Metal gel and preparation method thereof

By using a nano-scale polymer network to fix the liquid metal continuum in metal gels, the problems of low electrical conductivity and poor electromechanical stability in the polymer are solved, and the preparation of high electronic conductivity and flexible metal gels are achieved. Suitable for a variety of applications.

CN119019748APending Publication Date: 2024-11-26NANJING UNIV

Patent Information

Application Number
CN202411159674.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, liquid metals have island-like, skeleton-like and layered structures in polymers, resulting in low conductivity and lack of interaction with polymer matrix, affecting the electromechanical stability during dynamic deformation, which is difficult to achieve. High electronic conductivity and flexibility of metal gels.

Method used

By preparing a liquid metal-polymer mixed solution, the liquid metal continuum is fixed using the action force of a nano-scale polymer network to form a metal gel with high electron conductivity and flexibility, including preparing a polymer solution, uniformly dispersing liquid metals and polymers, The good solvent is then removed to form a metal gel.

Benefits of technology

It achieves high electronic conductivity and adjustable mechanical properties, and the material maintains stable performance in physical deformation or different environments. It is suitable for flexible stretchable electromagnetic shielding materials, sealing materials, implantable electrodes, etc.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019748A_ABST
    Figure CN119019748A_ABST
Patent Text Reader

Abstract

The invention discloses metal gel and a preparation method thereof, and belongs to the technical field of gel and polymer composite materials. Comprising the following steps: dissolving polymer powder in a good solvent to obtain a polymer solution; uniformly mixing the liquid metal with the polymer solution through a homogenizing process; and removing the good solvent in the liquid metal-polymer mixed solution to obtain the metal gel. Compared with the prior art, the method has the advantages that the liquid metal continuum serves as a fluid phase and is stably fixed in a nanoscale polymer network through interaction, and the unique structure enables the metal gel to have high conductivity (as high as 3.18 * 10 < 6 > S / m), tissue-like flexibility (the Young modulus is as low as 70 kPa) and low air permeability (4.50 * 10 <-22 > m < 2 > / s / Pa); the material can maintain stable performance when subjected to physical deformation or in different environments, and the problems that in the prior art, liquid metal is not used as a solvent phase, the compatibility between the liquid metal and a polymer network is poor, and the electronic conductivity of a gel material is low are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gel and composite materials, and more particularly to a metal gel and a preparation method thereof. Background Art

[0002] Gel is a semisolid material in which a fluid is fixed throughout the volume of a three-dimensional colloidal or polymer network. The fluid is the main component of the gel and determines the basic physical and chemical properties of the gel. Hydrogels use water as a fluid and exhibit biocompatibility, electrical insulation, softness, and affinity with water-soluble substances. Organogels have been developed using various organic liquids instead of water, which exhibit good hydrophobic-related properties. Ionic liquids were introduced as fluid-modifiable materials for ionic conductivity and thermal stability.

[0003] Liquid metals, known for their fluidity, high electrical conductivity, low gas permeability, and biocompatibility, have emerged as a versatile functional material in recent years. Combining liquid metals with polymers to impart metallic properties while maintaining softness has been extensively studied. In these liquid metal-polymer composites, the liquid metal exists in the polymer phase as islands, skeletons, and layers. However, the conductivity is generally not high due to the limited content and connectivity of the liquid metal. In addition, the lack of interaction between the polymer matrix and the liquid metal impairs the electromechanical stability during dynamic deformation.

[0004] In the related art, for example, Chinese patent document CN 115073764 A discloses a liquid metal microgel and its preparation method and application, comprising a core and a shell; the core is a micro-nano liquid metal particle, and the shell is a gel layer; wherein the gel layer is formed in situ on the surface of the liquid metal particle by a polymer material. However, the related art does not provide any technical inspiration on how to use liquid metal as a metal gel of the fluid phase to achieve a gel material with high electronic conductivity and flexibility. Summary of the invention

[0005] 1. Technical issues to be solved

[0006] In response to the problem in the prior art of how to use liquid metal as the fluid phase of metal gel to achieve high electronic conductivity and flexibility of gel and composite materials, the present invention provides a metal gel and a preparation method thereof, which develops a new type of gel material based on the existing gel system, wherein liquid metal is used as the fluid phase in the gel, and the nanoscale polymer network fixes the liquid metal continuum through the action of force, thereby achieving high electronic conductivity and flexibility, and maintaining stable performance when the material undergoes physical deformation or is in different environments.

[0007] 2. Technical solution

[0008] The purpose of the present invention is achieved through the following technical solutions.

[0009] A method for preparing a metal gel, comprising the following steps:

[0010] Prepare polymer solution: add polymer powders to good solvents respectively, dissolve them and stir them evenly to obtain polymer solution;

[0011] Preparing a liquid metal-polymer mixed solution: adding liquid metal to a polymer solution, and uniformly dispersing the mixed solution with a homogenizer to obtain a liquid metal-polymer mixed solution;

[0012] Processing of liquid metal-polymer mixed solution: removing the good solvent from the uniformly dispersed mixed solution by heating or freeze-drying to obtain metal gel.

[0013] Furthermore, the steps of preparing the polymer solution include: preparing type ι carrageenan solution; preparing sodium alginate solution; preparing gellan gum solution; preparing hyaluronic acid solution, and preparing poly (vinylidene fluoride-hexafluoropropylene) solution.

[0014] Furthermore, the step of preparing the iota carrageenan solution is specifically as follows: dissolving 0.80 wt% to 4.80 wt% of iota carrageenan powder in deionized water, and continuously stirring with a magnetic force at a temperature of 80° C. for 2 hours until the powder is dissolved, to obtain an iota carrageenan solution;

[0015] The steps of preparing the sodium alginate solution are as follows: dissolving 0.80 wt% to 4.80 wt% of sodium alginate powder in deionized water, and continuously stirring the sodium alginate powder with a magnetic force at a temperature of 25° C. for 2 hours until the sodium alginate powder is dissolved to obtain the sodium alginate solution.

[0016] Furthermore, the steps of preparing the gellan gum solution are specifically as follows: dissolving 0.80 wt% to 4.80 wt% of gellan gum powder in deionized water, and continuously stirring with magnetic force at a temperature of 25° C. for 2 hours until the gellan gum powder is dissolved, to obtain a gellan gum solution;

[0017] The specific steps of preparing the hyaluronic acid solution are as follows: dissolving 0.80wt% to 4.80wt% of hyaluronic acid powder in deionized water, and continuously stirring with magnetic force for 2 hours at a temperature of 25°C until the hyaluronic acid powder is dissolved to obtain the hyaluronic acid solution.

