Phthalonitrile / phenolic aldehyde aerogel as well as preparation method and application thereof

By designing and regulating molecular structure, combining crosslinking agents and precise process control, phthalonitrile/phenol aerogels with high mechanical strength and thermal stability are prepared, solving the lack of single resin performance and traditional aerogel environment. The pollution problem has achieved a comprehensive improvement in the performance of building insulation materials.

CN119019750APending Publication Date: 2024-11-26JILIN SHENGLONG ENVIRONMENTAL TECHNOLOGY CONSULTING SERVICE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411319001.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, single phenolic resin has poor ablation resistance and low carbon residual rate. Single phthalene resin may have incomplete curing or brittleness problems, and traditional aerogels use organic solvents to cause toxicity and environmental pollution. question.

Method used

By designing and regulating the molecular structure of phthalene and phenolic resin, chemical crosslinking of allyl phthalene monomer and phenolic resin is adopted to combine hexamethylenetetramine and (3-aminophenoxy) As a crosslinking agent, a phthalene/phenyl aerogel with enhanced mechanical strength and thermal stability was prepared, and a uniform pore distribution was obtained by precise control of the sol-gel process and drying process. Compound aerogel with good nanofiller dispersibility.

Benefits of technology

It significantly improves the mechanical strength and thermal stability of the aerogel, improves the overall performance of the material, solves the limitations of traditional single aerogels, and provides better performance of building insulation materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019750A_ABST
    Figure CN119019750A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of building thermal insulation materials, and particularly discloses a phthalonitrile / phenolic aldehyde aerogel and a preparation method and application thereof, and the preparation method comprises preparation of an allyl phthalonitrile monomer, preparation of a phenolic resin prepolymer and preparation of the phthalonitrile / phenolic aldehyde aerogel. The preparation method of the phthalonitrile / phenolic aldehyde aerogel not only solves the limitation of the traditional single aerogel, but also realizes the comprehensive improvement of the material performance through molecular design and process optimization, and provides a new possibility for application in preparation of building thermal insulation materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building thermal insulation materials, in particular to phthalonitrile / phenolic aerogel and a preparation method and application thereof. Background Art

[0002] High-performance, lightweight, long-lasting ablation-resistant and heat-resistant composite materials are important components of key components of national defense weapons and equipment and high-end aerospace equipment. Therefore, for low-density ablative materials, domestic and foreign research institutions and heat protection academic circles have conducted extensive research on reducing the volume density of ablative materials and improving ablation resistance and thermal insulation performance. With the increasing requirements for material performance in industries such as aerospace, materials with better thermal stability, mechanical properties and chemical stability are needed. Single phenolic resins have problems such as poor ablation resistance and low residual carbon rate, and single phthalonitrile resins may have problems with incomplete curing or brittleness. In addition, traditional aerogels use organic solvents, which have problems such as toxicity and environmental pollution.

[0003] Therefore, it is urgent to design and regulate the molecular structure of phthalonitrile resin and phenolic resin, such as by introducing different functional groups or adjusting the molecular chain structure, to obtain the desired properties. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a phthalonitrile / phenolic aerogel and a preparation method and application thereof.

[0005] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0006] One of the purposes of the present invention is to provide a method for preparing phthalonitrile / phenolic aerogel, comprising the following steps:

[0007] S1. Preparation of allyl phthalonitrile monomer: Take 3 parts by weight of bisphenol monomer, 3 parts by weight of anhydrous K 2 CO 3 , 10 parts by weight of dimethyl sulfoxide are added to the flask, the flask is placed in an oil bath at 90°C for heating and heat preservation and magnetic stirring is performed, and nitrogen and condensed water are introduced for protection. After one hour of reaction, 4 parts by weight of 4-PN are added to the flask and the reaction is continued for 6 hours, and then the heating is turned off and cooled to room temperature; the cooled black-red mixed solution is slowly added to a 0.05 mol / L mixed solution of dilute hydrochloric acid and ice water for precipitation, and the resin is stirred rapidly to allow the resin to be fully precipitated to remove anhydrous potassium carbonate and dimethyl sulfoxide; then the mixed solution after the precipitation is allowed to stand for 1 hour is vacuum filtered to obtain a solid crude product, and the filtrate is washed with deionized water until the filtrate is neutral, and the filtered product is placed in a vacuum drying oven at 30°C and dried for 12 hours to obtain allyl bisphenol A type phthalonitrile resin monomer powder;

[0008] S2, preparation of phenolic resin prepolymer: take 60g phenol, 68g formaldehyde, 1.72g oxalic acid and mix them evenly; heat to 95°C, react for about 2 hours, keep constant temperature at 95°C, and continue to react for 40 minutes; start vacuum dehydration, and reduce the temperature to 55°C; vacuum dehydration for about 1 hour, continue to react for 50 minutes, and the reaction temperature reaches 90°C to obtain a phenolic resin prepolymer;

