Anti-static foam partition plate and preparation method thereof

Through the combination of phenolic resin and polyurethane polyethylene glycol prepolymerizer and the treatment of modified graphene dispersion, the problems of unstable anti-static properties and insufficient mechanical properties of the existing anti-static foam partition are solved, and efficient anti-static properties are achieved and improve mechanical properties, simplify processes and reduce costs.

CN119019754AInactive Publication Date: 2024-11-26SHANGHAI JIUWU ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410982177.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing anti-static foam partition technology has problems such as unstable anti-static properties, affecting mechanical properties and aesthetics, and the preparation process is complex and the cost is high.

Method used

The phenolic resin, surfactant, polyurethane polyethylene glycol prepolymer and foaming agent are mixed and molded, followed by soaking and coating-modified graphene dispersion to form an anti-static foam partition.

Benefits of technology

The mechanical properties and long-term anti-static ability of the foam partition are improved, and the stable excellent mechanical properties and anti-static properties are ensured, while avoiding the problems of anti-static agent precipitation and conductive fillers changing the structure of the bubble body.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of foam partition plates, in particular to an anti-static foam partition plate and a preparation method thereof.The preparation method comprises the steps that phenolic resin, a surfactant, a polyurethane polyethylene glycol prepolymerization agent and a foaming agent are mixed and stirred evenly, then a curing agent is added, the mixture is rapidly stirred evenly, then the mixture is moved into a mold to be pressed, then the mixture is soaked in modified graphene dispersion liquid, and the anti-static foam partition plate is obtained. And after drying, coating a layer of modified graphene dispersion liquid on the surface of the foam partition plate by a casting method, and drying to obtain the anti-static foam partition plate. Wherein a polyurethane polyethylene glycol prepolymerization agent prepared from polyethylene glycol, isocyanate and tin octoate is mixed with phenolic resin, so that the mechanical property of the foam partition plate can be improved; after the vinyl triethyl silane is modified, the adsorption capacity of the graphene can be improved. During soaking, the interaction of the modified phenolic resin and the modified graphene can further improve the anti-static capacity and the mechanical property of the foam partition plate. Therefore, the anti-static foam partition plate prepared by the invention has excellent mechanical properties and anti-static capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foam partitions, and in particular to an antistatic foam partition and a preparation method thereof. Background Art

[0002] In current industrial production and product packaging, foam partitions are widely used as a lightweight material with good buffering performance. Especially in the field of electronic product packaging that is sensitive to static electricity, such as integrated circuits and communication equipment, foam partitions not only need to have good buffering performance, but also need to have excellent antistatic performance and fire resistance. And phenolic foam board happens to have many excellent properties, such as phenolic foam board has a uniform closed-cell structure, low thermal conductivity, high fire resistance, flame retardant, low smoke characteristics and excellent heat resistance. Therefore, phenolic foam has better thermal insulation performance and has incomparable fire resistance, but phenolic foam has relatively poor mechanical properties and antistatic ability still needs to be improved. Existing antistatic foam partition technical solutions mostly rely on adding antistatic agents or conductive fillers to achieve antistatic function, and these methods have many shortcomings. First, by adding antistatic agents such as quaternary ammonium salts and phosphate compounds, although the antistatic performance of the product can be improved in a short period of time, the antistatic agent is easily precipitated during long-term use, resulting in a decrease in antistatic performance. Secondly, although the method of adding conductive fillers such as carbon black can give the product long-term stable antistatic properties, it will change the foam structure of the foam plastic, affect the mechanical properties of the product, and cause the product color to darken, affecting the appearance. In addition, the existing technical solutions also generally have problems such as complex preparation process and high cost.

[0003] Patent technology document CN114835940A discloses a powder-resistant phenolic resin foam and a preparation method thereof. The preparation method of the modified phenolic resin of the invention is as follows: first, the hydroxyl group of p-hydroxybenzoic acid is protected by tert-butyldimethylsilyl chloride, and further connected to polyethylene glycol by esterification reaction, the protective group of the hydroxyl group is removed, and finally the modified phenolic resin is synthesized by reacting with acetaldehyde; the preparation of the powder-resistant phenolic resin foam is as follows: the modified phenolic resin, emulsifier, foaming agent and inorganic filler are mixed and stirred evenly, then a curing agent is quickly added and stirred evenly, and then transferred into a mold for compression molding to obtain the powder-resistant phenolic resin foam. The powder-resistant phenolic resin foam prepared by the invention has good mechanical properties, but the antistatic ability still needs to be improved.

