, in S2, an external force is applied in a direction perpendicular to the gap between the viscous polymer material and the glass container.

[0041] In one embodiment, the external force includes external force of mechanical operations such as knocking and scraping.

[0042] In one embodiment, in S2, an external force is applied in a direction perpendicular to the gap between the viscous polymer material and the glass container.

[0043] Beneficial Effects

[0044] 1. By adopting the rapid separation method provided by the present invention, the complexity of separation is reduced, the separation efficiency of polymer materials and glassware is improved, the loss of materials is reduced, and the working hours are reduced.

[0045] 2. By adopting the rapid separation method provided by the present invention, the polymer material can be quickly and effectively separated from the inner wall of the glass reactor after the polymerization reaction is completed, thereby reducing material loss caused by excessive adhesion.

[0046] 3. By adopting the rapid separation method provided by the present invention, the viscous polymer material and the glassware can be quickly separated.

[0047] 4. By adopting the rapid separation method provided by the present invention, after the polymer material and the glassware are separated, no broken glass residue remains on the surface of the polymer material.

[0048] 5. By adopting the rapid separation method provided by the present invention, a gap can be generated at the contact point between the viscous polymer material and the glassware, and a tiny gap close to a vacuum state can be generated between the viscous polymer material in contact with the wall of the glassware and the wall of the glassware. The polymer material and the glassware can be separated quickly without the need for subsequent treatment of the polymer material after separation, thereby improving the efficiency of obtaining the polymer material. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 : Schematic diagram comparing the differences before and after treatment of viscous polymer material obtained by polymerization reaction in a beaker.

[0050] Figure 2 : Schematic diagram comparing the differences before and after treatment of viscous polymer materials obtained by polymerization reaction in a round-bottom flask.

[0051] Figure 3 : A diagram showing the state in which the viscous polymer material is in close contact with the wall of the round-bottom flask in S1 of Example 1.

[0052] Figure 4 : The effect diagram after the viscous polymer material and the round-bottom flask are separated in Example 1.

[0053] Figure 5 : The effect diagram after the viscous polymer material and the round-bottom flask are separated in Example 2. DETAILED DESCRIPTION

[0054] Before conducting the separation experiment between the polymer material and the round-bottom flask, a viscous polymer material is first prepared. The specific preparation method is shown in Example 1.

[0055] Example 1

[0056] The method for preparing the viscous polymer material comprises the following steps:

[0057] 100 g of methyl methacrylate was put into a round-bottom flask and heated to 100° C. for a first stage polymerization reaction. After the first stage polymerization reaction was completed, the temperature was lowered to 25° C. for a second stage polymerization reaction to obtain a viscous polymer material.

[0058] A magnetic stirrer is placed in the round-bottom flask, and the first stage of polymerization reaction is completed when the magnetic stirrer continuously rotates at an angle less than 360°.

[0059] During the second stage polymerization reaction, no oily or viscous substance is present, and it is determined that the reaction is complete.

[0060] The viscous polymer material is in close contact with the wall of the round-bottom flask, and its state is shown in FIG. Figure 3 .

[0061] Example 2

[0062] This embodiment provides a method for quickly separating a viscous polymer material from a round-bottom flask, comprising the following steps:

[0063] S1. The round-bottom flask containing the viscous polymer material was heated at a temperature of 115°C for 5 min, and after heating, the round-bottom flask was cooled to 25°C;

[0064] S2. Keep the round-bottom flask upright and inverted at -20°C for 48 hours, take out the round-bottom flask and knock on it with external force to separate the viscous polymer material from the round-bottom flask.

[0065] In the S2, an external force is applied in a direction perpendicular to the gap between the viscous polymer material and the round-bottom flask.

[0066] The viscous polymer material in S1 is the viscous polymer material provided in Example 1.

[0067] Example 3

[0068] This embodiment provides a method for quickly separating a viscous polymer material from a round-bottom flask, comprising the following steps:

[0069] S1. Place the round-bottom flask containing the viscous polymer material at 25°C;

[0070] S2. Use external force to knock the round-bottom flask to separate the viscous polymer material from the round-bottom flask.

[0071] The viscous polymer material in S1 is the viscous polymer material provided in Example 1.

[0072] In the embodiments 2 and 3, the viscous polymer material is separated from the round-bottom flask by using the same external force to knock the round-bottom flask.