[0009] S3. Preparation of phthalonitrile / phenolic aerogel: Take ethanol, allyl bisphenol A type phthalonitrile resin monomer powder and phenolic resin prepolymer in a mass ratio of 8:1:1, mix them evenly, and stir at 60°C and 600rpm for 1h to completely dissolve; then add hexamethylenetetramine and (3-aminophenoxy)phenyl sulfone to the above-mentioned mixed solution in sequence, the addition amount of hexamethylenetetramine is 15wt%, and the addition amount of (3-aminophenoxy)phenyl sulfone is 3wt%; stir at 60°C and 600rpm for 1-1.5h to completely dissolve; finally, transfer the sample to a glass bottle, seal it with raw tape, place it in an oven at 80°C for reaction for 48h, and then take it out; dry it at room temperature for 24h, and then dry it at 80°C for 24h to obtain phthalonitrile / phenolic aerogel.

[0010] Furthermore, the bisphenol monomer is 2,2'-diallylbisphenol A.

[0011] The second object of the present invention is to provide a phthalonitrile / phenolic aerogel prepared by the above method.

[0012] The third object of the present invention is to provide an application of phthalonitrile / phenolic aerogel in the preparation of building thermal insulation materials.

[0013] Compared with the prior art, the present invention utilizes the chemical reactivity of phthalonitrile resin and phenolic resin to achieve chemical crosslinking between the two resins. The construction of this crosslinked network not only enhances the mechanical strength and thermal stability of the aerogel, but also significantly improves the overall performance of the material through molecular-level interactions; in addition, the present invention also explores the influence of curing conditions on the performance of composite resin aerogels; finally, the present invention also characterizes the microstructure of the composite resin aerogel, and uses a scanning electron microscope (SEM) to observe the pore structure of the aerogel and the dispersion of nanofillers. The research results confirm that by precisely controlling the sol-gel process and drying process, a composite aerogel with uniform pore distribution and good nanofiller dispersion can be obtained.

[0014] In summary, the preparation method of phthalonitrile / phenolic aerogel of the present invention not only solves the limitations of traditional single aerogels, but also achieves a comprehensive improvement in material performance through molecular design and process optimization, providing new possibilities for its application in the preparation of building thermal insulation materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a scanning electron microscope image of the phthalonitrile / phenolic composite aerogel prepared in Example 1. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the invention.

[0017] Example 1

[0018] (1) Preparation of phthalonitrile / phenolic composite resin: 30.8 g of allyl bisphenol A, 52.3 g of phenol, 68 g of formaldehyde, and 1.72 g of oxalic acid were heated to 95 degrees and reacted for about 3 hours. The temperature was kept constant at 95 degrees and the reaction continued for 40 minutes. Vacuum dehydration was started and the temperature was lowered to about 55 degrees. Vacuum dehydration was carried out for about 1 hour. Then 35.6 g of anhydrous K 2 CO 3 , 300ml dimethyl sulfoxide, put the flask into a 90℃ oil bath to heat and keep warm, adjust the magnetic stirrer to a suitable speed, and introduce nitrogen and condensed water for protection. After one hour of reaction, add 82.3g 4-PN into the flask and continue to react for 6 hours, then turn off the heating and cool to room temperature. Slowly add the cooled black-red mixed solution into a 0.05mol / L mixed solution of dilute hydrochloric acid and ice water to precipitate, and stir quickly to allow the resin to precipitate fully to remove raw materials such as anhydrous potassium carbonate and DMSO. Then, the mixed solution after the precipitation is allowed to stand for 1 hour is vacuum filtered to obtain a solid crude product, and washed with deionized water until the filtrate is neutral. The filtered product is placed in a vacuum drying oven at 30℃ and dried for 12 hours to finally obtain allyl bisphenol A type phthalonitrile resin monomer powder.

[0019] (2) Preparation of phthalonitrile / phenolic aerogel: Resin dissolution: Weigh a certain mass of ethanol (EtOH), then add phthalonitrile / phenolic resin in a ratio of 8:2, and stir at 60°C, 600rpm for 1h to completely dissolve. Crosslinker dissolution: Add 15wt% hexamethylenetetramine (HMTA) and 3wt% (3-aminophenoxy)phenyl sulfone to the above mixed solution, and stir at 60°C, 600rpm for 1 to 1.5h to completely dissolve. Gelation: Transfer the sample to a glass bottle, seal it with raw tape, place it in an oven at 80°C for 48h, and then take it out. Drying strategy: Dry at room temperature for 24h, and then dry at 80°C for 24h to obtain phthalonitrile / phenolic aerogel sample 1. The reaction equation of phthalonitrile / phenolic composite resin is as follows:

[0020]

[0021] The microstructure of the phthalonitrile / phenolic aerogel sample 1 was characterized. The pore structure and dispersion of the nanofiller of the phthalonitrile / phenolic aerogel sample 1 were observed using a scanning electron microscope (SEM). Figure 1 As shown by Figure 1 It can be seen that by precisely controlling the sol-gel process and drying process, a composite aerogel with uniform pore distribution and good nanofiller dispersion can be obtained.