[0004] Patent technical document 113388215B discloses an antistatic PVC foam and a preparation method thereof. The preparation method of the antistatic PVC foam of the invention is to first prepare conductive mica powder with mica powder, potassium antimonate, polyoxyethylene alkanolamide, sodium dodecyl diphenyl ether disulfonate and polyethylene glycol, and then prepare antistatic PVC foam with PVC resin, isocyanate, foaming agent, acid anhydride, epoxy compound, octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, stabilizer and conductive mica powder. The antistatic PVC foam prepared by the invention has a certain antistatic ability, but it is flammable.

[0005] Therefore, according to the above-mentioned related technologies, it is urgent to develop an antistatic foam separator and a preparation method thereof. Summary of the invention

[0006] In view of this, the purpose of the present invention is to provide an antistatic foam partition and a preparation method thereof, so as to improve the mechanical properties and antistatic ability of the foam partition in the prior art.

[0007] Based on the above purpose, the present invention provides an antistatic foam partition and a preparation method thereof.

[0008] A method for preparing an antistatic foam partition comprises the following steps:

[0009] Step S1. Mix the phenolic resin, surfactant, polyurethane polyethylene glycol prepolymer and foaming agent, stir evenly to obtain a foaming liquid;

[0010] Step S2. quickly add a curing agent to the foaming liquid, stir it quickly and evenly, and then transfer it into a mold for compression molding to obtain a foam partition;

[0011] Step S3. Soaking the foam partition in the modified graphene dispersion and drying it to obtain a pretreated foam partition;

[0012] Step S4. uniformly coating the surface of the pretreated foam partition with a layer of modified graphene dispersion by casting, and drying to obtain an antistatic foam partition;

[0013] The polyurethane polyethylene glycol prepolymer is prepared from the following raw materials in parts by weight: 6-7.5 parts of polyethylene glycol, 3-3.5 parts of isocyanate, and 1-1.5 parts of tin octoate;

[0014] The modified graphene is obtained by grafting graphene with vinyltriethylsilane.

[0015] Preferably, the surfactant in step S1 is any one of Tween 60 and Tween 80 or a combination thereof, and the foaming agent is any one of n-pentane, isopentane and n-hexane or a combination thereof; and the curing agent in step S2 is any one of phosphoric acid and p-toluenesulfonic acid or a combination thereof.

[0016] Preferably, the mass ratio of the phenolic resin, surfactant, polyether polyol reaction solution and foaming agent in step S1 is 95-100:4.5-6:10-11.5:4.5-5.0.

[0017] Preferably, the mass ratio of the foaming liquid to the curing agent in step S2 is 100-105:13-17.

[0018] Preferably, the molding process in step S2 is: first at a temperature of 75-90°C for 10-15 minutes, and then curing at 50-65°C for 30-35 minutes; the soaking time in step S3 is 30-45 minutes, and the temperature during the drying process is 35-40°C; the temperature during the drying process in step S4 is 35-40°C.

[0019] Preferably, the preparation method of the polyurethane polyethylene glycol prepolymer is as follows:

[0020] The polyethylene glycol is evacuated with a vacuum oil pump at 110-120°C to remove moisture from the polyethylene glycol; then nitrogen is introduced, and the temperature is cooled to 45-50°C, isocyanate is added, and the temperature is adjusted to maintain the system temperature at 75-80°C. After the reaction, tin octoate is added, and the reaction is continued for 1-1.5h, and the temperature is cooled to 35-40°C, the material is discharged, nitrogen is filled, and then sealed to obtain a polyurethane polyethylene glycol prepolymer.

[0021] Preferably, the preparation method of the modified graphene dispersion is as follows:

[0022] Step A1. Mix water, ethanol and vinyl triethylsilane, and ultrasonically vibrate for 5-10 minutes to obtain a mixed solution;

[0023] Step A2. Add water to the graphene, stir evenly, then add the mixed solution at 75-80° C., reflux for 4-4.5 hours, cool to 25-30° C., and then wash with deionized water 2-3 times to obtain modified graphene;

[0024] Step A3. Add water to the modified graphene to obtain a modified graphene dispersion with a mass fraction of 4.5%-5%.