[0018] The specific steps of preparing the poly(vinylidene fluoride-hexafluoropropylene) solution are as follows: dissolving 0.80wt% to 4.80wt% of poly(vinylidene fluoride-hexafluoropropylene) particles in N-methylpyrrolidone, and continuously stirring with a magnetic force for 2 hours at a temperature of 25°C until it is dissolved to obtain a poly(vinylidene fluoride-hexafluoropropylene) solution.

[0019] Furthermore, the steps of preparing the liquid metal-polymer mixed solution include: preparing a gallium-indium alloy-ι-carrageenan mixed solution; preparing a gallium-ι-carrageenan mixed solution; preparing a gallium-indium-tin alloy-ι-carrageenan mixed solution; preparing a gallium-indium alloy-sodium alginate mixed solution; preparing a gallium-indium alloy-gellan gum mixed solution; preparing a gallium-indium alloy-hyaluronic acid mixed solution; preparing a gallium-indium alloy-poly (vinylidene fluoride-hexafluoropropylene) mixed solution.

[0020] Furthermore, the steps of preparing the liquid metal-polymer mixed solution are specifically as follows:

[0021] The liquid metal gallium-indium alloy and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-indium alloy-iota carrageenan mixed solution;

[0022] The liquid metal gallium and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-iota carrageenan mixed solution;

[0023] The liquid metal gallium indium tin alloy and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 minutes to 15 minutes at a temperature of 80°C using a handheld homogenizer to obtain a gallium indium tin alloy-iota carrageenan mixed solution.

[0024] Furthermore, the step of preparing the liquid metal-polymer mixed solution also includes:

[0025] The liquid metal gallium-indium alloy and the sodium alginate solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-sodium alginate mixed solution;

[0026] The liquid metal gallium-indium alloy and the gellan gum solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred with a handheld homogenizer at a temperature of 25° C. and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min to obtain a gallium-indium alloy-gellan gum mixed solution;

[0027] The liquid metal gallium-indium alloy and the hyaluronic acid solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-hyaluronic acid mixed solution.

[0028] The liquid metal gallium-indium alloy and poly(vinylidene fluoride-hexafluoropropylene) solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 minutes to 15 minutes at a temperature of 25°C using a handheld homogenizer to obtain a gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) mixed solution.

[0029] Furthermore, the steps of treating the liquid metal-polymer mixed solution are specifically as follows:

[0030] The obtained liquid metal-polymer mixed solution was added into polytetrafluoroethylene watch glasses respectively, and the watch glasses were placed in an environment of 25° C. to 80° C. to remove the good solvent, thereby obtaining a metal gel.

[0031] The novel metal gel prepared according to the metal gel preparation method comprises liquid metal and polymer network; wherein the liquid metal forms a continuum as the fluid phase of the gel; and the nanoscale polymer network fixes the liquid metal fluid by interaction.

[0032] 3. Beneficial effects

[0033] Compared with the prior art, the advantages of the present invention are:

[0034] (1) Developed a new gel system, which for the first time realized the use of liquid metal as the fluid phase in the gel material;

[0035] (2) A material structure completely different from existing liquid metal composites was obtained;

[0036] (3) The different polymer network systems used can form forces with liquid metal, improving the forces between the polymer network and the metal and avoiding the problems of structural phase separation and instability;

[0037] (4) The prepared series of metal gels all exhibit high electronic conductivity and tunable mechanical properties;

[0038] (5) The high conductivity and flexibility of metal gels enable them to be used in flexible and stretchable electromagnetic shielding materials, sealing materials with ultra-low oxygen permeability, and implantable electrodes, which have great advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a schematic diagram of a computer tomography image of a metal gel in one embodiment of the present invention;

[0040] Figure 2 is a computer tomography image of a metal gel in one embodiment of the present invention and a schematic diagram of a polymer network extracted therefrom;

[0041] Figure 3 is a schematic diagram of a SEM image of a nanoscale polymer network of a metal gel in one embodiment of the present invention;

[0042] Figure 4 Schematic diagram of the preparation process of metal gel in one embodiment of the present invention;

[0043] Figure 5 Schematic diagram of the variation of the electronic conductivity and Young's modulus of the gallium-indium alloy-ι-type carrageenan metal gel with the liquid metal content in one embodiment of the present invention;

[0044] Figure 6 It is a schematic diagram of the electromagnetic shielding effectiveness in the initial state and the deformed state when the gallium-indium alloy-ι-type carrageenan metal gel is used as an electromagnetic shielding material in one embodiment of the present invention;

[0045] Figure 7 Schematic diagram showing the performance comparison between the oxygen permeability and Young's modulus of the gallium-indium alloy-ι-type carrageenan metal gel and other sealing materials in one embodiment of the present invention;

[0046] Figure 8 Schematic diagram showing the performance comparison between gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) metal gel and other electrode materials when used for electrical stimulation of rat sciatic nerve in one embodiment of the present invention;

[0047] Fig. 9 It is a schematic diagram showing the performance comparison between gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) metal gel and other electrode materials when used for long-term implantation of rat sciatic nerve electrical stimulation in one embodiment of the present invention;

[0048] Fig.10 A schematic diagram of a photo of gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) metal gel and polyimide attached to the inner wall of the intestine in one embodiment of the present invention;

[0049] Fig.11 It is a schematic diagram of histopathological sections of gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) metal gel and polyimide after being implanted into the intestine in one embodiment of the present invention;

[0050] Fig.12 This is a schematic diagram of real-time signal monitoring of intestinal signal monitoring electrodes using gallium-indium alloy-poly (vinylidene fluoride-hexafluoropropylene) metal gel in one embodiment of the present invention. DETAILED DESCRIPTION

[0051] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0052] Example 1

[0053] like Figures 1 to 3 As shown, this embodiment provides a metal gel including liquid metal and a polymer network.

[0054] Among them, liquid metal, as the fluid phase in the metal gel, occupies 85.1% to 92.4% of the volume fraction. The liquid metals in the metal gel are interconnected and form a continuum.