[0022] Example 2

[0023] (1) Synthesis of allyl phthalonitrile monomer: 61.61 g of allyl bisphenol A and 55.2 g of anhydrous K 2 CO 3 , 200ml of dimethyl sulfoxide and a magnetic stirrer are added to a three-necked or four-necked flask with a condenser in sequence, the flask is placed in an 80°C oil bath for heating and heat preservation, and the magnetic stirrer is adjusted to a suitable speed, while nitrogen and condensed water are introduced for protection. After one hour of reaction, 69.2g of 4-PN is added to the flask and the reaction is continued for 7 hours, then the heating is turned off and cooled to room temperature. The molar ratio of allyl bisphenol A, anhydrous K2CO3, and 4-PN is 1:2:2, and allyl bisphenol A and K2CO3 are slightly excessive. The cooled black-red mixed solution is slowly added to a 0.05mol / L dilute hydrochloric acid ice water mixed solution for precipitation, and the resin is stirred rapidly to fully precipitate to remove raw materials such as anhydrous potassium carbonate and DMSO. Then, after the precipitate was allowed to stand for 1 hour, the mixed solution was vacuum filtered to obtain a solid crude product, and the solid crude product was washed with deionized water until the filtrate was neutral. The filtered product was placed in a vacuum drying oven at 30° C. and dried for 12 hours to finally obtain 67.8 g of allyl bisphenol A type phthalonitrile resin monomer powder.

[0024] (2) Phenolic resin prepolymer: Add 60g phenol, 68g formaldehyde, and 1.72g oxalic acid; heat to 95 degrees, and react for about 2 hours. Keep the temperature at 95 degrees, continue to react for 40 minutes, start vacuum dehydration, and reduce the temperature to about 55 degrees. Vacuum dehydration for about 1 hour, continue to react for about 50 minutes, and when the reaction temperature reaches 90 degrees, start to prepare for discharge.

[0025] (3) Preparation of phthalonitrile / phenolic aerogel: Resin dissolution: Weigh 8 parts of ethanol (EtOH), then add 1 part of allyl phthalonitrile monomer powder and 1 part of phenolic resin powder, and stir at 60°C, 600 rpm for 1 hour to completely dissolve. Crosslinker dissolution: Add 15wt% hexamethylenetetramine (HMTA) and 3wt% (3-aminophenoxy)phenyl sulfone to the above mixed solution, and stir at 60°C, 600 rpm for 1 to 1.5 hours to completely dissolve. Gelation: Transfer the sample to a glass bottle, seal it with raw tape, place it in an oven at 80°C for 48 hours, and then take it out. Drying strategy: Dry at room temperature for 24 hours, and then dry at 80°C for 24 hours to obtain phthalonitrile / phenolic aerogel sample 2. The reaction equation of allyl phthalonitrile monomer / phenolic resin powder is as follows:

[0026]

[0027] Example 3

[0028] The other conditions are the same as those in Example 1, except that in step (1), the bisphenol monomer used is bisphenol F. Finally, the phthalonitrile / phenolic aerogel sample 3 is obtained. The structure of bisphenol F is shown in the figure below:

[0029]

[0030] Example 4

[0031] The other conditions are the same as those in Example 1, except that in step (1), the bisphenol monomer used is bisphenol A. Finally, phthalonitrile / phenolic aerogel sample 4 is obtained. The structure of bisphenol A is shown in the figure below:

[0032]

[0033] Example 5

[0034] The other conditions are the same as those in Example 1, except that in step (1), the bisphenol monomer used is an adamantane-type bisphenol monomer. Finally, a phthalonitrile / phenolic aerogel sample 5 is obtained. The structure of the adamantane-type bisphenol monomer is shown in the figure below:

[0035]

[0036] Example 6

[0037] Other conditions were the same as those in Example 1, except that in the preparation of the phthalonitrile / phenolic resin aerogel, the ratio of ethanol to phthalonitrile / phenolic resin was 7:3.

[0038] Preparation of phthalonitrile / phenolic aerogel: Resin dissolution: Weigh a certain mass of ethanol (EtOH), then add phthalonitrile / phenolic resin in a ratio of 7:3, and stir at 60°C, 600rpm for 1h to completely dissolve. Crosslinker dissolution: Add 15wt% hexamethylenetetramine (HMTA) and 3wt% (3-aminophenoxy)phenyl sulfone to the above mixture, and stir at 60°C, 600rpm for 1 to 1.5h to completely dissolve. Gelation: Transfer the sample to a glass bottle, seal it with raw tape, place it in an oven at 80°C for reaction for 48h, and then take it out. Drying strategy: Dry at room temperature for 24h, and then dry at 80°C for 24h to obtain phthalonitrile / phenolic aerogel sample 6.