[0025] Preferably, the mass ratio of water, ethanol and vinyltriethylsilane in step A1 is 3.5-4:35-38:8-11.

[0026] Preferably, the mass ratio of graphene, water and mixed liquid in step A2 is 7-10:185-190:45-50.

[0027] An antistatic foam partition is prepared by the above preparation method.

[0028] Beneficial effects of the present invention:

[0029] The present invention provides an antistatic foam partition and a preparation method thereof. The polyurethane polyethylene glycol prepolymer used in the present invention can improve the mechanical properties of the foam partition after being mixed with the phenolic resin, and the modified graphene not only has long-term antistatic ability, but can also interact with the modified phenolic resin in the foam partition to further improve the antistatic ability and mechanical properties of the foam partition; the graphene also has good adsorption capacity after modification, and the method of first dipping and then coating used in the present invention can also further improve the adsorption capacity of the modified graphene coating on the surface of the antistatic foam partition. Therefore, the antistatic foam partition prepared by the present invention has long-term stable excellent mechanical properties and antistatic ability. DETAILED DESCRIPTION

[0030] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0031] Embodiment 1: A method for preparing an antistatic foam partition comprises the following steps:

[0032] Step S1. 6 g of polyethylene glycol was evacuated with a vacuum oil pump at 110°C to remove the moisture in the polyethylene glycol; then nitrogen was passed through, and the temperature was cooled to 45°C, 3 g of isocyanate was added, and the temperature was adjusted to maintain the system temperature at 75°C. After reacting for 1 hour, 1 g of tin octoate was added, and the reaction was continued for another 1 hour, and the temperature was cooled to 35°C, the material was discharged, nitrogen was filled, and then sealed to obtain a polyurethane polyethylene glycol prepolymer:

[0033] Step S2. 95 g of phenolic resin, 4.5 g of Tween 60, 10 g of polyurethane polyethylene glycol prepolymer and 4.5 g of n-pentane were mixed and stirred to obtain a foaming liquid;

[0034] Step S3. 13 g of phosphoric acid was quickly added to 100 g of the foaming liquid, and the mixture was rapidly stirred at 75° C. for 10 min, and then transferred into a mold, and molded at 50° C. for 30 min to obtain a foam partition;

[0035] Step S4. 3.5 g of water, 35 g of ethanol and 8 g of vinyl triethyl silane were mixed and ultrasonically vibrated for 5 min to obtain a mixed solution; 185 g of water was added to 7 g of graphene and stirred evenly, and then 45 g of the mixed solution was added to reflux at 75 ° C for 4 h, cooled to 25 ° C, and then washed twice with deionized water, and water was added to obtain a modified graphene dispersion with a mass fraction of 4.5%;

[0036] Step S5. Soaking the foam separator in the modified graphene dispersion for 30 minutes, and drying at 35° C. to obtain a pretreated foam separator;

[0037] Step S6. Use a casting method to evenly coat a layer of modified graphene dispersion on the surface of the pretreated foam partition, and dry it at 35° C. to obtain an antistatic foam partition.

[0038] Embodiment 2: A method for preparing an antistatic foam partition comprises the following steps:

[0039] Step S1. 6.5 g of polyethylene glycol was evacuated with a vacuum oil pump at 115 ° C to remove the moisture in the polyethylene glycol; then nitrogen was passed through, and the temperature was cooled to 46 ° C, 3.1 g of isocyanate was added, and the temperature was adjusted to maintain the system temperature at 76 ° C. After reacting for 1.1 hours, 1.1 g of tin octoate was added, and the reaction was continued for 1.1 hours, and the temperature was cooled to 36 ° C, the material was discharged, nitrogen was filled, and then sealed to obtain a polyurethane polyethylene glycol prepolymer:

[0040] Step S2. 96 g of phenolic resin, 4.6 g of Tween 60, 10.5 g of polyurethane polyethylene glycol prepolymer and 4.6 g of n-pentane were mixed and stirred to obtain a foaming liquid;

[0041] Step S3. 14 g of phosphoric acid was quickly added to 101 g of the foaming liquid, and the mixture was rapidly stirred at 80° C. for 11 min, and then transferred into a mold, and molded at 55° C. for 31 min to obtain a foam partition;