[0055] The polymer network presents a nano-scale dispersed three-dimensional porous network structure and a uniform and stable fixed liquid metal fluid.

[0056] Specifically, the liquid metal is interconnected in the entire bulk phase to form a continuum, and the polymer network presents a three-dimensional porous structure dispersed at the nanoscale. The polymer network and the liquid metal interact with each other, so that the liquid metal is fixed in the polymer network and ensures that the liquid metal does not leak.

[0057] Specifically, inside the gel, the liquid metal continuum acts as the fluid phase in the gel, providing a good electron path for the metal gel. The metal gel has an electronic conductivity close to the intrinsic value of liquid metal, reaching a maximum of 3.18×10 6 The three-dimensional porous polymer network provides good mechanical support for the metal gel, with adjustable mechanical properties (Young's modulus as low as 70 kPa), and a large amount of liquid metal is stably fixed in the nanoscale dispersed polymer network, which enhances the stability of the gel.

[0058] Metal gels are classified into seven systems according to the types of liquid metal and polymer network used: gallium-indium alloy-ι-carrageenan metal gel, gallium-ι-carrageenan metal gel, gallium-indium-tin alloy-ι-carrageenan metal gel, gallium-indium alloy-sodium alginate metal gel, gallium-indium alloy-gellan gum metal gel, gallium-indium alloy-hyaluronic acid metal gel, and gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) metal gel. Their electronic conductivity is more than 2.00×10 6 S / m, and have different mechanical properties (Young's modulus as low as 70kPa). Among them, poly (vinylidene fluoride-hexafluoropropylene) or PVDF-HFP is a polymer formed by copolymerization of vinylidene fluoride and hexafluoropropylene.

[0059] The new metal gel in this embodiment is a brand-new metal gel material. This metal gel has broad application prospects in flexible wearable and implantable electronic devices. It can be used for flexible and stretchable electromagnetic shielding materials with high shielding effectiveness, flexible ultra-low oxygen permeability sealing materials and implantable electrodes.

[0060] Specifically, the gallium-indium alloy-ι-type carrageenan metal gel, as a flexible and stretchable electromagnetic shielding material with high electromagnetic shielding performance, can be used for high-efficiency electromagnetic shielding, and exhibits an average total electromagnetic shielding effectiveness of 47.8dB to 65.4dB in the frequency range of 8.2GHz to 12.4GHz, an average total electromagnetic shielding effectiveness of 48dB to 65.8dB under a 50% stretching condition, and an average total electromagnetic shielding effectiveness of 50dB to 67.4dB under a 100% stretching condition, which remains basically unchanged, and the electromagnetic shielding effectiveness does not decay even if the 100% stretching is repeated 1000 times;

[0061] Gallium-indium alloy-ι-type carrageenan metal gel is a sealing material with ultra-low oxygen permeability. It can be used as a sealing material with ultra-low oxygen permeability (4.5×10 -22 m 2 / s / Pa), which is comparable to aluminum-plastic film and as soft as traditional soft materials such as hydrogels (Young's modulus 336kPa);

[0062] Gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) metal gel is a sciatic nerve stimulation electrode that is as soft as biological tissue. When used as a sciatic nerve stimulation electrode, compared with rigid platinum electrodes and printed liquid metal electrodes, the metal gel can achieve a more obvious stimulation effect at a lower voltage and show stable performance during long-term implantation;

[0063] When gallium-indium alloy-poly (vinylidene fluoride-hexafluoropropylene) metal gel is used as a biosensor electrode on the intestinal mucosa, unlike the polyimide film commonly used in flexible electronic products, the metal gel can fit the folds of the mucosa well, and will not cause physical damage to the intestinal mucosa after implantation into the rat colon. The mucosal junction protein ZO-1 remains intact, so the metal gel can effectively detect the coupled changes of intestinal electrical signals and ion concentrations.

[0064] Example 2

[0065] like Figure 4 As shown, this embodiment discloses a method for preparing a metal gel, comprising the following steps:

[0066] Preparation of polymer solution:

[0067] preparing an iota carrageenan solution;

[0068] Specifically, 0.80 wt% to 4.80 wt% of iota carrageenan powder is dissolved in deionized water, and magnetic stirring is continuously performed at a temperature of 80° C. for 2 hours until the iota carrageenan powder is dissolved to obtain an iota carrageenan solution.

[0069] preparing sodium alginate solution;

[0070] Specifically, 0.80 wt% to 4.80 wt% of sodium alginate powder is dissolved in deionized water, and the powder is continuously magnetically stirred at 25° C. for 2 hours until the powder is dissolved to obtain a sodium alginate solution.

[0071] preparing a gellan gum solution;

[0072] Specifically, 0.80 wt% to 4.80 wt% of gellan gum powder is dissolved in deionized water, and magnetic stirring is continuously performed at a temperature of 25° C. for 2 hours until the gellan gum powder is dissolved to obtain a gellan gum solution.

[0073] preparing a hyaluronic acid solution;

[0074] Specifically, 0.80 wt% to 4.80 wt% of hyaluronic acid powder is dissolved in deionized water, and magnetic stirring is continued at 25° C. for 2 hours until the hyaluronic acid powder is dissolved to obtain a hyaluronic acid solution.

[0075] preparing a poly(vinylidene fluoride-hexafluoropropylene) solution;

[0076] 0.80 wt % to 4.80 wt % of poly(vinylidene fluoride-hexafluoropropylene) particles were dissolved in N-methylpyrrolidone, and magnetic stirring was continued for 2 hours at a temperature of 25° C. until the particles were dissolved to obtain a poly(vinylidene fluoride-hexafluoropropylene) solution.

[0077] Preparation of liquid metal-polymer mixed solution:

[0078] The liquid metal gallium-indium alloy and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-indium alloy-iota carrageenan mixed solution;

[0079] The liquid metal gallium and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-iota carrageenan mixed solution;

[0080] The liquid metal gallium indium tin alloy and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 to 15 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium indium tin alloy-iota carrageenan mixed solution;

[0081] The liquid metal gallium-indium alloy and the sodium alginate solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-sodium alginate mixed solution;

[0082] The liquid metal gallium-indium alloy and the gellan gum solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred with a handheld homogenizer at a temperature of 25° C. and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min to obtain a gallium-indium alloy-gellan gum mixed solution;

[0083] The liquid metal gallium-indium alloy and the hyaluronic acid solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 to 15000 rpm for 5 to 15 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-hyaluronic acid mixed solution;

[0084] The liquid metal gallium-indium alloy and poly(vinylidene fluoride-hexafluoropropylene) solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 to 15000 rpm for 5 to 15 minutes at a temperature of 25°C using a handheld homogenizer to obtain a gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) mixed solution.