[0073] Performance Testing

[0074] 1. Separation effect test

[0075] Observe the effect of separating the viscous polymer material from the round-bottom flask in Examples 2 and 3, record the separation state, and observe whether there is glass material adhering to the surface of the polymer material. The test results are shown in Table 1. The effect of separating the viscous polymer material from the round-bottom flask in Example 2 is shown in Table 2. Figure 4 The effect of separating the viscous polymer material from the round-bottom flask in Example 3 is shown in Figure 5 .

[0076] 2. Tensile performance test

[0077] The tensile modulus and elongation at break of the polymer materials obtained in Example 2 and Example 3 were tested according to the GB1040-79 test method. The test results are shown in Table 2.

[0078] 3. Impact performance test

[0079] The notched Izod impact strength of the polymer material obtained in Example 1 was measured according to GB / T 1843-2008 for the Izod impact strength of plastics. The test results are shown in Table 2.

[0080] Table 1

[0081] Example Separation effect Example 2 No glass material to adhere to Example 3 Glass material adhesion

[0082] Table 2

[0083]

[0084] pass Figure 4 It can be seen that there is no glass material adhering to the surface of the polymer material obtained in Example 2, and no broken glass residue remains, which achieves effective separation of the viscous polymer material from the round-bottom flask. The stripped polymer material can be directly mechanically crushed and then used as a production material.

[0085] pass Figure 5 It can be seen that glass material adheres to the surface of the polymer material obtained in Example 3. For the polymer material with glass material adhered, post-processing is still required to separate the polymer material from the glass material. The specific post-processing separation method includes the following steps:

[0086] A1. Transfer the polymer materials that remain on the round-bottom flask and are not completely peeled off, including the polymer materials that are adhered to the broken glass slag after being crushed, to a beaker, and add a soluble organic solvent to dissolve it. The dissolution time is greater than 24 hours.

[0087] A2. Heat the completely dissolved solution to 60°C, and filter it while it is hot. Repeat the operation 2-3 times until there is no fine glass residue left in the solution.

[0088] A3. The solution diluted by adding a large amount of soluble organic solvent needs to be heated and concentrated again before it can be used to produce materials.

Claims

1. A method for quickly separating a viscous polymer material from a glass container, characterized in that: The following steps are involved: S1. Heat the glass container containing the viscous polymer material first, and then cool it down; S2. Place the glass container at low temperature and separate the viscous polymer material from the glass container by external force.

2. The method for quickly separating a viscous polymer material from a glass container as claimed in claim 1, characterized in that: In S1, the glassware is heated at a temperature of 110 to 120° C. for 1 to 10 minutes.

3. The method for rapidly separating a viscous polymer material from a glass vessel as claimed in claim 1, characterized in that: In S1, the glass container containing the viscous polymer material is first heated to a temperature higher than the glass transition temperature of the polymer material.

4. The method for rapidly separating a viscous polymer material from a glass vessel as claimed in claim 3, characterized in that: In the above S1, the glass container containing the viscous polymer material is first heated to a temperature that is 30° C. higher than the glass transition temperature of the polymer material.

5. The method for rapidly separating a viscous polymer material from a glass container as claimed in claim 1, characterized in that: In the step S1, the temperature is lowered to a temperature lower than the glass transition temperature of the polymer material.

6. The method for rapidly separating a viscous polymer material from a glass container as claimed in claim 5, characterized in that: In the step S1, the temperature is lowered to a temperature which is 10° C. or higher below the glass transition temperature of the polymer material.

7. The method for rapidly separating a viscous polymer material from a glass container as claimed in claim 1, characterized in that: In the S2, the bottom of the glass vessel does not come into contact with the placement location.

8. The method for rapidly separating a viscous polymer material from a glass container as claimed in claim 1, characterized in that: The tensile modulus of the polymer material tested according to the GB1040-79 testing method is less than 8400 MPa, and the elongation at break is less than 2.5%.

9. The method for rapidly separating a viscous polymer material from a glass container as claimed in claim 1, characterized in that: In S2, the glassware is placed in an environment with a temperature of -15°C or below.

10. The method for rapidly separating a viscous polymer material from a glass container as claimed in claim 1, characterized in that: In the S2, an external force is applied in a direction perpendicular to the gap between the viscous polymer material and the glass container.

Citation Information

Patent Citations

  • High polymer material and preparation method thereof, self-repairing system and reprocessable system