[0042] Step S4. 3.6 g of water, 36 g of ethanol and 9 g of vinyltriethylsilane were mixed and ultrasonically vibrated for 6 min to obtain a mixed solution; 186 g of water was added to 8 g of graphene and stirred evenly, and then 46 g of the mixed solution was added to reflux at 76 ° C for 4.1 h, cooled to 26 ° C, and then washed twice with deionized water, and water was added to obtain a modified graphene dispersion with a mass fraction of 4.6%;

[0043] Step S5. Soaking the foam separator in the modified graphene dispersion for 35 minutes, and drying at 36° C. to obtain a pretreated foam separator;

[0044] Step S6. Use a casting method to evenly coat a layer of modified graphene dispersion on the surface of the pretreated foam partition, and dry it at 36° C. to obtain an antistatic foam partition.

[0045] Embodiment 3: A method for preparing an antistatic foam partition comprises the following steps:

[0046] Step S1. 7g of polyethylene glycol was evacuated with a vacuum oil pump at 117°C to remove moisture from the polyethylene glycol; nitrogen was then passed through, and the temperature was cooled to 48°C, 3.4g of isocyanate was added, and the temperature was adjusted to maintain the system temperature at 78°C. After reacting for 1.4h, 1.4g of tin octoate was added, and the reaction was continued for another 1.4h, the temperature was cooled to 38°C, the material was discharged, nitrogen was filled, and then sealed to obtain a polyurethane polyethylene glycol prepolymer:

[0047] Step S2. 98 g of phenolic resin, 5.5 g of Tween 80, 11 g of polyurethane polyethylene glycol prepolymer and 4.8 g of isopentane were mixed and stirred to obtain a foaming liquid;

[0048] Step S3. 15 g of p-toluenesulfonic acid was quickly added to 104 g of the foaming liquid, and the mixture was rapidly stirred at 85° C. for 14 min, and then transferred into a mold, and molded at 55° C. for 34 min to obtain a foam partition;

[0049] Step S4. 3.8 g of water, 37 g of ethanol and 10 g of vinyl triethyl silane were mixed and ultrasonically vibrated for 8 min to obtain a mixed solution; 188 g of water was added to 9 g of graphene and stirred evenly, and then 48 g of the mixed solution was added to reflux at 78 ° C for 4.4 h, cooled to 28 ° C, and then washed with deionized water 3 times, and water was added to obtain a modified graphene dispersion with a mass fraction of 4.8%;

[0050] Step S5. Soaking the foam separator in the modified graphene dispersion for 34 minutes, and drying at 38° C. to obtain a pretreated foam separator;

[0051] Step S6. Use a casting method to evenly coat a layer of modified graphene dispersion on the surface of the pretreated foam partition, and dry it at 38° C. to obtain an antistatic foam partition.

[0052] Embodiment 4: A method for preparing an antistatic foam partition comprises the following steps:

[0053] Step S1. 7.5 g of polyethylene glycol was evacuated with a vacuum oil pump at 120°C to remove moisture from the polyethylene glycol; nitrogen was then passed through, and the temperature was cooled to 50°C, 3.5 g of isocyanate was added, and the temperature was adjusted to maintain the system temperature at 80°C. After reacting for 1.5 hours, 1.5 g of tin octoate was added, and the reaction was continued for another 1.5 hours, and the temperature was cooled to 40°C, the material was discharged, nitrogen was filled, and then sealed to obtain a polyurethane polyethylene glycol prepolymer:

[0054] Step S2. 100 g of phenolic resin, 6 g of Tween 80, 11.5 g of polyurethane polyethylene glycol prepolymer and 5.0 g of n-hexane were mixed and stirred to obtain a foaming liquid;

[0055] Step S3. 17 g of p-toluenesulfonic acid was quickly added to 105 g of the foaming liquid, and the mixture was rapidly stirred at 90° C. for 15 min, and then transferred into a mold, and molded at 65° C. for 35 min to obtain a foam partition;

[0056] Step S4. 4 g of water, 38 g of ethanol and 11 g of vinyl triethyl silane were mixed and ultrasonically oscillated for 10 min to obtain a mixed solution; 190 g of water was added to 10 g of graphene and stirred evenly, and then 50 g of the mixed solution was added to reflux at 80 ° C for 4.5 h, cooled to 30 ° C, and then washed with deionized water 3 times, and water was added to obtain a modified graphene dispersion with a mass fraction of 5%;

[0057] Step S5. Soaking the foam partition in the modified graphene dispersion for 45 minutes, and drying at 40° C. to obtain a pretreated foam partition;

[0058] Step S6. Use a casting method to evenly coat a layer of modified graphene dispersion on the surface of the pretreated foam partition, and dry it at 40° C. to obtain an antistatic foam partition.