[0085] Specifically, in this step, the liquid metal undergoes high-speed stirring and shearing in a homogenizer, forming small droplets dispersed in the solution, and the polymer network is dispersed on the metal surface and in the good solvent.

[0086] Handling of liquid metal-polymer mixed solutions:

[0087] The uniformly dispersed mixed solution is heated to remove the good solvent.

[0088] Specifically, the obtained mixed solutions of liquid metal and polymer of different systems are added into polytetrafluoroethylene watch glasses respectively, and then placed in an environment of 25° C. to 80° C. to remove the good solvent, thereby obtaining the metal gel.

[0089] In this step, initially, the liquid metal droplets are dispersed in the form of nanodroplets, in which the entangled polymer chains form physically cross-linked networks. These networks also capture a large amount of good solvent. As drying proceeds, the good solvent in these networks is gradually replaced by liquid metal. The micropores between the liquid metal droplets, which were originally filled with water, are transformed into nanopores filled with liquid metal. Eventually, the liquid metal fluid becomes the dominant component, forming a continuous structure, and the polymer network is embedded in this liquid metal continuum.

[0090] The metal gels prepared according to the above steps have excellent electronic conductivity and diverse mechanical properties. As shown in Table 1, metal gels can be successfully prepared based on different polymer networks (iota carrageenan, sodium alginate, gellan gum, hyaluronic acid and poly (vinylidene fluoride-hexafluoropropylene)) and different liquid metals (gallium-indium alloy, gallium and gallium-indium-tin alloy). The liquid metal accounts for the vast majority of the gel volume (>87.6vol%), indicating that the liquid metal acts as a fluid phase in it, and their electronic conductivity is greater than 2.00×10 6 S / m, the Young's modulus can reach as low as 70kPa, and it has good flexibility.

[0091] Table 1. Values ​​of liquid metal content, electronic conductivity, and Young's modulus for seven metal gel systems based on different polymer networks and liquid metals

[0092]

[0093] like Figure 5 As shown in the figure, the electronic conductivity and Young's modulus of the gallium-indium alloy-ι-carrageenan metal gel vary with the liquid metal content. Taking the gallium-indium alloy-ι-carrageenan metal gel as an example, the liquid metal content in the gel is adjustable. Even if the volume fraction of the liquid metal is reduced, the electronic conductivity and Young's modulus can still be maintained at a good level. When the liquid metal volume fraction is 92.4%, the metal gel shows a 3.18×10 6 The electronic conductivity of 10.5 S / m and the Young's modulus of 336 kPa are superior to the performance of gel materials reported so far.

[0094] This new type of metal gel material developed using liquid metal as the fluid phase has a special structure, namely, a liquid metal continuum is realized in the gel material and is fixed in the system by a nano-dispersed polymer network. This special structure makes the metal gel have a wide range of applications.

[0095] like Figure 6As shown, the electromagnetic shielding effectiveness diagram of the gallium indium alloy-ι-type carrageenan metal gel in the initial state and the deformed state when used as an electromagnetic shielding material. There is an urgent need for soft, stretchable electromagnetic shielding materials with excellent shielding performance, but although traditional metals provide high electromagnetic shielding effectiveness, they are rigid and non-stretchable, and the existing stretchable electromagnetic shielding materials often fail to meet the requirements and show insufficient or sharply decreased electromagnetic shielding effectiveness under strain. Gallium indium alloy-ι-type carrageenan metal gel can be used for flexible, stretchable and efficient electromagnetic shielding, showing an average total electromagnetic shielding effectiveness of 47.8dB to 65.4dB in the frequency range of 8.2GHz to 12.4GHz, an average total electromagnetic shielding effectiveness of 48dB to 65.8dB under the condition of 50% stretching, and an average total electromagnetic shielding effectiveness of 50dB to 67.4dB under the condition of 100% stretching, which remains basically unchanged. Even if the 100% stretching is repeated 1000 times, the electromagnetic shielding effectiveness does not decay.

[0096] like Figure 7 The figure shows the oxygen permeability and Young's modulus of the gallium-indium alloy-ι-carrageenan metal gel compared with other sealing materials (aluminum-plastic film, elastomer and hydrogel). Soft sealing materials are an important technology to enclose electronic devices and protect them from active substances such as oxygen, which is crucial to ensure their long-term stability. However, soft materials including hydrogels and elastomers are characterized by high chain mobility and large free volume, resulting in high permeability. Metal gel has become a promising solution with ultra-low oxygen permeability (4.5×10 -22 m 2 / s / Pa), which is comparable to aluminum-plastic film and is as soft as traditional soft materials such as hydrogels (Young's modulus 336 kPa).

[0097] like Figures 8 to 9 As shown, this is a statistical comparison of the performance of gallium-indium alloy-poly (vinylidene fluoride-hexafluoropropylene) metal gel and other electrode materials (platinum and printed liquid metal) when used for electrical stimulation of the sciatic nerve of rats. For electrodes in implantable bioelectronics, the material is required to have metal-like conductivity, tissue-like softness and stability in a deformed state and fluid environment. These properties are critical for minimizing signal loss, achieving mechanical compatibility at the device-tissue interface, and reducing immune response. Existing conductive materials do not meet these comprehensive requirements. In contrast, soft metal gels have excellent conductivity and stability, providing a better choice for electronic conductors in implantable bioelectronics. Figure 8 As shown in the study, when used as sciatic nerve stimulation electrodes, which are crucial for the treatment of neurological diseases, metal gels can achieve more significant stimulation effects at lower voltages compared to rigid platinum electrodes and printed liquid metal electrodes. Fig. 9As shown, the performance is stable during long-term implantation, while under the same conditions, the performance of the printed liquid metal electrode decreases significantly.