[0039] Example 7

[0040] Other conditions were the same as those in Example 1, except that in the preparation of the phthalonitrile / phenolic aerogel, the curing agent contents used were 20 wt % hexamethylenetetramine (HMTA) and 3.5 wt % (3-aminophenoxy)phenyl sulfone, respectively.

[0041] Preparation of phthalonitrile / phenolic aerogel: Resin dissolution: Weigh a certain mass of ethanol (EtOH), then add phthalonitrile / phenolic resin in a ratio of 7:3, and stir at 60°C, 600rpm for 1h to completely dissolve. Crosslinker dissolution: Add 20wt% hexamethylenetetramine (HMTA) and 3.5wt% (3-aminophenoxy)phenyl sulfone to the above mixture, and stir at 60°C, 600rpm for 1 to 1.5h to completely dissolve. Gelation: Transfer the sample to a glass bottle, seal it with raw tape, place it in an oven at 80°C for 48h, and then take it out. Drying strategy: Dry at room temperature for 24h, and then dry at 80°C for 24h to obtain phthalonitrile / phenolic aerogel sample 7.

[0042] The prepared phthalonitrile / phenolic aerogel samples 1 to 7 were respectively taken, and their properties were tested using a common testing method in the art. The test results are shown in Table 1.

[0043] Table 1

[0044]

[0045] It can be seen from Table 1 that the phthalonitrile / phenolic aerogel prepared in the present invention exhibits significant performance advantages.

[0046] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. A method for preparing phthalonitrile / phenolic aerogel, characterized in that: The following steps are involved: S1. Preparation of allyl phthalonitrile monomer: 3 parts by weight of bisphenol monomer, 3 parts by weight of anhydrous K2CO3, and 10 parts by weight of dimethyl sulfoxide are added to a flask, and the flask is placed in an oil bath at 90°C for heating and heat preservation and magnetic stirring, while nitrogen and condensed water are introduced for protection. After one hour of reaction, 4 parts by weight of 4-PN are added to the flask and the reaction is continued for 6 hours, and then the heating is turned off and cooled to room temperature; the cooled black-red mixed solution is slowly added to a 0.05 mol / L mixed solution of dilute hydrochloric acid and ice water for precipitation, and the resin is stirred rapidly to fully precipitate to remove anhydrous potassium carbonate and dimethyl sulfoxide; then the mixed solution after the precipitation is allowed to stand for 1 hour is vacuum filtered to obtain a solid crude product, and the filtrate is washed with deionized water until the filtrate is neutral, and the filtered product is placed in a vacuum drying oven at 30°C for 12 hours to obtain an allyl bisphenol A type phthalonitrile resin monomer powder; S2, preparation of phenolic resin prepolymer: take 60g phenol, 68g formaldehyde, 1.72g oxalic acid and mix them evenly; heat to 95°C, react for about 2 hours, keep constant temperature at 95°C, and continue to react for 40 minutes; start vacuum dehydration, and reduce the temperature to 55°C; vacuum dehydration for about 1 hour, continue to react for 50 minutes, and the reaction temperature reaches 90°C to obtain a phenolic resin prepolymer; S3. Preparation of phthalonitrile / phenolic aerogel: Take ethanol, allyl bisphenol A type phthalonitrile resin monomer powder and phenolic resin prepolymer in a mass ratio of 8:1:1, mix them evenly, and stir at 60°C and 600rpm for 1h to completely dissolve; then add hexamethylenetetramine and (3-aminophenoxy)phenyl sulfone to the above-mentioned mixed solution in sequence, the addition amount of hexamethylenetetramine is 15wt%, and the addition amount of (3-aminophenoxy)phenyl sulfone is 3wt%; stir at 60°C and 600rpm for 1-1.5h to completely dissolve; finally, transfer the sample to a glass bottle, seal it with raw tape, place it in an oven at 80°C for reaction for 48h, and then take it out; dry it at room temperature for 24h, and then dry it at 80°C for 24h to obtain phthalonitrile / phenolic aerogel.

2. The method for preparing phthalonitrile / phenolic aerogel according to claim 1, characterized in that: The bisphenol monomer is 2,2'-diallylbisphenol A.

3. A phthalonitrile / phenolic aerogel prepared by the method according to claim 1 or 2.

4. Use of the phthalonitrile / phenolic aerogel as claimed in claim 3 in the preparation of building thermal insulation materials.

Citation Information

Cited By

  • Phthalonitrile modified phenolic aerogel as well as preparation method and application thereof

    CN119859311A