[0059] Comparative Example 1:

[0060] Compared with Example 1, the present comparative example does not add polyurethane polyethylene glycol prepolymer during the preparation of the antistatic foam partition, and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally the antistatic foam partition is obtained.

[0061] Comparative Example 2:

[0062] Compared with Example 1, this comparative example only replaces the "modified graphene dispersion" with the "ordinary graphene dispersion", and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally an antistatic foam partition is obtained.

[0063] Comparative Example 3: A method for preparing an antistatic foam partition, comprising the following steps:

[0064] Step S1. 6 g of polyethylene glycol was evacuated with a vacuum oil pump at 110°C to remove the moisture in the polyethylene glycol; then nitrogen was passed through, and the temperature was cooled to 45°C, 3 g of isocyanate was added, and the temperature was adjusted to maintain the system temperature at 75°C. After reacting for 1 hour, 1 g of tin octoate was added, and the reaction was continued for another 1 hour, and the temperature was cooled to 35°C, the material was discharged, nitrogen was filled, and then sealed to obtain a polyurethane polyethylene glycol prepolymer:

[0065] Step S2. 95 g of phenolic resin, 4.5 g of Tween 60, 10 g of polyurethane polyethylene glycol prepolymer and 4.5 g of n-pentane were mixed and stirred to obtain a foaming liquid;

[0066] Step S3. 13 g of phosphoric acid was quickly added to 100 g of the foaming liquid, and the mixture was rapidly stirred at 75° C. for 10 min, and then transferred into a mold, and molded at 50° C. for 30 min to obtain a foam partition;

[0067] Step S4. 3.5 g of water, 35 g of ethanol and 8 g of vinyl triethyl silane were mixed and ultrasonically vibrated for 5 min to obtain a mixed solution; 185 g of water was added to 7 g of graphene and stirred evenly, and then 45 g of the mixed solution was added to reflux at 75 ° C for 4 h, cooled to 25 ° C, and then washed twice with deionized water, and water was added to obtain a modified graphene dispersion with a mass fraction of 4.5%;

[0068] Step S5. A layer of modified graphene dispersion is evenly coated on the surface of the foam partition by a casting method, and then dried at 35° C. to obtain an antistatic foam partition.

[0069] Performance Test:

[0070] The performance tests were performed on the antistatic foam partitions prepared in Examples 1 to 4 and Comparative Examples 1 to 3:

[0071] Surface resistance test:

[0072] Referring to GB / T1410-2006 "Test Method for Volume Resistivity and Surface Resistivity of Solid Insulating Materials", the surface resistivity / volume resistivity tester (FT-303, Ningbo Argali Instrument Co., Ltd.) was used to directly test the surface resistance (Ω) of the antistatic foam separators prepared in Examples 1 to 4 and Comparative Examples 1 to 3.

[0073] Volume resistance test:

[0074] Referring to GB / T1410-2006 "Test Method for Volume Resistivity and Surface Resistivity of Solid Insulating Materials", the volume resistance (Ω) of the antistatic foam separators prepared in Examples 1 to 4 and Comparative Examples 1 to 3 was directly tested using a surface resistivity / volume resistivity tester (FT-303, Ningbo Argali Instrument Co., Ltd.);

[0075] Impact toughness test:

[0076] Referring to GB / T17657-2013 "Test Methods for Physical and Chemical Properties of Artificial Boards and Faced Artificial Boards", a pendulum impact tester (JB-300B, Jinan Chenxin Testing Machine Manufacturing Co., Ltd.) was used to test antistatic foam partitions with a size of 300 mm × 20 mm × hmm. There were 5 samples in each group. During the test, the impact force acted on the middle of the specimen. The energy Q consumed each time the specimen was broken was recorded with an accuracy of 1 J. The impact toughness (kJ / m2) of the antistatic foam partitions prepared in Examples 1 to 4 and Comparative Examples 1 to 3 was calculated according to the following formula: 2 );