[0098] like Figures 10 to 12 Shown are photos of gallium-indium alloy-poly (vinylidene fluoride-hexafluoropropylene) metal gel used as intestinal signal monitoring electrodes, intestinal tissue pathological sections, and real-time signal monitoring performance. Materials used in implantable bioelectronics must meet more stringent standards before they can be applied to complex organs such as the intestine. The intestinal mucosa is rich in biosignature signals and is a potential sensor-tissue interface for intestinal biosensing. However, the wrinkled inner surface of the intestine makes it challenging to construct a conformal sensor-mucosal interface. In addition, mechanically incompatible materials can easily cause physical damage to the mucosa, leading to the infiltration of harmful exogenous substances such as bacteria and toxins. When gallium-indium alloy-poly (vinylidene fluoride-hexafluoropropylene) metal gel is used as a biosensing electrode on the intestinal mucosa, Fig.10 As shown, unlike the polyimide films commonly used in flexible electronics, metal gels can conform well to the wrinkles of the mucosa, forming a good sensor-mucosa interface and, as shown in Fig.11 As shown, implantation into the rat colon did not cause physical damage to the intestinal mucosa, and the mucosal junction protein ZO-1 remained intact, as shown in Fig.12 As shown, metal gel can effectively detect coupled changes in intestinal electrical signals and ion concentrations.

[0099] Example 3

[0100] like Figure 4 As shown, this embodiment discloses a method for preparing a metal gel, comprising the following steps:

[0101] Preparation of polymer solution:

[0102] 0.80 wt% to 1.80 wt% of iota carrageenan powder is dissolved in deionized water.

[0103] Specifically, at a temperature of 80° C., magnetic stirring is continued for 2 hours until the carrageenan is dissolved to obtain an iota carrageenan solution.

[0104] 0.80 wt% to 1.80 wt% of sodium alginate powder is dissolved in deionized water.

[0105] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until the alginate is dissolved to obtain a sodium alginate solution.

[0106] 0.80 wt% to 1.80 wt% of gellan gum powder is dissolved in deionized water.

[0107] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until the gellan gum is dissolved to obtain a gellan gum solution.

[0108] 0.80 wt% to 1.80 wt% of hyaluronic acid powder is dissolved in deionized water.

[0109] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until it is dissolved to obtain a hyaluronic acid solution.

[0110] 0.80 wt % to 1.80 wt % of poly(vinylidene fluoride-hexafluoropropylene) particles are dissolved in N-methylpyrrolidone.

[0111] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until it is dissolved to obtain a poly(vinylidene fluoride-hexafluoropropylene) solution.

[0112] Preparation of liquid metal-polymer mixed solution:

[0113] The liquid metal gallium-indium alloy and the iota carrageenan solution are mixed in a weight ratio of 6:4 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 12000 rpm for 5 to 10 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-indium alloy-iota carrageenan mixed solution;

[0114] The liquid metal gallium and the iota carrageenan solution are mixed in a weight ratio of 6:4 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 12000 rpm for 5 to 10 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-iota carrageenan mixed solution;

[0115] The liquid metal gallium indium tin alloy and the iota carrageenan solution are mixed in a weight ratio of 6:4 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 12000 rpm for 5 to 10 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium indium tin alloy-iota carrageenan mixed solution;

[0116] The liquid metal gallium-indium alloy and the sodium alginate solution are mixed in a weight ratio of 1:1 to 6:4, and then sheared at a speed of 8000 rpm to 12000 rpm for 10 to 15 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-sodium alginate mixed solution;

[0117] The liquid metal gallium-indium alloy and the gellan gum solution are mixed in a weight ratio of 1:1 to 6:4, and then stirred and sheared at a speed of 8000 rpm to 12000 rpm for 10 to 15 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-gellan gum mixed solution;

[0118] The liquid metal gallium-indium alloy and the hyaluronic acid solution are mixed in a weight ratio of 1:1 to 6:4, and then sheared at a speed of 8000 rpm to 12000 rpm for 10 to 15 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-hyaluronic acid mixed solution;

[0119] The liquid metal gallium-indium alloy and poly(vinylidene fluoride-hexafluoropropylene) solution are mixed in a weight ratio of 1:1 to 6:4, and then sheared at a speed of 8000 rpm to 12000 rpm for 10 to 15 minutes at a temperature of 25°C using a handheld homogenizer to obtain a gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) mixed solution.

[0120] Specifically, in this step, the liquid metal undergoes high-speed stirring and shearing in a homogenizer, forming small droplets dispersed in the solution, and the polymer network is dispersed on the metal surface and in the good solvent.

[0121] Handling of liquid metal-polymer mixed solutions:

[0122] The uniformly dispersed mixed solution is heated to remove the good solvent.

[0123] Specifically, the obtained mixed solutions of liquid metal and polymer of different systems are added into polytetrafluoroethylene watch glasses respectively, and then placed in an environment of 40° C. to remove the good solvent, thereby obtaining the metal gel.

[0124] In this step, initially, the liquid metal droplets are dispersed in the form of nanodroplets, in which the entangled polymer chains form physically cross-linked networks. These networks also capture a large amount of good solvent. As drying proceeds, the good solvent in these networks is gradually replaced by liquid metal. The micropores between the liquid metal droplets, which were originally filled with water, are transformed into nanopores filled with liquid metal. Eventually, the liquid metal fluid becomes the dominant component, forming a continuous structure, and the polymer network is embedded in this liquid metal continuum.

[0125] Example 4

[0126] like Figure 4 As shown, this embodiment discloses a method for preparing a metal gel, comprising the following steps:

[0127] Preparation of polymer solution:

[0128] 1.80 wt% to 2.80 wt% of iota carrageenan powder is dissolved in deionized water.

[0129] Specifically, at a temperature of 80° C., magnetic stirring is continued for 2 hours until the carrageenan is dissolved to obtain an iota carrageenan solution.

[0130] 1.80 wt% to 2.80 wt% of sodium alginate powder is dissolved in deionized water.

[0131] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until the alginate is dissolved to obtain a sodium alginate solution.

[0132] 1.80 wt% to 2.80 wt% of gellan gum powder is dissolved in deionized water.

[0133] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until the gellan gum is dissolved to obtain a gellan gum solution.

[0134] 1.80 wt% to 2.80 wt% of hyaluronic acid powder is dissolved in deionized water.

[0135] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until it is dissolved to obtain a hyaluronic acid solution.

[0136] 1.80 wt% to 2.80 wt% of poly(vinylidene fluoride-hexafluoropropylene) particles were dissolved in N-methylpyrrolidone.