[0077] Impact toughness calculation formula:

[0078] Adhesion test:

[0079] Referring to the ASTM-D3359-17 "Evaluation of Adhesion by Tape Test" standard, the modified graphene coating of the antistatic foam partition is cut in an X shape, a pressure-sensitive adhesive is attached to the cut, and then the tape is removed, and the adhesion level is evaluated using the 0-5 level standard, where 0 is the strongest adhesion and 5 is the weakest adhesion. Adhesion tester (QFH-HG600, Huaguo Precision Instrument Co., Ltd.) is used to test the adhesion (level) of the modified graphene coating on the surface of the antistatic foam partition prepared in Examples 1 to 4 and Comparative Examples 1 to 3, and the test results are shown in Table 1.

[0080] Table 1

[0081] project Surface resistance / Ω Volume resistance / Ω <![CDATA[Impact toughness / kJ·m -2 > Adhesion / Grade Example 1 <![CDATA[3.0×10 6 ]]> <![CDATA[3.8×10 5 ]]> 6.17 0 Example 2 <![CDATA[2.8×10 6 ]]> <![CDATA[4.1×10 5 ]]> 5.86 0 Example 3 <![CDATA[3.1×10 6 ]]> <![CDATA[3.9×10 5 ]]> 5.93 0 Example 4 <![CDATA[2.7×10 6 ]]> <![CDATA[4.3×10 5 ]]> 6.04 0 Comparative Example 1 <![CDATA[5.6×10 6 ]]> <![CDATA[3.7×10 8 ]]> 2.54 2 Comparative Example 2 <![CDATA[4.9×10 7 ]]> <![CDATA[2.0×10 8 ]]> 4.56 2 Comparative Example 3 <![CDATA[5.2×10 7 ]]> <![CDATA[4.1×10 9 ]]> 3.71 2

[0082] Data Analysis:

[0083] It can be seen from Table 1 that the antistatic foam separator prepared by the present invention has the smallest surface resistance and volume resistance, the largest impact toughness, and the adhesion grade is 0.

[0084] This may be due to the fact that the polyurethane polyethylene glycol prepolymer used in the present invention can improve the mechanical properties of the foam partition after mixing with the phenolic resin, and the modified graphene not only has long-term antistatic ability, but also can interact with the modified phenolic resin in the foam partition to further improve the antistatic ability and mechanical properties of the foam partition; graphene also has good adsorption capacity after modification, and the method of first dipping and then coating used in the present invention can also further improve the adsorption capacity of the modified graphene coating on the surface of the antistatic foam partition. Therefore, the antistatic foam partition prepared by the present invention has good mechanical properties, antistatic ability and adsorption capacity of the surface coating.

[0085] Comparative Example 1 did not add polyurethane polyethylene glycol prepolymer during the preparation of the antistatic foam partition. It can be seen from Table 1 that its surface resistance and area resistance increased, impact toughness decreased, and adsorption level was also improved to Level 2 compared with Example 1. This may be because the polyurethane polyethylene glycol prepolymer was not added during the preparation of the antistatic foam partition. It can not only modify the phenolic resin, but also interact with the modified graphene to improve the antistatic ability, mechanical properties and adsorption capacity of the surface coating of the antistatic foam partition; Example 2 replaces the "modified graphene dispersion" with "ordinary graphene dispersion". It can be seen from Table 1 that its surface resistance and area resistance increased, impact toughness decreased, and adsorption level was also improved to Level 2 compared with Example 1. This may be because the adsorption capacity of graphene is improved after being modified by vinyl triethyl silane, so ordinary graphene cannot interact with modified phenolic resin during the preparation process compared with it. It cannot be stably adsorbed on the surface of the antistatic foam partition. Therefore, the antistatic ability, mechanical properties and surface coating adsorption capacity of the antistatic foam partition prepared in Example 2 are poorer than those prepared in Example 1; in Comparative Example 3, the foam partition was not immersed in the modified graphene dispersion during the preparation of the antistatic foam partition. It can be seen from Table 1 that its surface resistance and area resistance are greatly increased, the impact toughness is reduced, and the adsorption force level is also improved to Level 2 compared with Example 1. This may be because the method of first immersion and then coating can not only make the modified graphene interact with the modified phenolic resin in the foam partition to further improve the antistatic ability and mechanical properties of the foam partition, but also make the adsorption capacity of the modified graphene coating on the surface of the antistatic foam partition further improved. Therefore, the antistatic ability, mechanical properties and surface coating adsorption capacity of the antistatic foam partition prepared in Example 1 are poorer.

[0086] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0087] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing an antistatic foam partition, characterized in that: The following steps are involved: Step S1. Mix the phenolic resin, surfactant, polyurethane polyethylene glycol prepolymer and foaming agent, stir evenly to obtain a foaming liquid; Step S2. quickly add a curing agent to the foaming liquid, quickly stir it evenly, and then transfer it into a mold for compression molding to obtain a foam partition; Step S3. Soaking the foam partition in the modified graphene dispersion and drying it to obtain a pretreated foam partition; Step S4. uniformly coating the surface of the pretreated foam partition with a layer of modified graphene dispersion by casting, and drying to obtain an antistatic foam partition; The polyurethane polyethylene glycol prepolymer is prepared from the following raw materials in parts by weight: 6-7.5 parts of polyethylene glycol, 3-3.5 parts of isocyanate, and 1-1.5 parts of tin octoate; The modified graphene is obtained by grafting graphene with vinyltriethylsilane.

2. The method for preparing an antistatic foam partition according to claim 1, characterized in that: In step S1, the surfactant is any one of Tween 60 and Tween 80 or a combination thereof, and the foaming agent is any one of n-pentane, isopentane and n-hexane or a combination thereof; and in step S2, the curing agent is any one of phosphoric acid and p-toluenesulfonic acid or a combination thereof.

3. The method for preparing an antistatic foam partition according to claim 1, characterized in that: The mass ratio of the phenolic resin, the surfactant, the polyurethane polyethylene glycol prepolymer and the foaming agent in step S1 is 95-100: 4.5-6: 10-11.5: 4.5-5.

0.

4. The method for preparing an antistatic foam partition according to claim 1, characterized in that: The mass ratio of the foaming liquid to the curing agent in step S2 is 100-105:13-17.

5. The method for preparing an antistatic foam partition according to claim 1, characterized in that: The molding process described in step S2 is: first stirring at a temperature of 75-90°C for 10-15 minutes, and then curing at 50-65°C for 30-35 minutes; the soaking time described in step S3 is 30-45 minutes, and the temperature during the drying treatment is 35-40°C; the temperature during the drying treatment in step S4 is 35-40°C.

6. The method for preparing an antistatic foam partition according to claim 1, characterized in that: The preparation method of the polyurethane polyethylene glycol prepolymer is as follows: The polyethylene glycol is evacuated with a vacuum oil pump at 110-120°C to remove moisture from the polyethylene glycol; then nitrogen is introduced, and the temperature is cooled to 45-50°C, isocyanate is added, and the temperature is adjusted to maintain the system temperature at 75-80°C. After the reaction, tin octoate is added, and the reaction is continued for 1-1.5h, and the temperature is cooled to 35-40°C, the material is discharged, nitrogen is filled, and then sealed to obtain a polyurethane polyethylene glycol prepolymer.

7. The method for preparing an antistatic foam partition according to claim 1, characterized in that: The preparation method of the modified graphene dispersion is as follows: Step A1. Mix water, ethanol and vinyl triethylsilane, and ultrasonically vibrate for 5-10 minutes to obtain a mixed solution; Step A2. Add water to the graphene, stir evenly, then add the mixed solution at 75-80° C., reflux for 4-4.5 hours, cool to 25-30° C., and then wash with deionized water 2-3 times to obtain modified graphene; Step A3. Add water to the modified graphene to obtain a modified graphene dispersion with a mass fraction of 4.5%-5%.

8. The method for preparing an antistatic foam partition according to claim 7, characterized in that: The mass ratio of water, ethanol and vinyltriethylsilane in step A1 is 3.5-4:35-38:8-11.

9. The method for preparing an antistatic foam partition according to claim 7, characterized in that: The mass ratio of graphene, water and mixed liquid in step A2 is 7-10:185-190:45-50.

10. An antistatic foam partition, characterized in that: The foam partition is prepared by the preparation method according to any one of claims 1 to 9.