[0137] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until it is dissolved to obtain a poly(vinylidene fluoride-hexafluoropropylene) solution.

[0138] Preparation of liquid metal-polymer mixed solution:

[0139] The liquid metal gallium-indium alloy and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 6:4, and then stirred and sheared at a speed of 10000 rpm to 15000 rpm for 10 to 15 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-indium alloy-iota carrageenan mixed solution;

[0140] The liquid metal gallium and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 6:4, and then stirred and sheared at a speed of 10000 rpm to 15000 rpm for 10 to 15 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-iota carrageenan mixed solution;

[0141] The liquid metal gallium indium tin alloy and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 6:4, and then stirred and sheared at a speed of 10000 rpm to 15000 rpm for 10 to 15 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium indium tin alloy-iota carrageenan mixed solution;

[0142] The liquid metal gallium-indium alloy and the sodium alginate solution are mixed in a weight ratio of 6:4 to 7:3, and then sheared at a speed of 10000 rpm to 15000 rpm for 5 to 10 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-sodium alginate mixed solution;

[0143] The liquid metal gallium-indium alloy and the gellan gum solution are mixed in a weight ratio of 6:4 to 7:3, and then stirred and sheared at a speed of 10000 rpm to 15000 rpm for 5 to 10 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-gellan gum mixed solution;

[0144] The liquid metal gallium-indium alloy and the hyaluronic acid solution are mixed in a weight ratio of 6:4 to 7:3, and then sheared at a speed of 10000 rpm to 15000 rpm for 5 to 10 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-hyaluronic acid mixed solution;

[0145] The liquid metal gallium-indium alloy and poly(vinylidene fluoride-hexafluoropropylene) solution are mixed in a weight ratio of 6:4 to 7:3, and then sheared at a speed of 10000 rpm to 15000 rpm for 5 to 10 minutes at a temperature of 25°C using a handheld homogenizer to obtain a gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) mixed solution.

[0146] Specifically, in this step, the liquid metal undergoes high-speed stirring and shearing in a homogenizer, forming small droplets dispersed in the solution, and the polymer network is dispersed on the metal surface and in the good solvent.

[0147] Handling of liquid metal-polymer mixed solutions:

[0148] The uniformly dispersed mixed solution is heated to remove the good solvent.

[0149] Specifically, the obtained mixed solutions of liquid metal and polymer of different systems are added into polytetrafluoroethylene watch glasses respectively, and then placed in an environment of 60° C. to remove the good solvent, thereby obtaining the metal gel.

[0150] In this step, initially, the liquid metal droplets are dispersed in the form of nanodroplets, in which the entangled polymer chains form physically cross-linked networks. These networks also capture a large amount of good solvent. As drying proceeds, the good solvent in these networks is gradually replaced by liquid metal. The micropores between the liquid metal droplets, which were originally filled with water, are transformed into nanopores filled with liquid metal. Eventually, the liquid metal fluid becomes the dominant component, forming a continuous structure, and the polymer network is embedded in this liquid metal continuum.

[0151] Example 5

[0152] like Figure 4 As shown, this embodiment discloses a method for preparing a metal gel, comprising the following steps:

[0153] Preparation of polymer solution:

[0154] 2.80 wt% to 3.80 wt% of iota carrageenan powder is dissolved in deionized water.

[0155] Specifically, at a temperature of 80° C., magnetic stirring is continued for 2 hours until the carrageenan is dissolved to obtain an iota carrageenan solution.

[0156] 2.80 wt% to 3.80 wt% of sodium alginate powder was dissolved in deionized water.

[0157] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until the alginate is dissolved to obtain a sodium alginate solution.

[0158] 2.80 wt% to 3.80 wt% of gellan gum powder is dissolved in deionized water.

[0159] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until the gellan gum is dissolved to obtain a gellan gum solution.

[0160] 2.80 wt% to 3.80 wt% of hyaluronic acid powder was dissolved in deionized water.

[0161] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until it is dissolved to obtain a hyaluronic acid solution.

[0162] 2.80 wt% to 3.80 wt% of poly(vinylidene fluoride-hexafluoropropylene) particles were dissolved in N-methylpyrrolidone.

[0163] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until it is dissolved to obtain a poly(vinylidene fluoride-hexafluoropropylene) solution.

[0164] Preparation of liquid metal-polymer mixed solution:

[0165] The liquid metal gallium-indium alloy and the iota carrageenan solution are mixed in a weight ratio of 6:4 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 12000 rpm for 5 to 10 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-indium alloy-iota carrageenan mixed solution;

[0166] The liquid metal gallium and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 6:4, and then stirred and sheared at a speed of 8000 rpm to 12000 rpm for 5 to 10 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-iota carrageenan mixed solution;

[0167] The liquid metal gallium indium tin alloy and the iota carrageenan solution are mixed in a weight ratio of 6:4 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 12000 rpm for 5 to 10 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium indium tin alloy-iota carrageenan mixed solution;

[0168] The liquid metal gallium-indium alloy and the sodium alginate solution are mixed in a weight ratio of 1:1 to 6:4, and then sheared at a speed of 8000 rpm to 12000 rpm for 10 to 15 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-sodium alginate mixed solution;

[0169] The liquid metal gallium-indium alloy and the gellan gum solution are mixed in a weight ratio of 6:4 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 12000 rpm for 10 to 15 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-gellan gum mixed solution;

[0170] The liquid metal gallium-indium alloy and the hyaluronic acid solution are mixed in a weight ratio of 1:1 to 6:4, and then sheared at a speed of 8000 rpm to 12000 rpm for 10 to 15 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-hyaluronic acid mixed solution;

[0171] The liquid metal gallium-indium alloy and poly(vinylidene fluoride-hexafluoropropylene) solution are mixed in a weight ratio of 1:1 to 6:4, and then sheared at a speed of 10000 rpm to 15000 rpm for 5 to 10 minutes at a temperature of 25°C using a handheld homogenizer to obtain a gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) mixed solution.

[0172] Specifically, in this step, the liquid metal undergoes high-speed stirring and shearing in a homogenizer, forming small droplets dispersed in the solution, and the polymer network is dispersed on the metal surface and in the good solvent.

[0173] Handling of liquid metal-polymer mixed solutions:

[0174] The uniformly dispersed mixed solution is heated to remove the good solvent.

[0175] Specifically, the obtained mixed solutions of liquid metal and polymer of different systems are added into polytetrafluoroethylene watch glasses respectively, and then placed in an environment of 80° C. to remove the good solvent, thereby obtaining the metal gel.

[0176] In this step, initially, the liquid metal droplets are dispersed in the form of nanodroplets, in which the entangled polymer chains form physically cross-linked networks. These networks also capture a large amount of good solvent. As drying proceeds, the good solvent in these networks is gradually replaced by liquid metal. The micropores between the liquid metal droplets, which were originally filled with water, are transformed into nanopores filled with liquid metal. Eventually, the liquid metal fluid becomes the dominant component, forming a continuous structure, and the polymer network is embedded in this liquid metal continuum.

[0177] Example 6

[0178] like Figure 4 As shown, this embodiment discloses a method for preparing a metal gel, comprising the following steps:

[0179] Preparation of polymer solution:

[0180] 3.80 wt% to 4.80 wt% of iota carrageenan powder is dissolved in deionized water.

[0181] Specifically, at a temperature of 80° C., magnetic stirring is continued for 2 hours until the carrageenan is dissolved to obtain an iota carrageenan solution.

[0182] 3.80 wt% to 4.80 wt% of sodium alginate powder was dissolved in deionized water.

[0183] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until the alginate is dissolved to obtain a sodium alginate solution.

[0184] 3.80 wt% to 4.80 wt% of gellan gum powder is dissolved in deionized water.

[0185] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until the gellan gum is dissolved to obtain a gellan gum solution.

[0186] 3.80 wt% to 4.80 wt% of hyaluronic acid powder is dissolved in deionized water.

[0187] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until it is dissolved to obtain a hyaluronic acid solution.

[0188] 3.80 wt% to 4.80 wt% of poly(vinylidene fluoride-hexafluoropropylene) particles were dissolved in N-methylpyrrolidone.

[0189] Specifically, at a temperature of 25° C., magnetic stirring is continued for 2 hours until it is dissolved to obtain a poly(vinylidene fluoride-hexafluoropropylene) solution.

[0190] Preparation of liquid metal-polymer mixed solution:

[0191] The liquid metal gallium-indium alloy and the iota carrageenan solution are mixed in a weight ratio of 3:2, and then stirred and sheared at a speed of 10000 rpm to 15000 rpm for 10 to 15 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-indium alloy-iota carrageenan mixed solution;

[0192] The liquid metal gallium and the iota carrageenan solution are mixed in a weight ratio of 7:3, and then stirred and sheared at a speed of 10000 rpm to 15000 rpm for 10 to 15 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-iota carrageenan mixed solution;

[0193] The liquid metal gallium indium tin alloy and the iota carrageenan solution are mixed in a weight ratio of 7:3, and then stirred and sheared at a speed of 10000 rpm to 15000 rpm for 10 to 15 minutes at a temperature of 80° C. using a handheld homogenizer to obtain a gallium indium tin alloy-iota carrageenan mixed solution;

[0194] The liquid metal gallium-indium alloy and the sodium alginate solution are mixed in a weight ratio of 3:2, and then sheared at a speed of 10000 rpm to 15000 rpm for 5 to 10 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-sodium alginate mixed solution;

[0195] The liquid metal gallium-indium alloy and the gellan gum solution are mixed in a weight ratio of 3:2, and then stirred and sheared at a speed of 10000 rpm to 15000 rpm for 5 to 10 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-gellan gum mixed solution;

[0196] The liquid metal gallium-indium alloy and the hyaluronic acid solution are mixed in a weight ratio of 1:1, and then sheared at a speed of 10000 rpm to 15000 rpm for 5 to 10 minutes at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-hyaluronic acid mixed solution;

[0197] The liquid metal gallium-indium alloy and poly(vinylidene fluoride-hexafluoropropylene) solution are mixed in a weight ratio of 6:4, and then sheared at a speed of 10000rpm-15000rpm for 5-10 minutes at a temperature of 25°C using a handheld homogenizer to obtain a gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) mixed solution.

[0198] Specifically, in this step, the liquid metal undergoes high-speed stirring and shearing in a homogenizer, forming small droplets dispersed in the solution, and the polymer network is dispersed on the metal surface and in the good solvent.

[0199] Handling of liquid metal-polymer mixed solutions:

[0200] The uniformly dispersed mixed solution is heated to remove the good solvent.

[0201] Specifically, the obtained mixed solutions of liquid metal and polymer of different systems are added into polytetrafluoroethylene watch glasses respectively, and then placed in an environment of 60° C., and the good solvent is removed to obtain the metal gel.

[0202] In this step, initially, the liquid metal droplets are dispersed in the form of nanodroplets, in which the entangled polymer chains form physically cross-linked networks. These networks also capture a large amount of good solvent. As drying proceeds, the good solvent in these networks is gradually replaced by liquid metal. The micropores between the liquid metal droplets, which were originally filled with water, are transformed into nanopores filled with liquid metal. Eventually, the liquid metal fluid becomes the dominant component, forming a continuous structure, and the polymer network is embedded in this liquid metal continuum.

[0203] At present, there is no specific application of using liquid metal as the fluid phase in gel materials; in addition, in order to address the problems of incompatibility between the polymer gel network and the metal, structural phase separation and decreased mechanical properties that may exist when introducing a large amount of liquid metal into the gel, this scheme has developed a new gel material based on the gel system, in which liquid metal is used as the fluid phase in the gel, and the nano-scale dispersed three-dimensional porous polymer network is evenly and stably dispersed in the liquid metal fluid through the action of forces, thereby achieving high electronic conductivity and flexibility; and the performance of the material can be maintained stable when it undergoes physical deformation or is in different environments, solving the current problems of not using liquid metal as the fluid phase, poor compatibility between liquid metal and the polymer network, and low electronic conductivity of the gel material.

[0204] The above schematically describes the invention and its implementation methods, which is not restrictive. Without departing from the spirit or basic features of the invention, the invention can be implemented in other specific forms. What is shown in the accompanying drawings is only one of the implementation methods of the invention. The actual structure is not limited to this, and any figure mark in the claims should not limit the claims involved. Therefore, if a person of ordinary skill in the art is inspired by it, without departing from the purpose of the invention, a structural method and an embodiment similar to the technical solution are designed without creativity, which should all fall within the scope of protection of this patent. In addition, the word "including" does not exclude other elements or steps, and the word "one" before the element does not exclude the inclusion of "multiple" elements. The multiple elements stated in the product claim can also be implemented by one element through software or hardware. The words first, second, etc. are used to indicate names, and do not indicate any specific order.

Claims

1. A method for preparing a metal gel, comprising the steps of: Prepare polymer solution: add polymer powders to good solvents respectively, dissolve them and stir them evenly to obtain polymer solution; Preparing a liquid metal-polymer mixed solution: adding liquid metal to a polymer solution, and uniformly dispersing the mixed solution with a homogenizer to obtain a liquid metal-polymer mixed solution; Processing of liquid metal-polymer mixed solution: removing the good solvent from the uniformly dispersed mixed solution by heating or freeze-drying to obtain metal gel.

2. The method for preparing the metal gel according to claim 1, characterized in that: The steps of preparing the polymer solution include: preparing ι-type carrageenan solution; preparing sodium alginate solution; preparing gellan gum solution; preparing hyaluronic acid solution; preparing poly (vinylidene fluoride-hexafluoropropylene) solution.

3. The method for preparing the metal gel according to claim 2, characterized in that: The steps of preparing the iota carrageenan solution are specifically as follows: dissolving 0.80 wt% to 4.80 wt% of iota carrageenan powder in deionized water, and continuously stirring with a magnetic force for 2 hours at a temperature of 80° C. until the powder is dissolved, to obtain an iota carrageenan solution; The steps of preparing the sodium alginate solution are as follows: dissolving 0.80 wt% to 4.80 wt% of sodium alginate powder in deionized water, and continuously stirring the sodium alginate powder with a magnetic force at a temperature of 25° C. for 2 hours until the sodium alginate powder is dissolved to obtain the sodium alginate solution.

4. The method for preparing the metal gel according to claim 2, characterized in that: The steps of preparing the gellan gum solution are specifically as follows: dissolving 0.80 wt% to 4.80 wt% of gellan gum powder in deionized water, and continuously stirring with magnetic force for 2 hours at a temperature of 25° C. until the gellan gum powder is dissolved, to obtain the gellan gum solution; The steps of preparing the hyaluronic acid solution are specifically as follows: dissolving 0.80 wt% to 4.80 wt% of hyaluronic acid powder in deionized water, and continuously stirring with a magnetic force at a temperature of 25° C. for 2 hours until the hyaluronic acid powder is dissolved to obtain a hyaluronic acid solution; The specific steps of preparing the poly(vinylidene fluoride-hexafluoropropylene) solution are as follows: dissolving 0.80wt% to 4.80wt% of poly(vinylidene fluoride-hexafluoropropylene) particles in N-methylpyrrolidone, and continuously stirring with a magnetic force for 2 hours at a temperature of 25°C until it is dissolved to obtain a poly(vinylidene fluoride-hexafluoropropylene) solution.

5. The method for preparing the metal gel according to claim 1, characterized in that: The steps of preparing a liquid metal-polymer mixed solution include: preparing a gallium-indium alloy-ι-carrageenan mixed solution; preparing a gallium-ι-carrageenan mixed solution; preparing a gallium-indium-tin alloy-ι-carrageenan mixed solution; preparing a gallium-indium alloy-sodium alginate mixed solution; preparing a gallium-indium alloy-gellan gum mixed solution; preparing a gallium-indium alloy-hyaluronic acid mixed solution; preparing a gallium-indium alloy-poly (vinylidene fluoride-hexafluoropropylene) mixed solution.

6. The method for preparing the metal gel according to claim 5, characterized in that: The steps for preparing the liquid metal-polymer mixed solution are specifically as follows: The liquid metal gallium-indium alloy and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-indium alloy-iota carrageenan mixed solution; The liquid metal gallium and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 80° C. using a handheld homogenizer to obtain a gallium-iota carrageenan mixed solution; The liquid metal gallium indium tin alloy and the iota carrageenan solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 minutes to 15 minutes at a temperature of 80°C using a handheld homogenizer to obtain a gallium indium tin alloy-iota carrageenan mixed solution.

7. The method for preparing the metal gel according to claim 5 or 6, characterized in that: The steps of preparing the liquid metal-polymer mixed solution also include: The liquid metal gallium-indium alloy and the sodium alginate solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-sodium alginate mixed solution; The liquid metal gallium-indium alloy and the gellan gum solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred with a handheld homogenizer at a temperature of 25° C. and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min to obtain a gallium-indium alloy-gellan gum mixed solution; The liquid metal gallium-indium alloy and the hyaluronic acid solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 min to 15 min at a temperature of 25° C. using a handheld homogenizer to obtain a gallium-indium alloy-hyaluronic acid mixed solution; The liquid metal gallium-indium alloy and poly(vinylidene fluoride-hexafluoropropylene) solution are mixed in a weight ratio of 1:1 to 7:3, and then stirred and sheared at a speed of 8000 rpm to 15000 rpm for 5 minutes to 15 minutes at a temperature of 25°C using a handheld homogenizer to obtain a gallium-indium alloy-poly(vinylidene fluoride-hexafluoropropylene) mixed solution.

8. The method for preparing the metal gel according to claim 7, characterized in that: The specific steps for treating the liquid metal-polymer mixed solution are: The obtained liquid metal-polymer mixed solution was added into polytetrafluoroethylene watch glasses respectively, and the watch glasses were placed in an environment of 25° C. to 80° C. to remove the good solvent, thereby obtaining a metal gel.

9. A novel metal gel prepared according to the method for preparing a metal gel according to any one of claims 1 to 8, characterized in that: including liquid metals and polymer networks; Therein, liquid metal forms a continuum as the fluid phase of the gel; Nanoscale polymer networks use interactions to immobilize liquid metal fluids.

Citation Information

Patent Citations

  • Preparation method of liquid metal / chitosan derivative hydrogel film

    CN111647186A

  • Flexible conductive composite material based on liquid metal and preparation method thereof

    CN114974727A

  • Liquid metal microgel and preparation method and application thereof

    CN115073764A

  • Method for forming three-dimensional macrostructure using liquid metal by means of suspension printing

    WO2018045968A1

Cited By

  • Metal gel with high conductivity and strong interface adhesion as well as preparation method and application of metal gel

    CN121379108A

  • Liquid metal gel as well as preparation method and application thereof

    CN121669105A